Novel antibacterial collagen-like hydrogel as well as preparation method and application thereof
By cross-linking recombinant collagen-like protein Scl2 with tea polyphenols and metal ions, a new antibacterial hydrogel is formed, which solves the problems of poor antibacterial effect and insufficient mechanical properties of existing antibacterial hydrogels, and achieves efficient antibacterial performance and Appropriate mechanical properties and industrialization potential.
Patent Information
- Application Number
- CN202310340890.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
Existing antibacterial hydrogels have poor antibacterial effects and insufficient mechanical properties, making it difficult to effectively treat bacterially infected wounds.
Recombinant collagen Scl2 is cross-linked with tea polyphenols and metal ions (Ag+, Zn2+, Cu2+) to form a new antibacterial hydrogel with a stable network structure, improving its mechanical properties and antibacterial properties.
The mechanical properties and antibacterial effect of the hydrogel are significantly improved, becoming a substitute for antibiotics, safe and environmentally friendly, and suitable for industrial production.
Smart Images

Figure CN118725342A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional polymer materials, and specifically relates to a novel antibacterial collagen-like hydrogel and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] In recent years, microbial contamination caused by bacteria has seriously endangered human health and food safety. With the development of society and the advancement of science and technology, antibiotics have come into being. It can effectively kill and inhibit the infection of microorganisms and has played an indispensable role in protecting humans for nearly a century. At the same time, the improper use and abuse of antibiotics have led to the continuous emergence of drug-resistant bacteria. However, the process of developing new antibiotics is very long and the cost is extremely high. Therefore, it is particularly important to develop an antibacterial material that can replace antibiotics, avoid the development of bacterial resistance, and effectively treat bacterial-induced wound infections. In order to meet these requirements, researchers have continuously developed some new antibacterial materials such as peptides, metal nanoparticles, hydrogels, etc. Among these materials, hydrogels have attracted widespread attention due to their unique advantages such as good hydrophilicity, cell compatibility and non-cytotoxicity.
[0004] The inventors have found that bacterial Streptococcus pyogenes Scl2 is a collagen-like protein with a characteristic triple helix similar to animal collagen. Previously, patents CN 114262368 A and CN 115724924A disclosed that recombinant collagen-like proteins purified by nickel column affinity chromatography have the characteristics of self-assembly into hydrogels; patent CN114702692 A disclosed that the stability of collagen-like hydrogels was enhanced by soaking in flavonoids such as tea polyphenols. Next, the inventors aim to enrich the potential application value of recombinant collagen-like protein Scl2, further improve the mechanical properties of hydrogels, and then develop a new antibacterial hydrogel, in order to be able to be used in the treatment of bacterially infected wounds, with a broad-spectrum and efficient antibacterial effect. Summary of the invention
[0005] In order to address the deficiencies of the prior art, the purpose of the present invention is to provide a novel antibacterial collagen-like hydrogel and its preparation method and application, so as to enrich the potential application value of recombinant collagen-like Scl2 and solve the technical problem of poor antibacterial effect of hydrogels in the prior art.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] The first aspect of the present invention provides a method for preparing a novel antibacterial collagen-like hydrogel, wherein tea polyphenols and / or metal ions are cross-linked with the protein-like hydrogel;
[0008] The protein hydrogel is a collagen-like hydrogel;
[0009] The metal ion is Ag + 、Zn 2+ and Cu 2+ One or more of the .
[0010] The second aspect of the present invention provides a novel antibacterial collagen-like hydrogel prepared by the above preparation method.
[0011] The third aspect of the present invention provides the use of the novel antibacterial collagen-like hydrogel in an antibacterial product; wherein the antibacterial product inhibits Escherichia coli and / or Staphylococcus aureus.
[0012] The fourth aspect of the present invention provides the use of tea polyphenols and / or metal ions in improving the mechanical properties and antibacterial properties of hydrogels; wherein the metal ions are Ag + 、Zn 2+ and Cu 2+ One or more of the .
[0013] The beneficial effects of the present invention are:
[0014] The present invention uses recombinant collagen as a raw material, and prepares a novel antibacterial protein hydrogel with a stable network structure by adding or soaking metal ions and / or tea polyphenols. The mechanical strength of the hydrogel can be enhanced by only adding or soaking metal ions and / or tea polyphenols, and the anti-stretching and adhesion properties are high. The preparation method is simple, easy to operate, and has good stability.
[0015] The hydrogel prepared by the present invention does not need to introduce toxic chemical cross-linking agents, and the obtained hydrogel is safer and more environmentally friendly. Compared with the previous recombinant collagen, the mechanical properties of the hydrogel are significantly improved, and the tensile strength, deformation ability and adhesion strength are all improved. Moreover, due to the presence of metal ions and tea polyphenols, the prepared new antibacterial hydrogel is endowed with excellent antibacterial properties, and is expected to become a substitute for antibiotics, enriching the potential application value of recombinant collagen Scl2. In short, the new antibacterial collagen hydrogel prepared by the present invention is simple to prepare, safe and environmentally friendly, has appropriate mechanical properties and excellent antibacterial properties, and is expected to achieve industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0017] Figure 1 This is a picture of the novel antibacterial hydrogel prepared in Example 5 of the present invention;
[0018] Figure 2 This is a scanning electron micrograph of the novel antibacterial hydrogel prepared in Example 5 of the present invention;
[0019] Figure 3 This is a stress-strain curve of the recombinant collagen hydrogel prepared in Comparative Example 1;
[0020] Figure 4 This is a stress-strain curve diagram of the novel antibacterial hydrogel prepared in Example 5;
[0021] Figure 5 This is a comparison chart of the tensile properties of the novel antibacterial hydrogel prepared in Example 5 and the recombinant collagen hydrogel prepared in Comparative Example 1 against gelatin;
[0022] Figure 6 This is a graph showing the inhibition of the growth of Escherichia coli and Staphylococcus aureus by the new antibacterial hydrogel prepared in Example 5. DETAILED DESCRIPTION
[0023] In view of the problems of poor antibacterial effect and insufficient mechanical properties of existing hydrogels, the present invention proposes a method for preparing a novel antibacterial collagen-like hydrogel, wherein tea polyphenols and / or metal ions are cross-linked with protein hydrogels; the protein hydrogel is a collagen-like hydrogel; the metal ions are Ag + 、Zn 2+ and Cu 2+ One or more of the .
[0024] The present invention uses recombinant collagen as a raw material, and prepares a novel antibacterial protein hydrogel with a stable network structure by adding or soaking metal ions and tea polyphenols. Without introducing toxic chemical cross-linking agents, the mechanical properties of the hydrogel are significantly improved, and the obtained hydrogel is more environmentally friendly and safe. In addition, due to the presence of metal ions and tea polyphenols, the hydrogel is endowed with excellent antibacterial properties, enriching the potential application value of the hydrogel.
[0025] In one embodiment of the present invention, collagen-like protein is mixed with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, and then tea polyphenols are added. The pH is then adjusted to 6-8 with 0.05-2M NaOH solution and allowed to stand at room temperature.
[0026] The final concentration of tea polyphenols accounts for 0.1% to 1% of the volume of the entire hydrogel.
[0027] In one embodiment of the present invention, collagen-like protein is mixed with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, and then metal ions are added. The pH is then adjusted to 6-8 with 0.05-2M NaOH solution and allowed to stand at room temperature.
[0028] The final concentration of the metal ions is 0.01 mM to 0.1 mM.
[0029] In one embodiment of the present invention, collagen-like protein is mixed with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, and then metal ions are added. The pH is then adjusted to 6-8 with a 0.05-2M NaOH solution, and the solution is allowed to stand at room temperature to obtain a hydrogel. The hydrogel is then immersed in a 0.01%-1% tea polyphenol aqueous solution for 12h-24h.
[0030] The final concentration of the metal ions is 0.01 mM to 0.1 mM.
[0031] In one embodiment of the present invention, collagen-like protein is mixed with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, and then tea polyphenols are added. The pH is then adjusted to 6-8 with 0.05-2M NaOH solution, and the solution is allowed to stand at room temperature to obtain a hydrogel. The hydrogel is then immersed in a metal ion aqueous solution with a concentration of 0.01mM-0.1mM for 12h-24h.
[0032] The final concentration of tea polyphenols accounts for 0.1% to 1% of the volume of the entire hydrogel.
[0033] In one embodiment of the present invention, collagen-like protein is added with water to prepare a solution with a concentration of 25-50 mg / mL; the solution is heated at 50°C-70°C until completely dissolved, and then tea polyphenols are immediately added and allowed to stand at room temperature.
[0034] The final concentration of tea polyphenols accounts for 0.1% to 1% of the volume of the entire hydrogel.
[0035] In one embodiment of the present invention, collagen-like protein is added with water to prepare a solution with a concentration of 25-50 mg / mL; the solution is heated at 50° C.-70° C. until completely dissolved, and then metal ions are immediately added and allowed to stand at room temperature.
[0036] The final concentration of the metal ions is 0.01 mM to 0.1 mM.
[0037] In one embodiment of the present invention, collagen-like protein is added with water to prepare a solution with a concentration of 25 to 50 mg / mL; the solution is heated at 50°C to 70°C until completely dissolved, and then metal ions are immediately added, and the solution is allowed to stand at room temperature to obtain a hydrogel, and the hydrogel is immersed in a 0.01% to 1% tea polyphenol / electro-oxidized tea polyphenol aqueous solution for 12h to 24h.
[0038] The final concentration of the metal ions is 0.01 mM to 0.1 mM.
[0039] In one embodiment of the present invention, collagen-like protein is added with water to prepare a solution with a concentration of 25 to 50 mg / mL; the solution is heated at 50°C to 70°C until completely dissolved, and tea polyphenols are immediately added, and the solution is allowed to stand at room temperature to obtain a hydrogel, and the hydrogel is immersed in a metal ion aqueous solution with a concentration of 0.01mM to 0.1mM for 12h to 24h.
[0040] The final concentration of tea polyphenols accounts for 0.1% to 1% of the volume of the entire hydrogel.
[0041] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0042] The amino acid sequences and expressions of the collagen-like proteins used in the following examples and comparative examples refer to patent CN114262368 A or patent CN115724924 A.
[0043] Specifically, the purification and extraction method of collagen-like protein consists of the following steps:
[0044] 1) Transform the recombinant collagen-like protein expression vector into the Escherichia coli BL21 (DE3) strain and spread it on a solid LB medium plate containing kanamycin;
[0045] 2) picking a single clone from the plate obtained in step 1), transferring it to a test tube containing culture medium pre-added with kanamycin, and culturing it at 37°C with shaking overnight;
[0046] 3) Transfer the bacterial solution from step 3) to LB medium pre-added with kanamycin, and culture at 37°C with shaking until OD 600 Reach 0.4~0.6;
[0047] 4) Add IPTG to the bacterial solution in step 3) and culture at 37°C for 5h-6h;
[0048] 5) collecting the bacterial solution obtained in step 4) by centrifugation / filtration, removing the supernatant and collecting the bacterial precipitate;
[0049] 6) Add protein extract and lysozyme to the bacterial precipitate in step 5) and let stand on ice for 1 hour.
[0050] 7) The protein solution obtained in step 6) is ultrasonically disrupted, and the supernatant is collected by centrifugation / filtration.
[0051] 8) Add the crude protein solution from step 7) into a gravity column loaded with nickel.
[0052] 9) When there is no residual crude protein solution on the nickel column in step 8), add Buffer A (50 mM Tris, 250 mM NaCl, 30 mM imidazole) to wash the impurities.
[0053] 10) Add Buffer B (50 mM Tris, 250 mM NaCl, 400 mM imidazole) to the nickel column in step 9) to elute the target protein.
[0054] 11) Add Ag with a final concentration of 0 mM to 0.1 mM to the protein eluate in step 10). + / Zn 2+ / Cu 2+ , and stirred at 4°C overnight.
[0055] 12) The target protein to which the metal ions were added in step 11) was directly dialyzed with distilled water, and the dialysis time was 6 hours each time, for a total of 2 times.
[0056] 13) The dialyzed solution in step 12) is freeze-dried to obtain the recombinant collagen-like protein.
[0057] Example 1
[0058] A method for preparing a novel antibacterial collagen-like hydrogel comprises the following steps:
[0059] The collagen-like protein is mixed with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, and then tea polyphenols are added. The pH is then adjusted to 6-8 with 0.05-2M NaOH solution, and the hydrogel can be generated by standing at room temperature.
[0060] The final concentration of tea polyphenols is 0.1% to 1% of the volume of the entire hydrogel.
[0061] The obtained hydrogel has good stability and can inhibit Escherichia coli and Staphylococcus aureus.
[0062] Example 2
[0063] A method for preparing a novel antibacterial collagen-like hydrogel comprises the following steps:
[0064] Mix collagen with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, and then add metal ions Ag. + / Zn 2+ / Cu 2+ The pH is then adjusted to 6-8 with 0.05-2 M NaOH solution and allowed to stand at room temperature to generate a hydrogel.
[0065] The final concentration of metal ions is 0.01 mM to 0.1 mM.
[0066] The obtained hydrogel has good stability and can inhibit Escherichia coli and Staphylococcus aureus.
[0067] Example 3
[0068] A method for preparing a novel antibacterial collagen-like hydrogel comprises the following steps:
[0069] Mix collagen with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, and then add metal ions Ag. + / Zn 2+ / Cu 2+ Then, the pH is adjusted to 6-8 with 0.05-2M NaOH solution, and the hydrogel is formed by standing at room temperature. Finally, the hydrogel is immersed in a 0.01%-1% tea polyphenol / electro-oxidized tea polyphenol aqueous solution for 12h-24h.
[0070] The final concentration of metal ions is 0.01 mM to 0.1 mM.
[0071] The obtained hydrogel has good stability and can inhibit Escherichia coli and Staphylococcus aureus.
[0072] Example 4
[0073] A method for preparing a novel antibacterial collagen-like hydrogel comprises the following steps:
[0074] The collagen-like protein was mixed with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, and then tea polyphenols / electro-oxidized tea polyphenols were added. Then, the pH was adjusted to 6-8 with 0.05-2M NaOH solution and the hydrogel was formed by standing at room temperature. Finally, the hydrogel was immersed in a metal ion Ag solution with a concentration of 0.01mM-0.1mM. + / Zn 2+ / Cu 2+ 12h~24h in aqueous solution.
[0075] The final concentration of tea polyphenols / electro-oxidized tea polyphenols accounts for 0.1% to 1% of the volume of the entire hydrogel.
[0076] The obtained hydrogel has good stability and can inhibit Escherichia coli and Staphylococcus aureus.
[0077] Example 5
[0078] A method for preparing a novel antibacterial collagen-like hydrogel comprises the following steps:
[0079] Add water to collagen-like protein to prepare a solution with a concentration of 25-50 mg / mL; heat at 50°C-70°C until completely dissolved, then immediately add tea polyphenols and let stand at room temperature to generate a hydrogel.
[0080] The final concentration of tea polyphenols is 0.1% to 1% of the volume of the entire hydrogel.
[0081] The obtained hydrogel has good stability and can inhibit Escherichia coli and Staphylococcus aureus.
[0082] The pictures of the new antibacterial hydrogel are as follows: Figure 1 As shown, the new antibacterial hydrogel is soft and can maintain a certain shape. Figure 2 This is a scanning electron microscope image of the new antibacterial hydrogel. The new antibacterial hydrogel has a large number of pore structures and can absorb a large amount of water.
[0083] Example 6
[0084] A method for preparing a novel antibacterial collagen-like hydrogel comprises the following steps:
[0085] Add water to the collagen-like protein to prepare a solution with a concentration of 25-50 mg / mL; heat at 50-70°C until completely dissolved, and then immediately add the metal ion Ag. + / Zn 2+ / Cu 2+ The hydrogel can be formed by standing at room temperature.
[0086] The final concentration of metal ions is 0.01 mM to 0.1 mM.
[0087] The obtained hydrogel has good stability and can inhibit Escherichia coli and Staphylococcus aureus.
[0088] Example 7
[0089] A method for preparing a novel antibacterial collagen-like hydrogel comprises the following steps:
[0090] Add water to the collagen-like protein to prepare a solution with a concentration of 25-50 mg / mL; heat at 50-70°C until completely dissolved, and then immediately add the metal ion Ag. + / Zn 2+ / Cu2+ The hydrogel is formed by standing at room temperature. Finally, the hydrogel is immersed in a 0.01% to 1% tea polyphenol / electro-oxidized tea polyphenol aqueous solution for 12h to 24h.
[0091] The final concentration of metal ions is 0.01 mM to 0.1 mM.
[0092] The obtained hydrogel has good stability and can inhibit Escherichia coli and Staphylococcus aureus.
[0093] Example 8
[0094] A method for preparing a novel antibacterial collagen-like hydrogel comprises the following steps:
[0095] Add water to the collagen-like protein to prepare a solution with a concentration of 25-50 mg / mL; heat at 50°C-70°C until completely dissolved, then immediately add tea polyphenols and let stand at room temperature to form a hydrogel. Finally, soak the hydrogel in a metal ion Ag solution with a concentration of 0.01mM-0.1mM. + / Zn 2+ / Cu 2+ 12h~24h in aqueous solution.
[0096] The final concentration of tea polyphenols is 0.1% to 1% of the volume of the entire hydrogel.
[0097] The obtained hydrogel has good stability and can inhibit Escherichia coli and Staphylococcus aureus.
[0098] Comparative Example 1
[0099] A method for preparing a recombinant collagen hydrogel, which differs from Example 5 in that tea polyphenols are not added.
[0100] Performance Testing
[0101] 1. Stability test
[0102] In order to detect the stability of the new antibacterial hydrogel prepared in Example 5 and the recombinant collagen hydrogel prepared in Comparative Example 1, the mechanical properties of the hydrogel were tested. Specifically, the mechanical properties of the hydrogel were measured by a 500N microcomputer-controlled electronic universal testing machine. The compression test was carried out on a cylindrical hydrogel at a speed of 10mm / min, with a maximum strain of 90%. Adhesion strength determination: measured using a 500N microcomputer-controlled electronic universal testing machine; two glass slides (75mm×25mm) were used for each sample; gelatin solution was applied to the top of the glass slide (25mm×20mm), and after drying at room temperature, the hydrogel sample to be tested was added; the hydrogel was added to one of the gelatin coating areas, and then another glass slide was carefully placed on the hydrogel area; the two glass slides were placed in the universal testing machine for measurement, and a shear test was performed at a tensile loading rate of 10mm / min.
[0103] Test results such as Figure 3 , 4 , 5. Comparison Figure 3 , Figure 4 , Figure 5 It can be seen that after adding tea polyphenols, the mechanical properties of the novel antibacterial hydrogel prepared in Example 5 of the present invention are significantly improved, the deformation capacity is improved, and the tensile strength is also improved.
[0104] It can be seen that the novel antibacterial hydrogel prepared by the present invention has higher mechanical properties than the recombinant collagen hydrogel prepared in Comparative Example 1, and both tensile strength and deformation capacity are improved.
[0105] (2) Antibacterial testing
[0106] In order to detect the antibacterial property of the novel antibacterial hydrogel prepared in Example 5, the novel antibacterial hydrogel prepared in Example 5 was co-cultured with Escherichia coli and Staphylococcus aureus, respectively, and after 1 day, it was observed whether an inhibition zone appeared near the hydrogel in the culture medium.
[0107] Test results such as Figure 6 As shown, the culture medium containing the novel antibacterial hydrogel prepared in Example 5 produced obvious inhibition zones for Escherichia coli and Staphylococcus aureus, and no colonies were formed in the inhibition zones; while the Escherichia coli and Staphylococcus aureus in the control group grew normally and were not affected, indicating that the hydrogel prepared in the present invention has excellent antibacterial effect.
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a novel antibacterial collagen-like hydrogel. It is characterized in that Cross-linking tea polyphenols and / or metal ions with protein hydrogels; The protein hydrogel is a collagen-like hydrogel; The metal ion is Ag + 、Zn 2+ and Cu 2+ One or more of the .
2. The preparation method according to claim 1, It is characterized in that The preparation method comprises: mixing collagen-like protein with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, adding tea polyphenols, and then adjusting the pH to 6-8 with 0.05-2M NaOH solution, and standing at room temperature to obtain the product; Preferably, the final concentration of tea polyphenols is 0.1% to 1% of the volume of the entire hydrogel.
3. The preparation method according to claim 1, It is characterized in that The preparation method comprises: mixing collagen-like protein with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, adding metal ions, and then adjusting the pH to 6-8 with 0.05-2M NaOH solution, and standing at room temperature to obtain the product; The final concentration of metal ions is 0.01 mM to 0.1 mM.
4. The preparation method according to claim 1, It is characterized in that The preparation method comprises: mixing collagen-like protein with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, adding metal ions, and then adjusting the pH to 6-8 with a 0.05-2M NaOH solution, standing at room temperature to obtain a hydrogel, and soaking the hydrogel in a 0.01%-1% tea polyphenol aqueous solution for 12h-24h to obtain the hydrogel; The final concentration of metal ions is 0.01 mM to 0.1 mM.
5. The preparation method according to claim 1, It is characterized in that The preparation method comprises: mixing collagen-like protein with 0.05-0.2M hydrochloric acid to prepare an acid solution with a concentration of 25-50mg / mL, adding tea polyphenols, and then adjusting the pH to 6-8 with a 0.05-2M NaOH solution, standing at room temperature to obtain a hydrogel, and soaking the hydrogel in a metal ion aqueous solution with a concentration of 0.01mM-0.1mM for 12h-24h to obtain the hydrogel; The final concentration of tea polyphenols is 0.1% to 1% of the volume of the entire hydrogel.
6. The preparation method according to claim 1, It is characterized in that The preparation method comprises: adding water to collagen-like protein to prepare a solution with a concentration of 25 to 50 mg / mL; heating at 50°C to 70°C until completely dissolved, and then immediately adding tea polyphenols, and standing at room temperature to obtain the solution; The final concentration of tea polyphenols was 0.1% to 1% of the volume of the entire hydrogel; Alternatively, the preparation method is: adding water to the collagen-like protein to prepare a solution with a concentration of 25 to 50 mg / mL; heating at 50° C. to 70° C. until completely dissolved, then immediately adding metal ions, and standing at room temperature to obtain the solution; The final concentration of metal ions is 0.01 mM to 0.1 mM.
7. The preparation method according to claim 1, It is characterized in that The preparation method comprises: adding water to collagen-like protein to prepare a solution with a concentration of 25 to 50 mg / mL; heating at 50°C to 70°C until completely dissolved, immediately adding metal ions, and standing at room temperature to obtain a hydrogel, and soaking the hydrogel in a 0.01% to 1% tea polyphenol / electro-oxidized tea polyphenol aqueous solution for 12 hours to 24 hours to obtain the hydrogel; The final concentration of metal ions is 0.01mM to 0.1mM; Alternatively, the preparation method is as follows: adding water to collagen-like protein to prepare a solution with a concentration of 25 to 50 mg / mL; heating at 50°C to 70°C until completely dissolved, then immediately adding tea polyphenols, and standing at room temperature to obtain a hydrogel, and then soaking the hydrogel in a metal ion aqueous solution with a concentration of 0.01 mM to 0.1 mM for 12 h to 24 h to obtain the hydrogel; The final concentration of tea polyphenols is 0.1% to 1% of the volume of the entire hydrogel.
8. A novel antibacterial collagen-like hydrogel prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the novel antibacterial collagen-like hydrogel according to claim 8 in antibacterial products; The antimicrobial product inhibits Escherichia coli and / or Staphylococcus aureus.
10. Application of tea polyphenols and / or metal ions in improving the mechanical properties and antibacterial properties of hydrogels; The metal ion is Ag + 、Zn 2+ and Cu 2+ One or more of the .
Citation Information
Patent Citations
Method for improving stability of protein hydrogel
CN114702692A
Antibacterial egg white water gel as well as preparation method and application thereof
CN114870068A
Preparation method and application of supramolecule-macromolecule composite hydrogel material
CN115678047A
Antibacterial polymer raw material and its production
JP2000204182A