Purification method of polyaryletherketone

Through physical crushing and solvent mixing and heating treatment, the problems of low molecular weight and poor stability of polyaryl ether ketone are solved, and high-quality, low-temperature purification of polyaryl ether ketone is achieved to meet various application needs.

CN118725285AInactive Publication Date: 2024-10-01SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310336589.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent
Patent Text Reader

Abstract

The invention discloses a method for purifying polyaryletherketone, which comprises the following steps: s1, physically crushing a polyaryletherketone resin material to obtain polyaryletherketone resin powder with the particle size of less than or equal to 100 mu m; s2, cleaning the polyaryletherketone resin powder by adopting an alcohol solvent, and then filtering and drying to obtain a polyaryletherketone purified product; s3, mixing the purified polyaryletherketone product with an organic polar aprotic solvent, heating to 60-120 DEG C, stirring or boiling reflux for 2-6 hours, filtering and drying to obtain a primary pure polyaryletherketone product and filtrate; and s4, adding a polar solvent into the filtrate to separate out a solid, and then washing, filtering and drying to obtain primary low-molecular-weight polyaryletherketone powder. After the treatment method provided by the invention is adopted, the intrinsic viscosity of the high molecular weight polyaryletherketone (PEKK) resin can be increased to 0.65-0.96 dL / g, but low molecular weight polyaryletherketone (PEKK) powder with low intrinsic viscosity (0.19-0.34 dL / g) can also be obtained through the treatment method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, in particular to a purification method for polyaryletherketone. Background Art

[0002] Polyaryletherketone (PAEK) is a type of crystalline polymer formed by connecting phenylene rings through oxygen bridges (ether bonds) and carbonyl groups (ketones). Many different polymers can be formed according to the different connection order and ratio of ether bonds, ketone groups and benzene rings in the molecular chain. There are mainly polyetheretherketone (PEEK), polyetherketone (PEK), polyetherketoneketone (PAEK), polyetheretherketoneketone (PEEKK) and polyetherketoneetherketoneketone (PEKEKK). Polyaryletherketone contains rigid benzene rings in its molecular structure, so it has excellent high temperature performance, mechanical properties, electrical insulation, radiation resistance and chemical resistance. The ether bonds in the molecular structure of polyaryletherketone make it flexible, so it can be molded using the processing method of thermoplastic engineering plastics. In the polyaryletherketone series, the lower the ratio of ether bonds to ketone groups (E / K) in the molecular chain, the higher its melting point and glass transition temperature. Polyaryletherketone can be used to manufacture high-impact resistant gears, bearings, microwave turntable transmission parts, automotive gear seals, gear support seats, bushings, powder coatings and ultra-pure medium conveying pipelines, aerospace structural materials, etc.

[0003] The research and development of polyaryletherketones began in the 1960s. In 1962, Dupont in the United States and ICI in the United Kingdom reported that polyaryletherketones could be synthesized by electrophilic substitution in the presence of Friedel-Crafts catalysts. Later, people continued to study this technology and made significant contributions. In 1979, ICI in the United Kingdom produced high molecular weight PEK, laying the foundation for the synthesis of polyaryletherketones.

[0004] Due to the complex process of PAEK synthesis and the steric hindrance effect of its benzene ring structure, the connection between its molecular chains is not very long, resulting in the synthesized PAEK having a low molecular weight and a wide molecular weight distribution. The quality and stability of the products processed from the synthesized powder are very poor. The more low molecular weight parts in PAEK, the worse its mechanical properties and the poorer the quality of the products. The more high molecular weight parts, the higher the mechanical properties and the better the quality of the products. However, the more high molecular weight parts of PAEK, the higher its melt viscosity and processing temperature.

[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0006] The object of the present invention is to provide a method for purifying polyaryletherketone, which can overcome the technical problem that polyaryletherketone prepared in the prior art is difficult to simultaneously meet the requirements of high quality, good stability and low processing temperature.

[0007] To achieve the above object, an embodiment of the present invention provides a method for purifying polyaryletherketone, the method comprising:

[0008] s1. physically crushing the polyaryletherketone resin material to obtain a polyaryletherketone resin powder having a particle size less than or equal to 100 μm;

[0009] s2, washing the polyaryletherketone resin powder with an alcohol solvent, and then filtering and drying to obtain a purified polyaryletherketone product;

[0010] s3. Mix the purified polyaryletherketone product and the organic polar aprotic solvent, heat to 60°C-120°C, stir or boil under reflux for 2h-6h, filter and dry to obtain a first-grade purified polyaryletherketone product and a filtrate;

[0011] s4. Add a polar solvent to the filtrate, wash, filter and dry the precipitated solid to obtain a first-grade low molecular weight polyaryletherketone powder.

[0012] In one or more embodiments of the present invention, the alcohol solvent is selected from methanol, ethanol or a combination thereof.

[0013] In one or more embodiments of the present invention, in s4, the polar solvent is selected from formamide, trifluoroacetic acid, DMSO, acetonitrile, DMF, hexamethylphosphoramide, methanol, ethanol, acetic acid, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine or n-butanol.

[0014] In one or more embodiments of the present invention, s2 comprises: mixing an alcohol solvent and polyaryletherketone resin powder, heating to 60°C-140°C for stirring or ultrasonic oscillation reflux for 2h-8h; cooling to 20°C-25°C, filtering, and then drying to obtain a purified polyaryletherketone product.

[0015] In one or more embodiments of the present invention, after the alcohol solvent and the polyaryletherketone resin powder are mixed, the weight ratio of the polyaryletherketone resin powder is 30%-60%.

[0016] In one or more embodiments of the present invention, in said s1, the physical crushing method is selected from air flow crushing, ultrasonic crushing, mechanical ball milling or double roller crushing.

[0017] In one or more embodiments of the present invention, in s3, the organic polar aprotic solvent is selected from o-dichlorobenzene, dimethyl sulfoxide (DMSO) or N,N-dimethylformamide (DMF).

[0018] In one or more embodiments of the present invention, in said s3, the weight ratio of the purified polyaryletherketone to the organic polar aprotic solvent is 1:(1-1.4).

[0019] In one or more embodiments of the present invention, in said s3, the intrinsic viscosity of the first-grade pure polyaryletherketone is 0.19 dL / g-0.34 dL / g.

[0020] In one or more embodiments of the present invention, in said s4, the primary low molecular weight polyaryletherketone powder has an intrinsic viscosity of 0.65 dL / g-0.96 dL / g.

[0021] Compared with the prior art, the method of the present invention can not only obtain high molecular weight polyaryletherketone pure products, but also obtain polyaryletherketone powders in different relatively low molecular weight ranges, thereby realizing the adjustment and screening of the molecular weight distribution of polyaryletherketone to meet the needs of different processing and molding conditions and application scenarios, and greatly improving the quality of the products. DETAILED DESCRIPTION

[0022] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.

[0023] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0024] The embodiment of the present invention discloses a method for purifying polyaryletherketone, the method comprising:

[0025] s1. physically crushing the polyaryletherketone resin material to obtain a polyaryletherketone resin powder having a particle size less than or equal to 100 μm;

[0026] s2. Removal of interfering substances: The polyaryletherketone resin powder is washed with an alcohol solvent to remove interfering substances such as impurity ions, special gas adsorption, and organic residues, and then the polyaryletherketone purified product is obtained after filtering and drying;

[0027] s3. Gradient classification of resin analysis: Mix the purified polyaryletherketone product and the organic polar aprotic solvent, heat to 60°C-120°C, stir or boil under reflux for 2h-6h, filter and dry to obtain the first-grade purified polyaryletherketone product and the filtrate;

[0028] s4. Preparation of polyaryletherketones in different molecular weight ranges: polar solvents are added to the filtrate, and the precipitated solids are then washed, filtered, and dried to obtain a first-grade low molecular weight polyaryletherketone powder.

[0029] Polyaryletherketone resin materials are a type of crystalline polymer formed by connecting phenylene rings through oxygen bridges (ether bonds) and carbonyl groups (ketones). Depending on the order and proportion of the connection between ether bonds, ketone groups and benzene rings in the molecular chain, many different polymers can be formed, including but not limited to polyetheretherketone (PEEK), polyetherketone (PEK), polyetherketoneketone (PAEK), polyetheretherketoneketone (PEEKK) and polyetherketoneetherketoneketone (PEKEKK).

[0030] In a preferred embodiment, in step s1, the physical crushing and screening methods include but are not limited to air flow crushing, ultrasonic crushing, mechanical ball milling, double-roll crushing, etc., and the particle size of the polyaryletherketone powder obtained by crushing is less than or equal to 100 microns, preferably less than or equal to 50 microns, and more preferably less than or equal to 20 microns.

[0031] In a preferred embodiment, step s2 comprises: mixing the alcohol solvent and the polyaryletherketone resin powder, heating to 60°C-140°C for stirring or ultrasonic oscillation reflux for 2h-8h; cooling to 20°C-25°C, filtering, and then drying to obtain the purified polyaryletherketone product.

[0032] In a preferred embodiment, in step s2, the alcohol solvent is selected from methanol, ethanol or a combination thereof; after the alcohol solvent and the polyaryletherketone resin powder are mixed, the weight ratio of the polyaryletherketone resin powder is 30%-60%; and the drying temperature is controlled at 80°C to 120°C.

[0033] In a preferred embodiment, in s3, the organic polar aprotic solvent is selected from o-dichlorobenzene, dimethyl sulfoxide (DMSO) or N,N-dimethylformamide (DMF). The weight ratio of the purified polyaryletherketone to the organic polar aprotic solvent is 1:(1-1.4); the obtained primary pure polyaryletherketone has an intrinsic viscosity of 0.19dL / g-0.34dL / g; the filtration temperature is controlled at -20℃~60℃; the drying temperature is controlled at 80℃~120℃.

[0034] In a preferred embodiment, in s4, the polar solvent is selected from formamide, trifluoroacetic acid, DMSO, acetonitrile, DMF, hexamethylphosphoramide, methanol, ethanol, acetic acid, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine or n-butanol; the filtration temperature is controlled at -20°C to 80°C; and the drying temperature is controlled at 80°C to 150°C. The obtained primary low molecular weight polyaryletherketone powder has an intrinsic viscosity of 0.65 dL / g to 0.96 dL / g.

[0035] Example 1

[0036] In this embodiment, a method for purifying polyaryletherketone is provided, comprising the following steps:

[0037] (1) The polyaryletherketone resin material powder is physically crushed and sieved to obtain a polyaryletherketone resin powder with a particle size of about 20 μm.

[0038] (2) Weigh 65 g of polyaryletherketone resin powder into a round-bottom flask, then add 130 g of methanol. After the round-bottom flask is installed and a complete reflux device is constructed, the device temperature is set to 60° C., so that the polyaryletherketone resin powder solution in the flask is stirred and refluxed.

[0039] (3) After 6 hours, the temperature of the reflux device is set to 25°C. When the temperature of the solution in the flask stabilizes to 25°C, it is filtered. The obtained polyaryletherketone resin powder is placed in a drying oven at 100°C and dried to obtain a purified polyaryletherketone product.

[0040] (4) The purified polyaryletherketone obtained in the above step (3) is placed in a round-bottom flask, and then 65 g of o-dichlorobenzene is added to the round-bottom flask. After the round-bottom flask is installed and a complete reflux device is constructed, the device temperature is set to 120° C., so that the purified polyaryletherketone in the flask is stirred and refluxed in the o-dichlorobenzene solution.

[0041] (5) After 2 hours, the temperature was maintained at 120°C for filtration, and the primary filtrate was collected. The purified polyaryletherketone was washed with methanol at room temperature and the obtained solid was filtered. After being placed in a drying oven at 100°C, a first-level pure polyaryletherketone was obtained.

[0042] (6) Add water to the primary filtrate of step (5) to precipitate for 2 hours, filter at 80° C., wash the precipitated solid powder with methanol at room temperature, and dry at 100° C. to obtain a primary low molecular weight polyaryletherketone powder, whose intrinsic viscosity is measured to be 0.21 dL / g.

[0043] The intrinsic viscosity of the PEKK powder in the raw material is 0.54 dL / g. After being treated by the method of the present invention, the intrinsic viscosity of the obtained PEKK pure product (high molecular weight portion) is increased to 0.65 dL / g, indicating that more low molecular weight PEKK is dissolved and the intrinsic viscosity of the obtained pure product is greatly improved.

[0044] Example 2

[0045] In this embodiment, a method for purifying polyaryletherketone is provided, comprising the following steps:

[0046] (1) The polyaryletherketone resin material powder is physically crushed and sieved to obtain a polyaryletherketone resin powder with a particle size of about 20 μm.

[0047] (2) Weigh 65 g of polyaryletherketone resin powder into a round-bottom flask, then add 130 g of methanol. After the round-bottom flask is installed and a complete reflux device is constructed, the device temperature is set to 60° C., so that the polyaryletherketone resin powder solution in the flask is stirred and refluxed.

[0048] (3) After 6 hours, the temperature of the reflux device is set to 25°C. When the temperature of the solution in the flask stabilizes to 25°C, it is filtered. The obtained polyaryletherketone resin powder is placed in a drying oven at 100°C and dried to obtain a purified polyaryletherketone product.

[0049] (4) The purified polyaryletherketone obtained in the above step (3) is placed in a round-bottom flask, and then 80 g of dimethyl sulfoxide (DMSO) is added to the round-bottom flask. After the round-bottom flask is installed and a complete reflux device is constructed, the device temperature is set to 120° C., so that the purified polyaryletherketone in the flask is stirred and refluxed in the o-dichlorobenzene solution.

[0050] (5) After 2 hours, the temperature was maintained at 120°C for filtration, and the primary filtrate was collected. The PEKK was washed with methanol at room temperature and the obtained solid was filtered. After being placed in a drying oven at 100°C and dried, a first-grade pure polyaryletherketone was obtained.

[0051] (6) Add water to the primary filtrate of step (5) to precipitate for 2 hours, filter at 80° C., wash the precipitated solid powder with methanol at room temperature, and dry at 100° C. to obtain a primary low molecular weight polyaryletherketone powder, whose intrinsic viscosity is measured to be 0.34 dL / g.

[0052] The intrinsic viscosity of the PEKK powder in the raw material is 0.54 dL / g. After being treated by the method of the present invention, the intrinsic viscosity of the obtained PEKK pure product (high molecular weight portion) is increased to 0.96 dL / g, indicating that more low molecular weight PEKK is dissolved and the intrinsic viscosity of the obtained pure product is greatly improved.

[0053] Example 3

[0054] In this embodiment, a method for purifying polyaryletherketone is provided, comprising the following steps:

[0055] (1) The polyaryletherketone resin material powder is physically crushed and sieved to obtain a polyaryletherketone resin powder with a particle size of about 20 μm.

[0056] (2) Weigh 65 g of polyaryletherketone resin powder into a round-bottom flask, then add 130 g of methanol. After the round-bottom flask is installed and a complete reflux device is constructed, the device temperature is set to 60° C., so that the polyaryletherketone resin powder solution in the flask is stirred and refluxed.

[0057] (3) After 6 hours, the temperature of the reflux device is set to 25°C. When the temperature of the solution in the flask stabilizes to 25°C, it is filtered. The obtained polyaryletherketone resin powder is placed in a drying oven at 100°C and dried to obtain a purified polyaryletherketone product.

[0058] (4) The purified polyaryletherketone obtained in the above step (3) is placed in a round-bottom flask, and then 65 g of N,N-dimethylformamide (DMF) is added to the round-bottom flask. After the round-bottom flask is installed and a complete reflux device is constructed, the device temperature is set to 120° C., so that the purified polyaryletherketone in the flask is stirred and refluxed in the o-dichlorobenzene solution.

[0059] (5) After 2 hours, the temperature was maintained at 120°C for filtration, and the primary filtrate was collected. The purified polyaryletherketone was washed with methanol at room temperature and the obtained solid was filtered. After being placed in a drying oven at 100°C, a first-level pure polyaryletherketone was obtained.

[0060] (6) Add water to the primary filtrate of step (5) to precipitate for 2 hours, filter at 80° C., wash the precipitated solid powder with methanol at room temperature, and dry at 100° C. to obtain a primary low molecular weight polyaryletherketone powder, whose intrinsic viscosity is measured to be 0.19 dL / g.

[0061] The intrinsic viscosity of the PEKK powder in the raw material is 0.54 dL / g. After being treated by the method of the present invention, the intrinsic viscosity of the obtained PEKK pure product (high molecular weight portion) is increased to 0.72 dL / g, indicating that more low molecular weight PEKK is dissolved and the intrinsic viscosity of the obtained pure product is greatly improved.

[0062] Example 4

[0063] In this embodiment, a method for purifying polyaryletherketone is provided, comprising the following steps:

[0064] (1) The polyaryletherketone resin material powder is physically crushed and sieved to obtain a polyaryletherketone resin powder with a particle size of about 20 μm.

[0065] (2) Weigh 65 g of polyaryletherketone resin powder into a round-bottom flask, and then add 130 g of methanol (one or more alcohols). After the round-bottom flask is installed and a complete reflux device is constructed, the device temperature is set to 60°C so that the polyaryletherketone resin powder solution in the flask is stirred and refluxed.

[0066] (3) After 6 hours, the temperature of the reflux device is set to 25°C. When the temperature of the solution in the flask stabilizes to 25°C, it is filtered. The obtained polyaryletherketone resin powder is placed in a drying oven at 100°C and dried to obtain a purified polyaryletherketone product.

[0067] (4) The purified polyaryletherketone obtained in the above step (3) is placed in a round-bottom flask, and then 80 g of N,N-dimethylformamide (DMF) is added to the round-bottom flask. After the round-bottom flask is installed and a complete reflux device is constructed, the device temperature is set to 120° C., so that the purified polyaryletherketone in the flask is stirred and refluxed in the o-dichlorobenzene solution.

[0068] (5) After 2 hours, the temperature was maintained at 120°C for filtration, and the primary filtrate was collected. The purified polyaryletherketone was washed with methanol at room temperature and the obtained solid was filtered. After being placed in a drying oven at 100°C, a first-level pure polyaryletherketone was obtained.

[0069] (6) Add water to the primary filtrate of step (5) to precipitate for 2 hours, filter at 80° C., wash the precipitated solid powder with methanol at room temperature, and dry at 100° C. to obtain a primary low molecular weight polyaryletherketone powder, whose intrinsic viscosity is measured to be 0.27 dL / g.

[0070] The intrinsic viscosity of the PEKK powder in the raw material is 0.54 dL / g. After being treated by the method of the present invention, the intrinsic viscosity of the obtained PEKK pure product (high molecular weight portion) is increased to 0.85 dL / g, indicating that more low molecular weight PEKK is dissolved and the intrinsic viscosity of the obtained pure product is greatly improved.

[0071] It can be seen from the above embodiments that the intrinsic viscosity test result of the polyaryletherketone (PEKK) raw material is 0.54 dL / g, and after adopting the treatment method of the present invention, the intrinsic viscosity of the high molecular weight polyaryletherketone (PEKK) resin can be increased to 0.65-0.96 dL / g, but through the above treatment method, a low molecular weight polyaryletherketone (PEKK) powder with a low intrinsic viscosity (0.19-0.34 dL / g) can also be obtained.

[0072] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for purifying polyaryletherketone, characterized in that: The method comprises: s1. physically crushing the polyaryletherketone resin material to obtain a polyaryletherketone resin powder having a particle size less than or equal to 100 μm; s2, washing the polyaryletherketone resin powder with an alcohol solvent, and then filtering and drying to obtain a purified polyaryletherketone product; s3. Mix the purified polyaryletherketone product and the organic polar aprotic solvent, heat to 60°C-120°C, stir or boil under reflux for 2h-6h, filter and dry to obtain a first-grade purified polyaryletherketone product and a filtrate; s4. Add a polar solvent to the filtrate, wash, filter and dry the precipitated solid to obtain a first-grade low molecular weight polyaryletherketone powder.

2. The method for purifying polyaryletherketone according to claim 1, characterized in that: The alcohol solvent is selected from methanol, ethanol or a combination thereof.

3. The method for purifying polyaryletherketone according to claim 1, characterized in that: In s4, the polar solvent is selected from formamide, trifluoroacetic acid, DMSO, acetonitrile, DMF, hexamethylphosphoramide, methanol, ethanol, acetic acid, isopropanol, pyridine, tetramethylethylenediamine, acetone, triethylamine or n-butanol.

4. The method for purifying polyaryletherketone according to claim 1, characterized in that: The s2 includes: After mixing the alcohol solvent and the polyaryletherketone resin powder, heat to 60°C-140°C and stir or reflux under ultrasonic oscillation for 2h-8h; The mixture is cooled to 20°C-25°C, filtered, and then dried to obtain a purified polyaryletherketone product.

5. The method for purifying polyaryletherketone according to claim 4, characterized in that: After the alcohol solvent and the polyaryletherketone resin powder are mixed, the weight ratio of the polyaryletherketone resin powder is 30%-60%.

6. The method for purifying polyaryletherketone according to claim 1, characterized in that: In the above s1, the physical crushing method is selected from air flow crushing, ultrasonic crushing, mechanical ball milling or double roller crushing.

7. The method for purifying polyaryletherketone according to claim 1, characterized in that: In s3, the organic polar aprotic solvent is selected from o-dichlorobenzene, dimethyl sulfoxide (DMSO) or N,N-dimethylformamide (DMF).

8. The method for purifying polyaryletherketone according to claim 1, characterized in that: In the above s3, the weight ratio of the purified polyaryletherketone to the organic polar aprotic solvent is 1:(1-1.4).

9. The method for purifying polyaryletherketone according to claim 1, characterized in that: In the s3, the intrinsic viscosity of the first-grade pure polyaryletherketone is 0.19 dL / g-0.34 dL / g.

10. The method for purifying polyaryletherketone according to claim 1, characterized in that: In the s4, the primary low molecular weight polyaryletherketone powder has an intrinsic viscosity of 0.65 dL / g-0.96 dL / g.

Citation Information

Patent Citations

  • Post-treatment method of soluble poly(aryl ether ketone) resin

    CN107936244A

  • Purification method for preparing polyaryletherketone by electrophilic method

    CN111349231A

  • Method for controlling molecular weight distribution of polyetherketoneketone

    CN115058003A