Method for extracting lignin from brewer's grains

Through the combination of mechanical enrichment and deep eutectic solvent/γ-valerolactone biphasic solvent, the problems of high cost and pollution in the extraction process of lignin from brewer's grains are solved, and efficient and green lignin extraction is achieved, which improves the efficiency of lignin extraction. purity and extraction efficiency.

CN118725339APending Publication Date: 2024-10-01SOUTH CHINA UNIV OF TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411018424.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology has problems such as high cost, environmental pollution, and equipment corrosion when extracting lignin from brewer's grains. Moreover, the high water content and component heterogeneity of brewer's grains make the traditional crushing and grinding treatment ineffective, affecting the separation of lignin. extract.

Method used

The method of mechanical enrichment-assisted deep eutectic solvent/γ-valerolactone biphasic solvent is used to prepare lignocellulosic raw materials through hydrolysis, sieving and drying. The hydrogen bond acceptor and donor are combined to form a deep eutectic solvent, and then added γ-valerolactone forms a biphasic solvent and reacts with the lignocellulosic fiber, and the lignin is extracted through a purification step.

Benefits of technology

It improves the extraction efficiency and purity of lignin, reduces environmental pollution, conforms to the concept of green and environmentally friendly development, and reduces the impact of protein on extraction through physical screening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725339A_ABST
    Figure CN118725339A_ABST
Patent Text Reader

Abstract

The invention relates to a method for extracting lignin from brewer's grains, which comprises the following steps: (1) mechanically enriching wet brewer's grains to prepare a wood fiber raw material; (2) providing a dual-phase solvent of a eutectic solvent and gamma-valerolactone; and (3) mixing the wood fiber raw material with the two-phase solvent for reaction, and purifying the obtained reaction product to prepare the lignin. According to the method, the lignin in the brewer's grains can be efficiently extracted through the mechanical enrichment assisted eutectic solvent / gamma-valerolactone biphasic solvent, and the purity is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of biomass refining, and specifically relates to a method for extracting lignin from brewer's grains. Background Art

[0002] At present, the treatment of grain by-products among industrial wastes is a hot topic. As the largest country in beer brewing and consumption, my country's beer brewing industry has produced more than 10 million tons of solid waste brewer's grains. It is the main solid by-product in beer production, accounting for 85% of beer by-products. Brewer's grains are rich in wood fiber and protein, and are usually treated as animal feed. However, the high water content makes brewer's grains difficult to transport and store, and there are certain limitations as feed additives. Direct disposal or filling disposal is likely to cause environmental pollution. Among them, lignin is one of the most abundant natural polymers in nature and the only non-petroleum resource in nature that can provide renewable aromatic compounds. Therefore, in order to improve the resource utilization of brewer's grains, it is necessary to use reasonable methods and select green solvents to efficiently extract lignin from brewer's grains wood fiber.

[0003] The traditional methods for separating and extracting lignin from brewer's grains mainly use treatments with inorganic acids / alkalis, biological enzymes, organic solvents and other substances. These methods will increase costs, pollute the environment, corrode equipment and other disadvantages during the extraction process.

[0004] Before / during chemical solvent treatment, wood fiber will be treated with physical methods, such as crushing and grinding, ultrasound assistance, etc. However, due to the uneven size and shape of the components in the brewer's grains, if they are mixed and crushed and ground, the components of the separated brewer's grains cannot be well utilized, and the presence of protein will affect the separation and extraction of lignin. Summary of the invention

[0005] Based on this, it is necessary for the present application to provide a method for efficiently extracting lignin from brewer's grains by using a mechanical enrichment-assisted low eutectic solvent / γ-valerolactone biphasic solvent, and the purity of the lignin is high.

[0006] The technical solutions include the following:

[0007] A method for extracting lignin from brewer's grains comprises the following steps:

[0008] (1) Mechanically enriching wet brewer's grains to prepare lignocellulosic raw materials;

[0009] (2) providing a deep eutectic solvent and a biphasic solvent of γ-valerolactone; and,

[0010] (3) The wood fiber raw material is mixed with the two-phase solvent for reaction, and the obtained reaction product is purified to prepare lignin.

[0011] In one embodiment, in step (1), the mechanical enrichment step includes: hydrolyzing wet brewer's grains, screening, drying, and preparing a wood fiber raw material. Optionally, the number of revolutions of the hydrolyzing is 20,000-40,000. Optionally, the drying temperature is 58° C.-62° C. Optionally, the wood fiber raw material has a particle size of 0.8 mm or more and a moisture content of 4%-5%.

[0012] In one embodiment, in step (2), the preparation step of the biphasic solvent includes: mixing a hydrogen bond acceptor and a hydrogen bond donor, heating and stirring to form a low eutectic solvent, and then adding γ-valerolactone and stirring to prepare a biphasic solvent.

[0013] In one embodiment, the hydrogen bond acceptor is choline chloride, and the hydrogen bond donor is selected from at least one of p-toluenesulfonic acid monohydrate, p-hydroxybenzenesulfonic acid, benzenesulfonic acid, ethanolamine and 3-aminopropanol.

[0014] In one embodiment, the preparation of a biphasic solvent requires one or more of the following conditions to be met:

[0015] The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:(0.5-6);

[0016] The amount of γ-valerolactone added to the biphasic solvent is 40%-70%; and

[0017] The heating temperature is 60°C-100°C.

[0018] In one embodiment, in step (3), the mass ratio of the wood fiber raw material to the biphasic solvent is 1:(10-20).

[0019] In one embodiment, the temperature of the mixed reaction is 80° C.-120° C., and the time of the mixed reaction is 1 h to 3 h.

[0020] In one embodiment, the purification step includes cooling the reaction product, washing it for the first time and collecting the concentrate, adding water, standing it for precipitation, separating the precipitate, washing it for the second time, and drying it to prepare lignin.

[0021] In one embodiment, the medium for the first washing is an aqueous solution of ethanol. Optionally, the volume ratio of ethanol to water in the aqueous solution of ethanol is 19:1-9:1. Optionally, the amount of the aqueous solution of ethanol added is 1-3 times the volume of the reaction solution.

[0022] In one embodiment, the amount of water added is 10 to 15 times the volume of the concentrate.

[0023] Optionally, the static sedimentation time is 12h-24h.

[0024] In one embodiment, the second washing medium is water, and its pH value is 6.8-7.2. Optionally, the number of washings is 2-3 times.

[0025] Compared with the traditional technology, this application has the following beneficial effects:

[0026] The present application provides a method for extracting lignin after processing brewer's grains biomass lignocellulosic raw materials, which reasonably enriches the lignocellulosic components in the brewer's grains through physical screening, and effectively reduces the influence of protein in the brewer's grains on the extraction of lignin.

[0027] In the green two-phase solvent treatment of the present application, when a low eutectic solvent (DES) system is used to treat brewer's grains wood fiber enrichment, a γ-valerolactone (GVL) green organic solvent is introduced to increase the activity of lignin ether bonds and accelerate the breakage of β-O-4 aromatic ether bonds in lignin, thereby separating lignin, improving lignin extraction efficiency, and achieving high purity.

[0028] The various solvents used in this application, such as deionized water, ethanol, green two-phase solvents, etc., have no special requirements for equipment and can be reused through multiple cycles, effectively reducing environmental pollution and other issues, and complying with the green environmental protection development concept. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the process flow chart of brewer's grains lignin extraction.

[0030] Figure 2 This is the infrared spectrum of the extracted brewer's grains lignin. Transmittance represents transmittance, and Wavenumber represents wavenumber.

[0031] Figure 3 For the extraction of brewer's grains lignin. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0034] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0035] Deep eutectic solvents (DES) have the characteristics of easy preparation, low price, environmental friendliness, biodegradability, designable structure, good chemical and thermal stability. However, due to the large molecular weight, high viscosity and slow diffusion of the low eutectic system, the use of DES alone usually has the disadvantages of long processing time and unsatisfactory treatment effect. γ-Valerolactone (GVL), as a new type of green solvent, not only overcomes the non-renewable nature of fossil energy solvents, but also weakens the threat of traditional solvents to the environment and human health. It is an ideal candidate for organic solvents for biomass pretreatment. The present application found that the introduction of GVL into the DES system can not only reduce the viscosity of the DES system and accelerate the diffusion of the solvent system, but also increase the activity of the lignin ether bond and accelerate the breakage of the β-O-4 aromatic ether bond, thereby improving the separation efficiency of lignin.

[0036] An embodiment of the present application provides a method for extracting lignin from brewer's grains, comprising the following steps (1) to (3):

[0037] Step (1), mechanically enriching wet brewer's grains to prepare wood fiber raw materials. Mechanical screening and enrichment can effectively improve the yield of lignin extracted by DES / GVL green two-phase solvent.

[0038] In one specific example, the step of mechanical enrichment includes: hydroflushing wet brewer's grains, screening, and drying to prepare a lignocellulosic raw material.

[0039] In a specific example, the particle size of the wood fiber raw material is greater than 0.8 mm and the moisture content is 4%-5%.

[0040] In a specific example, the number of revolutions of the hydraulic decongestion is 20,000-40,000, and optional values ​​include but are not limited to 20,000, 25,000, 30,000, 35,000 or 40,000.

[0041] In a specific example, the drying temperature is 58°C-62°C, and optional values ​​include but are not limited to 58°C, 59°C, 60°C, 61°C or 62°C.

[0042] In a specific example, wet spent grains with a moisture content of 80%-85% and water are mixed at a solid-liquid ratio of 1:10, hydrolyzed at 20,000-40,000 rpm, sieved, and dried at 60°C to a moisture content of 4%-5%, and the brewer's spent grains wood fiber raw material with a particle size of 0.8 mm or more is collected.

[0043] Step (2), providing a low eutectic solvent and a biphasic solvent of γ-valerolactone.

[0044] In a specific example, a hydrogen bond acceptor and a hydrogen bond donor are mixed, heated and stirred to form a low eutectic solvent, and then γ-valerolactone is added and stirred to prepare a biphasic solvent.

[0045] In a specific example, the hydrogen bond acceptor is choline chloride, and the hydrogen bond donor is selected from at least one of p-toluenesulfonic acid monohydrate, p-hydroxybenzenesulfonic acid, benzenesulfonic acid, ethanolamine and 3-aminopropanol. Preferably, the hydrogen bond donor is selected from p-toluenesulfonic acid monohydrate, p-hydroxybenzenesulfonic acid, benzenesulfonic acid.

[0046] The process of the present application uses acidic DES / GVL to extract brewer's grains lignin, which further improves the lignin extraction rate and purity, obtains low molecular weight lignin, is conducive to the production of high-value lignin products, and thus improves the utilization value of lignin.

[0047] In a specific example, the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:(0.5-6), and optional values ​​include but are not limited to 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5 or 1:6.

[0048] In a specific example, the amount of γ-valerolactone added to the biphasic solvent is 40%-70%, and optional values ​​include but are not limited to 40%, 50%, 60% or 70%.

[0049] In a specific example, the heating temperature is 60°C-100°C, and optional values ​​include but are not limited to 60°C, 70°C, 80°C, 90°C or 100°C.

[0050] In a specific example, the stirring time is 25 min-35 min.

[0051] In a specific example, the stirring speed is 250 rpm-350 rpm.

[0052] Step (3), mixing the wood fiber raw material with the biphasic solvent for reaction, and purifying the obtained reaction product to prepare lignin.

[0053] In a specific example, the mass ratio of the wood fiber raw material to the biphasic solvent is 1:(10-20), and optional values ​​include but are not limited to 1:10, 1:15 or 1:20.

[0054] In a specific example, the conditions of the mixing reaction include a temperature of 80-120° C., a time of 1-3 h, and a stirring speed of 250 rpm-350 rpm.

[0055] In a specific example, the purification step includes cooling the reaction product, washing it for the first time and collecting the concentrate, adding water, standing it for precipitation, separating the precipitate, washing it for the second time, and drying it to prepare lignin.

[0056] In one specific example, the medium for the first wash is an aqueous solution of ethanol.

[0057] In a specific example, the volume ratio of ethanol to water in the aqueous solution of ethanol is 19:1-9:1;

[0058] In a specific example, the amount of ethanol aqueous solution added is 1 to 3 times the volume of the reaction solution.

[0059] In one specific example, the concentrate is collected by rotary evaporation.

[0060] In a specific example, the amount of water added is 10 to 15 times the volume of the concentrate.

[0061] In a specific example, the static sedimentation time is 12h-24h, and optional values ​​include but are not limited to 12h, 15h, 18h, 20h, 22h or 24h.

[0062] In one specific example, the water is deionized water.

[0063] In a specific example, the medium for the second washing is deionized water with a pH value of 6.8-7.2, and optionally, a pH value of 7.0.

[0064] In a specific example, the number of washes is 2-3 times.

[0065] In a specific example, the drying temperature is 100° C.-105° C., and the drying time is 3 h-4 h.

[0066] The embodiments of the present application will be described in detail below in conjunction with examples. It should be understood that these examples are only used to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are preferably referred to the guidance provided in the present application, and can also be based on the experimental manual or normal conditions in this area, can also be based on the conditions recommended by the manufacturer, or refer to experimental methods known in the art.

[0067] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.

[0068] In the following examples, the lignin content in the raw material was determined with reference to the technical report of the National Renewable Energy Laboratory of the United States, technical report number: NREL / TP-510-42618 "Determination of Structural Carbohydrates and Lignin in Biomass"; the protein content was determined by the Kjeldahl method with reference to GB 5009.5-2016 "National Food Safety Standard Determination of Protein in Food".

[0069] The lignin extraction rate and the purity of the extracted lignin in the following examples are calculated according to the following formula:

[0070] 1. Lignin extraction rate:

[0071]

[0072] W1——lignin extraction rate, %;

[0073] m1——mass of lignin extracted by biphasic solvent treatment, g;

[0074] m0——the mass of raw materials used for two-phase solvent treatment, g;

[0075] α——The content of lignin in raw materials, %.

[0076] 2. Extraction lignin purity:

[0077]

[0078] W2——Purity of lignin extracted by biphasic solvent, %;

[0079] m1——mass of lignin extracted by biphasic solvent treatment, g;

[0080] m2——the mass of acid-insoluble lignin in the lignin extracted by biphasic solvent, g;

[0081] m3——The mass of acid-soluble lignin in the lignin extracted by two-phase solvent, g.

[0082] β——Protein content in lignin extracted by two-phase solvent, %.

[0083] In the following examples, the wet brewer's grains were from the Snow Beer factory, which uses barley as the main fermentation raw material. Figure 1

[0084] Example 1

[0085] (1) Enrichment of wood fiber raw materials: The wet brewer's grains were hydrolyzed at 20,000 rpm, and the brewer's grains wood fiber concentrate was screened through a 0.8 mm sieve and dried at 60 °C to a moisture content of 4-5%.

[0086] (2) Green biphasic solvent synthesis: Choline chloride (ChCl) and benzenesulfonic acid hydrate were mixed in a molar ratio of 1:2 (6.22 g:8.78 g), heated and stirred at 80 °C for 30 min, and mixed until clear. Then 70% γ-valerolactone (35 g) was added and stirred evenly at a stirring speed of 300 rpm.

[0087] (3) Extraction of lignin from brewer's grains: 5 g of brewer's grains wood fiber concentrate was mixed with 50 g of a biphasic solvent for reaction, heated and stirred at 90 °C for 1 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0088] The results show that after the wet brewer's grains are treated with the mechanical enrichment assisted DES / GVL biphasic solvent (choline chloride / benzenesulfonic acid / 70% γ-valerolactone) of the present application, the extraction rate of lignin is 83%±1%, and the purity of the extracted lignin is 82%±1%.

[0089] Example 2

[0090] (1) Enrichment of wood fiber raw materials: The wet brewer's grains were hydrolyzed at 20,000 rpm, and the brewer's grains wood fiber concentrate was screened through a 0.8 mm sieve and dried at 60 °C to a moisture content of 4-5%.

[0091] (2) Synthesis of green biphasic solvent: Choline chloride (ChCl) and p-hydroxybenzenesulfonic acid hydrate were mixed in a molar ratio of 1:2 (4.28 g:10.74 g), heated and stirred at 80 °C for 30 min, and mixed until clear. Then 70% γ-valerolactone (35 g) was added and stirred evenly at a stirring speed of 300 rpm.

[0092] (3) Extraction of lignin from brewer's grains: 5 g of brewer's grains wood fiber concentrate was mixed with 50 g of a biphasic solvent for reaction, heated and stirred at 90 °C for 1 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0093] The results show that after the wet brewer's grains are treated with the mechanical enrichment assisted DES / GVL biphasic solvent (choline chloride / p-hydroxybenzenesulfonic acid / 70% γ-valerolactone) of the present application, the extraction rate of lignin is 87%±1%, and the purity of the extracted lignin is 85%±1%.

[0094] Example 3

[0095] (1) Enrichment of wood fiber raw materials: The wet brewer's grains were hydrolyzed at 20,000 rpm, and the brewer's grains wood fiber concentrate was screened through a 0.8 mm sieve and dried at 60 °C to a moisture content of 4-5%.

[0096] (2) Green biphasic solvent synthesis: Choline chloride (ChCl) and p-toluenesulfonic acid monohydrate were mixed in a molar ratio of 1:1 (6.23 g:8.68 g), heated and stirred at 80 °C for 30 min, and mixed until clear. Then 70% γ-valerolactone (35 g) was added and stirred evenly at a stirring speed of 300 rpm.

[0097] (3) Extraction of lignin from brewer's grains: 5 g of dried brewer's grains wood fiber concentrate was mixed with 50 g of a biphasic solvent for reaction, heated and stirred at 90 °C for 1 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0098] The results show that after the wet brewer's grains are treated with the mechanical enrichment assisted DES / GVL biphasic solvent (choline chloride / p-toluenesulfonic acid / 70% γ-valerolactone) of the present application, the extraction rate of lignin is 89%±1%, and the purity of the extracted lignin is 84%±1%.

[0099] Example 4

[0100] (1) Enrichment of wood fiber raw materials: The wet brewer's grains were hydrolyzed at 20,000 rpm, and the brewer's grains wood fiber concentrate was screened through a 0.8 mm sieve and dried at 60 °C to a moisture content of 4-5%.

[0101] (2) Synthesis of green biphasic solvent: Choline chloride (ChCl) and p-toluenesulfonic acid monohydrate were mixed in a molar ratio of 1:1 (8.42 g:11.58 g), heated and stirred at 80 °C for 30 min, and mixed until clear. Then 60% γ-valerolactone (30 g) was added and stirred evenly at a stirring speed of 300 rpm.

[0102] (3) Extraction of lignin from brewer's grains: 5 g of dry brewer's grains raw material was mixed with 50 g of biphasic solvent for reaction, heated and stirred at 90 °C for 1 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0103] The results show that after the wet brewer's grains are treated with the mechanical enrichment assisted DES / GVL biphasic solvent (choline chloride / p-toluenesulfonic acid / 60% γ-valerolactone) of the present application, the extraction rate of lignin is 90%±1%, and the purity of the extracted lignin is 81%±1%.

[0104] Example 5

[0105] (1) Enrichment of wood fiber raw materials: The brewer's grains were hydrolyzed at 25,000 rpm, and the brewer's grains wood fiber concentrate was screened and enriched through a 0.8 mm sieve, and then dried at 60 °C to a moisture content of 4-5%.

[0106] (2) Green biphasic solvent synthesis: Choline chloride (ChCl) and 3-aminopropanol were mixed at a molar ratio of 1:6 (5.90 g:19.1 g), heated and stirred at 90 °C for 30 min, and mixed until clear. Then 50% γ-valerolactone (25 g) was added and stirred evenly at a stirring speed of 300 rpm.

[0107] (3) Extraction of lignin from brewer's grains: 5 g of brewer's grains wood fiber concentrate was mixed with 50 g of a biphasic solvent for reaction, heated and stirred at 120 °C for 4 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0108] The results show that after the wet brewer's grains are treated with the mechanical enrichment assisted DES / GVL biphasic solvent (choline chloride / 3-aminopropanol / 50% γ-valerolactone) of the present application, the extraction rate of lignin is 75%±1%, and the purity of the extracted lignin is 83%±1%.

[0109] Example 6

[0110] (1) Enrichment of wood fiber raw materials: The brewer's grains were hydrolyzed at 25,000 rpm, and the brewer's grains wood fiber concentrate was screened and enriched through a 0.8 mm sieve, and then dried at 60 °C to a moisture content of 4-5%.

[0111] (2) Green biphasic solvent synthesis: Choline chloride (ChCl) and 3-aminopropanol were mixed at a molar ratio of 1:6 (7.08 g: 22.92 g), heated and stirred at 90 °C for 30 min, and mixed until clear. Then 40% γ-valerolactone (20 g) was added and stirred evenly at a stirring speed of 300 rpm.

[0112] (3) Extraction of lignin from brewer's grains: 5 g of brewer's grains wood fiber concentrate was mixed with 50 g of a biphasic solvent for reaction, heated and stirred at 120 °C for 4 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0113] The results show that after the wet brewer's grains are treated with the mechanical enrichment assisted DES / GVL biphasic solvent (choline chloride / 3-aminopropanol / 40% γ-valerolactone) of the present application, the extraction rate of lignin is 78%±1%, and the purity of the extracted lignin is 84%±1%.

[0114] Example 7

[0115] (1) Enrichment of wood fiber raw materials: The brewer's grains were hydrolyzed at 20,000 rpm, and the brewer's grains wood fiber concentrate was screened and enriched through a 0.8 mm sieve, and then dried at 60 °C to a moisture content of 4-5%.

[0116] (2) Synthesis of green biphasic solvent: Choline chloride (ChCl) and ethanolamine were mixed at a molar ratio of 1:6 (8.26 g: 21.74 g), heated and stirred at 90 °C for 30 min, and mixed until clear. Then 40% γ-valerolactone (20 g) was added and stirred evenly at a stirring speed of 300 rpm.

[0117] (3) Extraction of lignin from brewer's grains: 5 g of brewer's grains wood fiber concentrate was mixed with 50 g of a biphasic solvent for reaction, heated and stirred at 120 °C for 4 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0118] The results show that after the wet brewer's grains are treated with the mechanical enrichment assisted DES / GVL biphasic solvent (choline chloride / ethanolamine / 40% γ-valerolactone) of the present application, the extraction rate of lignin is 79%±1%, and the purity of the extracted lignin is 82%±1%.

[0119] Table 1 Lignin extraction conditions, extraction rate, purity

[0120]

[0121] Table 1 shows the lignin extraction conditions, lignin extraction rate and lignin purity in each embodiment. It can be seen from the table that:

[0122] (1) In Examples 1 to 3, as the benzenesulfonic acid group changes, the acidity coefficient increases. The treatment method of combining acidic DES / GVL with mechanical enrichment of wood fiber raw materials can improve the extraction rate of brewer's grains lignin. Under low temperature and short time treatment conditions, the maximum extraction efficiency can be 89±1%, and the highest purity can reach 85±1%.

[0123] (2) Example 3-Example 4: As the concentration of GVL decreases, the acidic DES content in the system increases, the destructive ability to wood fiber is enhanced, and the lignin extraction efficiency is slightly improved. However, due to the destruction of cellulose under the treatment of the strong acidic DES, the purity of lignin decreases, but it can still reach 81%.

[0124] (3) Example 5-Example 7, the hydrogen bond donor of DES was changed. Although the raw material treated with alkaline DES / GVL was inferior to that treated with acidic DES / GVL, with the increase of the molar ratio of the donor, the increase of the reaction temperature and the decrease of the GVL concentration, the alkaline DES / GVL treatment of brewer's grains could obtain a maximum extraction efficiency of 79%±1% and a maximum purity of 83%±1%.

[0125] Comparative Example 1

[0126] (1) The brewer's grains are dried at 60°C to a moisture content of 4-5% without being subjected to decomposition, screening and enrichment treatment.

[0127] (2) Synthesis of green biphasic solvent: Choline chloride (ChCl) and p-toluenesulfonic acid monohydrate were mixed in a molar ratio of 1:1 (8.42 g:11.58 g), heated and stirred at 80 °C for 30 min, and mixed until clear. Then 60% γ-valerolactone (30 g) was added and stirred evenly at a stirring speed of 300 rpm.

[0128] (3) Extraction of lignin from brewer's grains: 5 g of dry brewer's grains raw material was mixed with 50 g of biphasic solvent for reaction, heated and stirred at 90 °C for 1 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0129] The results showed that the extraction rate of lignin from wet brewer's grains without screening was 78%±1% after being treated with DES / GVL biphasic solvent (choline chloride / p-toluenesulfonic acid / 60% γ-valerolactone), and the purity of the extracted lignin was 82%±1%.

[0130] Comparative Example 2

[0131] (1) Enrichment of wood fiber raw materials: The brewer's grains were hydrolyzed at 20,000 rpm, and the brewer's grains wood fiber concentrate was screened and enriched through a 0.8 mm sieve, and then dried at 60 °C to a moisture content of 4-5%.

[0132] (2) Synthesis of green biphasic solvent: Choline chloride (ChCl) and ethanolamine were mixed in a molar ratio of 1:6 (13.76 g:36.24 g), heated and stirred at 90 °C for 30 min, and mixed until clear.

[0133] (3) Extraction of lignin from brewer's grains: 5 g of brewer's grains wood fiber concentrate was mixed with 50 g of a biphasic solvent for reaction, heated and stirred at 120 °C for 4 h, and cooled to room temperature after the reaction was completed to obtain a reaction product. Ethanol (95%) was added to the reaction product, stirred, washed 2-3 times (100 ml each time), filtered, concentrated, added 500 ml of water, allowed to stand, precipitated, and centrifuged to obtain a precipitate containing lignin, which was washed 2-3 times with deionized water (20 ml each time), and dried to obtain lignin.

[0134] The results showed that after the wet brewer's grains were screened and treated with DES solvent, the extraction rate of lignin was 65%±1%, and the purity of the extracted lignin was 80%±1%.

[0135] Comparative Example 1 is a comparative case of Example 4. In Example 4, the brewer's grains lignocellulosic raw materials were screened and enriched, and the effect of treatment with DES / GVL green biphasic solvent was better than that of Comparative Example 1 without screening treatment. The lignin extraction efficiency was increased from 78% to 90%, and the lignin purity was not much different. This shows that mechanical screening enrichment can effectively improve the efficiency of DES / GVL green biphasic solvent extraction of lignin.

[0136] Comparative Example 2 is a comparative case of Example 7. The treatment effect of Example 7 with the addition of GVL is better than that of Comparative Example 2 without the addition of GVL. The lignin extraction efficiency is increased from 65% to 79%, and the lignin purity is not much different. This shows that GVL can effectively improve the efficiency of DES / GVL green two-phase solvent extraction of lignin.

[0137] In summary, this application uses brewer's grain biomass as raw material, firstly obtains brewer's grain wood fiber concentrate by mechanical screening enrichment, and then extracts brewer's grain lignin component by DES / GVL green biphasic solvent treatment. During the entire preparation process, the experimental operation is relatively simple, the reaction conditions are relatively mild, and the lignin extraction effect is good. The research results of this invention provide a theoretical basis and technical support for the comprehensive study of brewer's grain biomass and the efficient utilization of lignocellulosic resource biomass.

[0138] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0139] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.

Claims

1. A method for extracting lignin from brewer's grains, characterized in that: The steps include: (1) Mechanically enriching wet brewer's grains to prepare lignocellulosic raw materials; (2) providing a deep eutectic solvent and a biphasic solvent of γ-valerolactone; and, (3) The wood fiber raw material is mixed with the two-phase solvent for reaction, and the obtained reaction product is purified to prepare lignin.

2. The method according to claim 1, characterized in that In step (1), the mechanical enrichment step includes: hydraulically degassing the wet brewer's grains, screening, drying, and preparing a wood fiber raw material; Optionally, the number of revolutions of the hydraulic decongestion is 20,000-40,000; Optionally, the drying temperature is 58°C-62°C; Optionally, the wood fiber raw material has a particle size of more than 0.8 mm and a moisture content of 4%-5%.

3. The method according to claim 1 or 2, characterized in that: In step (2), the preparation step of the biphasic solvent includes: mixing the hydrogen bond acceptor and the hydrogen bond donor, heating and stirring to form a low eutectic solvent, and then adding γ-valerolactone and stirring to prepare a biphasic solvent.

4. The method according to claim 3, characterized in that The hydrogen bond acceptor is choline chloride, and the hydrogen bond donor is selected from at least one of p-toluenesulfonic acid monohydrate, p-hydroxybenzenesulfonic acid, benzenesulfonic acid, ethanolamine and 3-aminopropanol.

5. The method according to claim 4, characterized in that The preparation of biphasic solvents requires one or more of the following conditions to be met: The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:(0.5-6); The amount of γ-valerolactone added to the biphasic solvent is 40%-70%; and The heating temperature is 60°C-100°C.

6. The method according to claim 5, characterized in that In step (3), the mass ratio of the wood fiber raw material to the biphasic solvent is 1:(10-20); and / or, The temperature of the mixed reaction is 80°C-120°C, and the time of the mixed reaction is 1h-3h.

7. The method according to claim 6, characterized in that The purification steps include cooling the reaction product, washing it for the first time and collecting the concentrated liquid, adding water, standing it for precipitation, separating the precipitation, washing it for the second time, and drying it to prepare lignin.

8. The method according to claim 7, characterized in that The medium for the first wash is an aqueous solution of ethanol; Optionally, the volume ratio of ethanol to water in the ethanol aqueous solution is 19:1-9:1; Optionally, the amount of the ethanol aqueous solution added is 1 to 3 times the volume of the reaction solution.

9. The method according to claim 7, characterized in that: The amount of water added is 10 to 15 times the volume of the concentrate; and / or The static sedimentation time is 12h-24h.

10. The method according to any one of claims 7 to 9, characterized in that: The medium for the second washing is water, and its pH value is 6.8-7.2; Optionally, the number of washes is 2-3 times.

Citation Information

Cited By

  • Lignin extraction-sulfonic acid modification integrated preparation method based on eutecticevaporate solvent coupled microwave, lignin sulfonate and application

    CN120904479A