Sulfonyl imide polyurethane single-ion polymer electrolyte membrane and preparation method and application thereof
By using sulfonylimide-based polyurethane single-ion polymer electrolyte membrane in lithium batteries, combining the microphase separation structure of aromatic hard segments and PEO soft chains and the strong charge delocalization of sulfonylimide-based anions, the single-ion polymer electrolyte membrane is solved. Ionic polymer electrolytes achieve efficient lithium ion transport and electrochemical stability in lithium batteries due to the difficulty in balancing low ionic conductivity and mechanical properties.
Patent Information
- Application Number
- CN202410707770.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-03
AI Technical Summary
Existing single-ion polymer electrolytes in lithium batteries have problems such as low ionic conductivity and difficulty in balancing mechanical properties, which limits their practical application in lithium batteries.
Sulfonimide-based polyurethane single-ion polymer electrolyte membrane is used, which is composed of aromatic hard segments and flexible PEO soft chains. The anions are located in the hard segments through micro-phase separation structure and strong charge delocalization of sulfonimide-based anions. function to increase the dissociation degree of lithium ions, increase the lithium salt concentration and lower the glass transition temperature by adjusting the ratio of soft and hard segments.
It achieves high ionic conductivity, excellent mechanical properties and a wide electrochemical stability window, and is suitable for lithium batteries, especially showing excellent electrochemical properties in high-voltage lithium batteries.
Smart Images

Figure CN118725252A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic polymer functional materials and electrochemical technology, and in particular to a sulfonyl imide-based polyurethane single-ion polymer electrolyte membrane and a preparation method and application thereof. Background Art
[0002] Lithium batteries have advantages such as high specific energy and energy density, and play an irreplaceable role in energy storage devices. Among them, lithium metal batteries with high energy density and safety are considered to be one of the most promising energy storage systems. However, the potential safety issues caused by traditional liquid electrolytes pose a serious obstacle to the implementation of lithium metal electrodes. For a long time, solid polymer electrolytes with many advantages such as good safety, high flexibility, light weight and low processing cost have been considered to be one of the most promising candidates for the realization of lithium metal batteries.
[0003] At present, the research on dual-ion polymer electrolytes formed by dissolving low molecular weight lithium salts in a polymer matrix is relatively extensive. During the charge and discharge cycle, the lithium and its counter ions of the dual-ion polymer electrolyte move in opposite directions within the polymer matrix. Anions accumulate on the anode side and develop into concentration polarization, which affects the battery performance (including impedance increase, voltage loss, and unnecessary side reactions), and ultimately leads to battery failure. In response to this problem, single-ion polymer electrolytes with fixed anions have attracted attention. They have the advantages of a lithium ion migration number close to 1 and effective suppression of lithium "dendrites", which can significantly improve the safety, energy density and cycle stability of lithium batteries. At present, single-ion polymer electrolytes still have problems such as low ionic conductivity and difficulty in combining excellent electrochemical and mechanical properties in the same material, which limits their practical application in lithium batteries.
[0004] Polyurethane can form a microphase separation structure driven by thermodynamic incompatibility and hydrogen bonding between different segments. The polyurethane-based single-ion polymer electrolyte prepared with polyethylene oxide (PEO) with a strong solvation effect as the soft segment and diisocyanate and aromatic anion as the hard segment can play a supporting role and provide a certain mechanical strength, while the soft segment still maintains a low glass transition temperature, which is conducive to the transmission of lithium ions. However, the polyurethane-based single-ion polymer electrolyte still has the problem of low ion conductivity, generally below 10 -9 ~10 -7 S / cm, such as Chinese patents CN201810639338.X and CN202111395228.1. Patent CN202111395228.1 prepared a type of fluorinated polyurethane single-ion polymer electrolyte, which has high mechanical strength (~10MPa) and excellent ionic conductivity, reaching 10 -7 S / cm. However, the Li +The / EO ratio can only be changed within a small range, and the lithium salt concentration cannot be changed while maintaining the long soft segment (PEO) chain length. At the same time, due to the regular structure, the ionic conductivity of the prepared polymer electrolyte is still low.
[0005] In summary, single-ion polymer electrolytes have problems such as insufficient ion conductivity and the inability to achieve both excellent ion conductivity and certain mechanical properties, which greatly limits their practical applications. Polyurethane single-ion polymer electrolytes with aromatic hard segments and PEO soft segments can undergo microphase separation and exhibit certain ion conductivity and excellent mechanical strength, but their ion conductivity needs to be further improved. Summary of the invention
[0006] The purpose of the present invention is to solve the above technical problems and to provide a sulfonyl imide based polyurethane single ion polymer electrolyte membrane and a preparation method and application thereof.
[0007] Sulfonyl imide polyurethane single ion polymer electrolyte membrane, the chemical structure of the sulfonyl imide polyurethane single ion polymer electrolyte membrane is as follows:
[0008]
[0009] In the above formula, p is an integer between 2 and 110, m:n=1:(0.1 to 20), R1 is R2 is R3 is -CF3, -CH3, -CHF2,
[0010] The preparation method of sulfonyl imide polyurethane single ion polymer electrolyte membrane is carried out according to the following steps:
[0011] Step S1: Under the protection of nitrogen atmosphere and ice water bath, dinitrobenzoyl chloride, sulfonamide compound, 4-dimethylaminopyridine and triethylamine are dissolved in anhydrous acetonitrile solvent, reacted at a temperature of 10 to 50° C. for 12 to 94 hours, purged and then extracted to obtain reaction product a;
[0012] Step S2: under the protection of nitrogen atmosphere, the reaction product a obtained in step S1 and methanol are added to deionized water, heated to reflux, and then iron powder and acetic acid are added, and the reflux reaction is continued for 1 to 4 hours. After the reaction is completed, the reaction is cooled and filtered, and the pH is adjusted to alkaline, and then filtered and extracted to obtain the reaction product b;
[0013] Step S3: under the protection of nitrogen atmosphere, adding the reaction product b obtained in step S2, polyethylene oxide and diisocyanate into a solvent, reacting at a temperature of 30 to 120° C. for 12 to 94 hours, washing the reaction product with water and alcohol in sequence, purging and drying to obtain a crude product;
[0014] Step S4: The crude product obtained in step S3 is lithiated using a lithium hydroxide aqueous solution, and then dialyzed to obtain a polymer, and finally the polymer is made into a membrane to obtain a sulfonyl imide polyurethane single-ion polymer electrolyte membrane.
[0015] Application of sulfonyl imide polyurethane single ion polymer electrolyte membrane, and application of the sulfonyl imide polyurethane single ion polymer electrolyte membrane in solid-state lithium metal batteries.
[0016] Principle of the present invention:
[0017] 1. The single-ion polymer electrolyte prepared by the present invention is composed of a rigid aromatic hard segment and a flexible PEO soft chain, wherein the anion is located in the hard segment of the structure, and can be microphase separated into a microphase structure in which the hard domain is uniformly dispersed in a continuous soft phase, while exhibiting good ionic conductivity and mechanical properties.
[0018] 2. The polyurethane single-ion polymer electrolyte prepared by the present invention has a sulfonyl imide anion side chain, and the strong charge delocalization effect of the anion can effectively improve the degree of lithium ion dissociation.
[0019] 3. Fast ion transport nanochannels can be formed in the hard domains of the polymer electrolyte membrane prepared by the present invention, thereby preventing the formation of ion aggregates in the hard domains and reducing the influence of regular hard domains on the effective carrier concentration.
[0020] 4. The present invention can effectively increase the lithium salt concentration of the sample by adjusting the ratio of the soft segment to the hard segment, and the soft segment can maintain a low glass transition temperature, so that the prepared single-ion polymer electrolyte has both high lithium salt concentration and low glass transition temperature.
[0021] Beneficial effects of the present invention:
[0022] (1) The sulfonyl imide-based polyurethane single-ion polymer electrolyte membrane prepared by the present invention has the advantages of excellent ion conductivity, good mechanical properties, a lithium ion migration number close to 1, and a wide electrochemical stability window.
[0023] (2) The full battery assembled using the sulfonyl imide polyurethane single-ion polymer electrolyte membrane prepared by the present invention exhibits excellent electrochemical performance at both room temperature and high temperature, and has potential application value in high-voltage lithium batteries.
[0024] The invention can obtain a sulfonyl imide-based polyurethane single-ion polymer electrolyte membrane and a preparation method and application thereof. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 represents an infrared spectrum of the electrolyte I prepared in Example 1;
[0026] Figure 2 represents the AC impedance spectrum of the electrolyte I prepared in Example 1 at 30°C;
[0027] Figure 3 represents the LSV curve of electrolyte I prepared in Example 1 at room temperature;
[0028] Figure 4 : represents the charge and discharge curve of the electrolyte I prepared in Example 1 at 80°C;
[0029] Figure 5 represents the AC impedance spectrum of the electrolyte II prepared in Example 2 at 30°C;
[0030] Figure 6 The figure shows the AC impedance spectrum of the electrolyte II prepared in Example 2 at 80°C. DETAILED DESCRIPTION
[0031] Specific implementation method 1: The chemical structure of the sulfonimide-based polyurethane single-ion polymer electrolyte membrane of this implementation method is as follows:
[0032]
[0033] In the above formula, p is an integer between 2 and 110, m:n=1:(0.1 to 20), R1 is R2 is R3 is -CF3, -CF3, -CHF2,
[0034] Specific implementation method 2: The preparation method of the sulfonyl imide polyurethane single ion polymer electrolyte membrane of this implementation method is carried out according to the following steps:
[0035] Step S1: Under the protection of nitrogen atmosphere and ice water bath, dinitrobenzoyl chloride, sulfonamide compound (structure such as R3), 4-dimethylaminopyridine and triethylamine are dissolved in anhydrous acetonitrile solvent, reacted at a temperature of 10 to 50° C. for 12 to 94 hours, purged and then extracted to obtain reaction product a;
[0036] Step S2: under the protection of nitrogen atmosphere, the reaction product a obtained in step S1 and methanol are added to deionized water, heated to reflux, and then iron powder and acetic acid are added, and the reflux reaction is continued for 1 to 4 hours. After the reaction is completed, the reaction is cooled and filtered, and the pH is adjusted to alkaline, and then filtered and extracted to obtain the reaction product b;
[0037] Step S3: under the protection of nitrogen atmosphere, the reaction product b obtained in step S2, polyethylene oxide and diisocyanate (structure such as R2) are added to a solvent, reacted at a temperature of 30 to 120° C. for 12 to 94 hours, and the reaction product is washed with water and alcohol in sequence, purged and dried to obtain a crude product;
[0038] Step S4: The crude product obtained in step S3 is lithiated using a lithium hydroxide aqueous solution, and then dialyzed to obtain a polymer, and finally the polymer is made into a membrane to obtain a sulfonyl imide polyurethane single-ion polymer electrolyte membrane.
[0039] Specific implementation method three: This implementation method is different from specific implementation method one or two in that the dinitrobenzoyl chloride described in step S1 is prepared according to the following steps: under the protection of nitrogen atmosphere, oxalyl chloride and N, N-dimethylformamide are added to anhydrous acetonitrile, stirred for 3 to 8 hours, and then dinitrobenzoic acid (structure such as R1) is added, and the reaction is continued at 0 to 60° C. for 12 to 72 hours, and then distilled under reduced pressure to obtain dinitrobenzoyl chloride; the oxalyl chloride described in step S1 is prepared according to the following steps: under the protection of nitrogen atmosphere, oxalyl chloride and N, N-dimethylformamide are added to anhydrous acetonitrile, stirred for 3 to 8 hours, and then dinitrobenzoic acid (structure such as R1) is added, and the reaction is continued at 0 to 60° C. for 12 to 72 hours, and then distilled under reduced pressure to obtain dinitrobenzoyl chloride; The molar ratio of oxalyl chloride to dinitrobenzoic acid is (1.01-1.2):1; the ratio of the mass of oxalyl chloride, the volume of N,N-dimethylformamide and the volume of anhydrous acetonitrile is (0.67-1.34) g:0.01 mL:30 mL; the dinitrobenzoic acid is one or more of 2,4-dinitrobenzoic acid, 3,5-dinitrobenzoic acid, 3,4-dinitrobenzoic acid and 4-methyl-3,5-dinitrobenzoic acid.
[0040] The other steps are the same as those in the first or second embodiment.
[0041] Specific embodiment 4: The difference between this embodiment and specific embodiments 1 to 3 is that the molar ratio of dinitrobenzoyl chloride to sulfonamide compound in step S1 is 1:(1.01-1.2); the ratio of the mass of 4-dimethylaminopyridine, the volume of triethylamine and the volume of anhydrous acetonitrile solvent is (0.06-0.12) g:(3-6) mL:30 mL.
[0042] The other steps are the same as those in Specific Embodiments 1 to 3.
[0043] Specific embodiment 5: The difference between this embodiment and specific embodiments 1 to 4 is that the sulfonamide compound described in step S1 is methylsulfonamide, trifluoromethanesulfonamide, benzenesulfonamide, benzenesulfonamide, 4-(trifluoromethyl)benzenesulfonamide, 3-(trifluoromethyl)benzenesulfonamide, pentafluorobenzenesulfonamide, difluoromethanesulfonamide or 4-(trifluoromethoxy)benzenesulfonamide.
[0044] The other steps are the same as those in Specific Embodiments 1 to 4.
[0045] Specific embodiment six: The difference between this embodiment and specific embodiments one to five is that the molar ratio of the reaction product a to the iron powder in step S2 is 1:(6-10); the volume ratio of the methanol, deionized water and acetic acid is (60-90):(20-30):(20-40).
[0046] The other steps are the same as those in Specific Embodiments 1 to 5.
[0047] Specific embodiment seven: The difference between this embodiment and specific embodiments one to six is that: the molar ratio of the reaction product b, polyethylene oxide and diisocyanate described in step S3 is 1: (0.1~20): (1.1~21); the ratio of the mass of the reaction product b to the volume of the solvent is (0.80~0.92) g: 50mL; the diisocyanate is p-phenylene diisocyanate, 1,3-phenylene diisocyanate, m-phenylenediisocyanate, 4,4'-methylenebis(phenyl isocyanate) or hexamethylene diisocyanate.
[0048] The other steps are the same as those in Specific Embodiments 1 to 6.
[0049] Specific embodiment eight: The difference between this embodiment and specific embodiments one to seven is that the solvent described in step S3 includes but is not limited to N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone or anhydrous acetonitrile.
[0050] The other steps are the same as those in Specific Embodiments 1 to 7.
[0051] Specific embodiment nine: The difference between this embodiment and specific embodiments one to eight is: the specific steps of membrane preparation in step S4: completely dissolve the polymer into N,N-dimethylformamide, cast it in a polytetrafluoroethylene mold, first dry it at 40°C until there is no obvious solvent, then dry it at 60°C and 80°C for 48h in turn, and finally vacuum dry it at 100°C for 24h to obtain a sulfonyl imide polyurethane single-ion polymer electrolyte membrane, the thickness of the sulfonyl imide polyurethane single-ion polymer electrolyte membrane is 0.005~2mm.
[0052] The other steps are the same as those in Specific Embodiments 1 to 8.
[0053] Specific implementation method ten: application of the sulfonyl imide-based polyurethane single-ion polymer electrolyte membrane of this implementation method, application of the sulfonyl imide-based polyurethane single-ion polymer electrolyte membrane in solid-state lithium metal batteries.
[0054] The following examples are used to verify the beneficial effects of the present invention:
[0055] Example 1: Preparation of Electrolyte I, according to the following steps:
[0056] Step S1: Under the protection of nitrogen atmosphere and ice water bath, 4-methyl-3,5-dinitrobenzoyl chloride, 0.72 g trifluoromethanesulfonamide, 0.06 g 4-dimethylaminopyridine and 3 mL triethylamine were dissolved in 30 mL anhydrous acetonitrile solvent, reacted at 30° C. for 72 h, purged and then extracted with dichloromethane to obtain reaction product a;
[0057] The 4-methyl-3,5-dinitrobenzoyl chloride described in step S1 is prepared according to the following steps: under the protection of nitrogen atmosphere, 0.67 g of oxalyl chloride and 0.01 mL of N,N-dimethylformamide (DMF) are added to 30 mL of anhydrous acetonitrile, stirred for 5 h, and then 1 g of 4-methyl-3,5-dinitrobenzoic acid is added, and the reaction is continued at 30° C. for 20 h, and then distilled under reduced pressure to obtain 4-methyl-3,5-dinitrobenzoyl chloride;
[0058] Step S2: under nitrogen atmosphere, the reaction product a obtained in step S1 and 60 mL of methanol were added to 20 mL of deionized water, heated to reflux, and then 2.23 g of iron powder and 20 mL of acetic acid were added, and the reflux reaction was continued for 2 h. After the reaction was completed, the mixture was cooled and filtered, and the pH was adjusted to alkaline with sodium bicarbonate, and then filtered with suction and extracted with dichloromethane to obtain the reaction product b;
[0059] Step S3: Under nitrogen atmosphere protection, 0.80 g of the reaction product b obtained in step S2, 6.00 g of polyethylene oxide (PEO, molecular weight 1500) and 1.10 g of p-phenylene diisocyanate were added to 50 mL of N,N-dimethylformamide, and reacted at 70° C. for 72 h. The reaction product was washed with water and then with alcohol in sequence, and after purging, was placed in a vacuum drying oven at 80° C. for drying for 48 h to completely remove the solvent and water to obtain a crude product;
[0060] Step S4: The crude product obtained in step S3 is lithified with a lithium hydroxide aqueous solution, and then dialyzed to obtain a polymer. Finally, 0.2 g of the polymer is dissolved in 5 mL of N,N-dimethylformamide, stirred for 2 h to fully dissolve, and cast into a polytetrafluoroethylene mold. First, it is dried at 40°C until there is no obvious solvent, and then dried at 60°C and 80°C for 48 h, and finally dried at 100°C in vacuum for 24 h to obtain electrolyte I.
[0061] The specific structural formula of electrolyte I is as follows:
[0062]
[0063] Note: Since a polymer is prepared in this example, n in the structural formula only reflects a ratio and does not have a specific value.
[0064] Figure 1 The infrared spectrum of the electrolyte I prepared in Example 1 is shown; Figure 1 As shown, it can be proved that the polymer product with the above structural formula was successfully prepared in this embodiment.
[0065] The thickness of the electrolyte I prepared in this example is 0.138 mm, and the conductivity is 6.22×10 -7 S cm -1 , the fracture stress is 3.4MPa.
[0066] Example 2: Preparation of Electrolyte II, according to the following steps:
[0067] Step S1: Under the protection of nitrogen atmosphere and ice water bath, 3,5-dinitrobenzoyl chloride, 0.98 g trifluoromethanesulfonamide, 0.12 g 4-dimethylaminopyridine and 6 mL triethylamine were dissolved in 30 mL anhydrous acetonitrile solvent, reacted at 30° C. for 72 h, purged and then extracted with dichloromethane to obtain reaction product a;
[0068] The 3,5-dinitrobenzoyl chloride described in step S1 is prepared according to the following steps: under the protection of nitrogen atmosphere, 0.67 g of oxalyl chloride and 0.01 mL of N,N-dimethylformamide (DMF) are added to 30 mL of anhydrous acetonitrile, stirred for 5 h, and then 2 g of 3,5-dinitrobenzoic acid is added. After continuing the reaction at 30° C. for 20 h, the mixture is distilled under reduced pressure to obtain 3,5-dinitrobenzoyl chloride;
[0069] Step S2: under nitrogen atmosphere, the reaction product a obtained in step S1 and 90 mL of methanol were added to 30 mL of deionized water, heated to reflux, and then 4.74 g of iron powder and 40 mL of acetic acid were added, and the reflux reaction was continued for 2 h. After the reaction was completed, the mixture was cooled and filtered, and the pH was adjusted to alkaline with sodium bicarbonate, and then filtered and extracted with dichloromethane to obtain a reaction product b;
[0070] Step S3: Under nitrogen atmosphere protection, 0.61 g of the reaction product b obtained in step S2, 6.00 g of polyethylene oxide (PEO, molecular weight 1500) and 1.09 g of p-phenylene diisocyanate were added to 50 mL of N,N-dimethylformamide, and reacted at 70° C. for 72 h. The reaction product was washed with water and then with alcohol in sequence, and after purging, was placed in a vacuum drying oven at 80° C. for drying for 48 h to completely remove the solvent and water to obtain a crude product;
[0071] Step S4: The crude product obtained in step S3 is lithified with a lithium hydroxide aqueous solution, and then dialyzed to obtain a polymer. Finally, 0.2 g of the polymer is dissolved in 5 mL of N,N-dimethylformamide, stirred for 2 h to fully dissolve, and cast into a polytetrafluoroethylene mold. First, it is dried at 40°C until there is no obvious solvent, and then dried at 60°C and 80°C for 48 h, and finally vacuum dried at 100°C for 24 h to obtain electrolyte II.
[0072] The specific structural formula of electrolyte II is as follows:
[0073]
[0074] The thickness of the electrolyte II prepared in this example is 0.121 mm, and the conductivity is 1.08×10 -7 S cm -1 , the fracture stress is 4.7MPa.
[0075] Experimental part:
[0076] Characterization of polymer electrolyte performance;
[0077] (1) Characterization method of ionic conductivity: The prepared single-ion polymer electrolyte membrane was sandwiched between two stainless steel electrodes with a diameter of 1 cm to form a polymer electrolyte blocking electrode system. The Nyquist plot of the sample was drawn through AC impedance testing, and the bulk impedance (R b ). The ionic conductivity σ of the sample is calculated according to the following formula:
[0078]
[0079] Where d is the thickness of the single-ion polymer electrolyte membrane and S is the area of the stainless steel electrode.
[0080] (2) Characterization method of electrochemical stability window: Button cells were assembled with stainless steel sheet and lithium sheet as working electrode and reference electrode, respectively. The electrochemical stability window of the sample was tested at a scan rate of 0.1 mV·s-1 in the range of 0 to 6 V using linear sweep voltammetry.
[0081] Battery performance test;
[0082] With LiFePO4 as the positive electrode and lithium metal as the negative electrode, a LiFePO4 / quasi-solid-state single-ion polymer electrolyte plasticized with a small amount of plasticizer / Li full battery was assembled, and the electrochemical test of the full battery was carried out using the Xinwei battery testing system.
[0083] Among them, Figure 2 and Figure 5 As shown in the figure, the ionic conductivity of electrolyte I at 30°C is nearly 5 times higher than that of electrolyte II, which is mainly caused by the difference in anion structure. Since electrolyte I uses benzoyl (trifluoromethanesulfonyl) imide as anion, fluorine-containing sulfonyl imide anions have strong charge delocalization and are conducive to the formation of a stable interface layer, the ionic conductivity and interfacial compatibility of electrolyte I with lithium metal electrodes are higher than those of electrolyte II without fluorine atoms, making it show better battery performance.
[0084] In the papers published before the present invention, the method of post-polymerization grafting was used to prepare sulfonyl imide-based single-ion polymer electrolytes. Although the amino group has high reactivity with isocyanate, the polyurea prepared by the first step of the reaction has poor processing performance and is not easy to dissolve, which increases the difficulty of post-grafting treatment. Based on this, the innovative preparation process of the present invention is applicable to a variety of sulfonyl imide anion structures and weakens the limitation of polyurea processing properties on the structure of single-ion polymer electrolytes, which is conducive to the development and application of high ionic conductivity sulfonyl imide-based single-ion polymer electrolytes.
Claims
1. Sulfonyl imide polyurethane single ion polymer electrolyte membrane, characterized in that The chemical structural formula of the sulfonyl imide polyurethane single ion polymer electrolyte membrane is as follows: In the above formula, p is an integer between 2 and 110, m:n=1:(0.1 to 20), R1 is R2 is R3 is -CF3-CH3, -CHF2, 2. The method for preparing the sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 1, characterized in that The preparation method is carried out according to the following steps: Step S1: Under the protection of nitrogen atmosphere and ice water bath, dinitrobenzoyl chloride, sulfonamide compound, 4-dimethylaminopyridine and triethylamine are dissolved in anhydrous acetonitrile solvent, reacted at a temperature of 10 to 50° C. for 12 to 94 hours, purged and then extracted to obtain reaction product a; Step S2: under the protection of nitrogen atmosphere, the reaction product a obtained in step S1 and methanol are added to deionized water, heated to reflux, and then iron powder and acetic acid are added, and the reflux reaction is continued for 1 to 4 hours. After the reaction is completed, the reaction is cooled and filtered, and the pH is adjusted to alkaline, and then filtered and extracted to obtain the reaction product b; Step S3: under the protection of nitrogen atmosphere, adding the reaction product b obtained in step S2, polyethylene oxide and diisocyanate into a solvent, reacting at a temperature of 30 to 120° C. for 12 to 94 hours, washing the reaction product with water and alcohol in sequence, purging and drying to obtain a crude product; Step S4: The crude product obtained in step S3 is lithiated using a lithium hydroxide aqueous solution, and then dialyzed to obtain a polymer, and finally the polymer is made into a membrane to obtain a sulfonyl imide polyurethane single-ion polymer electrolyte membrane.
3. The method for preparing the sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 2, characterized in that The dinitrobenzoyl chloride described in step S1 is prepared according to the following steps: under the protection of nitrogen atmosphere, oxalyl chloride and N,N-dimethylformamide are added to anhydrous acetonitrile, stirred for 3 to 8 hours, and then dinitrobenzoic acid is added. After continuing to react at 0 to 60° C. for 12 to 72 hours, reduced pressure distillation is performed to obtain dinitrobenzoyl chloride; the molar ratio of the oxalyl chloride to the dinitrobenzoic acid is (1.01 to 1.2): 1; the ratio of the mass of the oxalyl chloride, the volume of N,N-dimethylformamide and the volume of anhydrous acetonitrile is (0.67 to 1.34) g: 0.01 mL: 30 mL; the dinitrobenzoic acid is one or more of 2,4-dinitrobenzoic acid, 3,5-dinitrobenzoic acid, 3,4-dinitrobenzoic acid and 4-methyl-3,5-dinitrobenzoic acid.
4. The method for preparing the sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 2, characterized in that In step S1, the molar ratio of dinitrobenzoyl chloride to sulfonamide compound is 1:(1.01-1.2); the ratio of the mass of 4-dimethylaminopyridine, the volume of triethylamine and the volume of anhydrous acetonitrile solvent is (0.06-0.12) g:(3-6) mL:30 mL.
5. The method for preparing the sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 2, characterized in that The sulfonamide compound described in step S1 is methylsulfonamide, trifluoromethanesulfonamide, benzenesulfonamide, benzenemethylsulfonamide, 4-(trifluoromethyl)benzenesulfonamide, 3-(trifluoromethyl)benzenesulfonamide, pentafluorobenzenesulfonamide, difluoromethanesulfonamide or 4-(trifluoromethoxy)benzenesulfonamide.
6. The method for preparing the sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 2, characterized in that The molar ratio of the reaction product a to the iron powder in step S2 is 1:(6-10); the volume ratio of the methanol, deionized water and acetic acid is (60-90):(20-30):(20-40).
7. The method for preparing the sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 2, characterized in that The molar ratio of the reaction product b, polyethylene oxide and diisocyanate described in step S3 is 1: (0.1-20): (1.1-21); the ratio of the mass of the reaction product b to the volume of the solvent is (0.80-0.92) g: 50 mL; the diisocyanate is p-phenylene diisocyanate, 1,3-phenylene diisocyanate, m-phenylenediisocyanate, 4,4'-methylenebis(phenyl isocyanate) or hexamethylene diisocyanate.
8. The method for preparing the sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 2, characterized in that The solvent described in step S3 includes, but is not limited to, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone or anhydrous acetonitrile.
9. The method for preparing a sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 2, characterized in that The specific steps of membrane preparation in step S4 are as follows: the polymer is completely dissolved in N,N-dimethylformamide, cast in a polytetrafluoroethylene mold, first dried at 40°C until there is no obvious solvent, then dried at 60°C and 80°C for 48h, and finally vacuum dried at 100°C for 24h to obtain a sulfonyl imide polyurethane single-ion polymer electrolyte membrane, wherein the thickness of the sulfonyl imide polyurethane single-ion polymer electrolyte membrane is 0.005-2mm.
10. The use of the sulfonyl imide polyurethane single ion polymer electrolyte membrane according to claim 1, characterized in that The application of the sulfonyl imide-based polyurethane single-ion polymer electrolyte membrane in solid-state lithium metal batteries.
Citation Information
Patent Citations
Single-ion polymer electrolyte, and preparation method and application thereof
CN108832178A
Self-repairing polymer electrolyte matrix and preparation method thereof, self-repairing polymer electrolyte, lithium ion battery and application thereof
CN109659605A
Polyimide single-ion polymer, preparation method thereof and solid polymer electrolyte membrane
CN111548490A
POSS-based polyion liquid solid electrolyte membrane and preparation method thereof
CN111900465A
Fluorine-containing polyurethane single-ion polymer electrolyte membrane and preparation method and application thereof
CN114015007A