Hydrogen-sensitive color-changing film based on nano material and preparation method of hydrogen-sensitive color-changing film

By using sodium tungstate, sodium metavanadate and carbon nanotubes in a hydrogen-sensitive color-changing film for hydrothermal reaction, a V-doped WO3-carbon nanotube composite is formed, and combined with vinyl silicone rubber and silane coupling agent, It solves the problems of long response time and poor mechanical properties of hydrogen-sensitive color-changing films, and achieves high-sensitivity and fast-response hydrogen detection effects.

CN118725375AActive Publication Date: 2024-10-01SUZHOU PAN HYDROGEN NEW MATERIAL TECH CO LTD +1

Patent Information

Application Number
CN202411207434.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-10-01
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Existing hydrogen-sensitive color-changing films have long response times to hydrogen and have average mechanical properties, which cannot meet the needs of high sensitivity and fast response.

Method used

Sodium tungstate, sodium metavanadate and carbon nanotubes are used for hydrothermal reaction in an acidic environment to form V-doped WO3-carbon nanotube composite materials, combined with vinyl silicone rubber and silane coupling agent, through calcination and molding processes Hydrogen-sensitive color-changing films with high specific surface area and excellent dispersion were prepared.

Benefits of technology

The sensitivity and response speed of the hydrogen-sensitive color-changing film are significantly improved, the adsorption capacity and selectivity for hydrogen are enhanced, and the mechanical properties and stability of the film are improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of hydrogen-sensitive materials, and discloses a hydrogen-sensitive color-changing film based on a nano material and a preparation method of the hydrogen-sensitive color-changing film. The preparation method comprises the following steps: by taking sodium tungstate as a tungsten source and sodium metavanadate as a vanadium source, under the combined action of n-propyl alcohol as an organic inducer and carbon nanotubes in an acidic environment, carrying out hydrothermal reaction to obtain a precursor; calcining the precursor in an argon atmosphere to obtain the V-doped WO3-carbon nanotube composite material with a unique nano structure and a higher specific surface area; the V-doped WO3-carbon nanotube composite material is used as a hydrogen sensitive material, the V-doped WO3-carbon nanotube composite material, vinyl silicone rubber and a dispersing agent are stirred and mixed, and the hydrogen-sensitive color-changing film based on the nano material is obtained through open milling and forming. The V-doped WO3 has a high specific surface area and rich reaction sites, the hydrogen adsorption capacity can be improved, the hydrogen selectivity is improved, the carbon nanotubes have excellent mechanical properties, the mechanical properties of the film are effectively improved, and the prepared hydrogen-sensitive color-changing film has the characteristics of high sensitivity, short response time and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogen-sensitive materials, and in particular to a hydrogen-sensitive color-changing film based on nanomaterials and a preparation method thereof. Background Art

[0002] Energy and environmental issues, as the two major themes of the development of the world today, have received more and more attention. With the over-exploitation of fossil energy, more and more problems are faced. The depletion of secondary energy and the pollution caused by the use of secondary energy have become difficult problems that need to be solved. Hydrogen energy has the advantages of high efficiency, cleanliness, environmental protection, and renewability. It has great practical value. The development and use of hydrogen energy is of great significance to cope with the energy crisis and the pollution problems caused by the use of secondary energy, and has received widespread attention. However, hydrogen is also flammable and explosive, and there are certain safety hazards in the preparation, storage, transportation and use. Since hydrogen is colorless, odorless and has strong permeability, in order to safely use hydrogen energy, it is necessary to develop and use hydrogen-sensitive materials with high sensitivity and stable working performance to detect hydrogen leaks.

[0003] Chinese patent CN114180850A provides a vanadium-doped crystalline tungsten trioxide electrochromic film and a preparation method thereof. The molar ratio of vanadium atoms to tungsten atoms in the vanadium-doped crystalline tungsten trioxide electrochromic film is (0.01-0.1). The preparation process is as follows: 1cm×4cm ITO glass is ultrasonically cleaned by acetone, ethanol, and deionized water, respectively, and placed in an oven for drying; sodium metavanadate and sodium tungstate are weighed, dissolved in deionized water, 30% hydrogen peroxide solution is added, and an appropriate amount of sulfuric acid solution is added to adjust the pH; a three-electrode system is used for deposition to obtain a tungsten oxide film; and the film is calcined in a muffle furnace to obtain a crystalline tungsten oxide film. The preparation method is simple to operate, low in cost, and does not require the addition of a template agent. The prepared film has uniform pore structure, excellent electrochromic performance, and good cycle stability. However, the film has a long response time and average sensitivity. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a hydrogen-sensitive color-changing film based on nanomaterials and a preparation method thereof, which solves the problem that the hydrogen-sensitive color-changing film has a long response time to hydrogen and general mechanics.

[0005] In order to achieve the above object, the present invention discloses a method for preparing a hydrogen-sensitive color-changing film based on nanomaterials, comprising the following steps: Step 1: dissolve sodium tungstate in deionized water, mix well, add sodium metavanadate, adjust the pH to 1.6-2.4 with aqueous hydrochloric acid solution, add n-propanol, stir and mix, add carbon nanotube dispersion to obtain a mixed solution, transfer the mixed solution to a reactor, and cause a hydrothermal reaction. After the reaction is completed, cool and centrifuge at a rate of 6000 r / min for 6 minutes. The solid product obtained by centrifugation is washed with deionized water and anhydrous ethanol until neutral, and then vacuum dried in a vacuum drying oven at 60°C for 12 hours to obtain a V-doped WO3-carbon nanotube composite material precursor; Step 2: placing the V-doped WO3-carbon nanotube composite material precursor in a muffle furnace, and calcining it in an inert gas atmosphere. After the calcination, cooling it to room temperature in an inert gas atmosphere, grinding and sieving it, to obtain a V-doped WO3-carbon nanotube composite material; Step 3: Put the V-doped WO3-carbon nanotube composite material, vinyl silicone rubber and dispersant into a mixer and stir and mix them evenly, then refine them in an open mill, and then mold them in a molding machine to obtain a hydrogen-sensitive color-changing film based on nanomaterials.

[0006] Preferably, in step 1, the mass ratio of sodium tungstate, deionized water, sodium metavanadate, n-propanol and carbon nanotube dispersion is 100:130-150:0.2-0.7:1-3:18-30.

[0007] Preferably, in step 1, the temperature of the hydrothermal reaction is 150-180° C., and the time of the hydrothermal reaction is 8-12 h.

[0008] Preferably, in step 1, the aqueous hydrochloric acid solution is an aqueous hydrochloric acid solution with a concentration of 0.3 mol / L.

[0009] Preferably, in the step 1, the concentration of the carbon nanotube dispersion is 50 g / L, and the carbon nanotube dispersion is an aqueous solution of carbon nanotubes after acidification; The steps for preparing the acid-treated carbon nanotubes are as follows: The multi-walled carbon nanotubes were added into a 37wt% hydrochloric acid solution in a mass ratio of 1:5. The mixture was stirred for 1 hour and then ultrasonically dispersed at a temperature of 70-80°C for 3-4 hours. The mixture was filtered and washed with deionizer until neutral. The mixture was vacuum dried at 60°C for 6 hours to obtain the acidified carbon nanotubes.

[0010] Preferably, in the step 2, the calcination temperature is 450-520° C., and the calcination time is 2-3 hours.

[0011] Preferably, in step 2, the inert gas includes argon.

[0012] Preferably, in the step 2, the average particle size of the V-doped WO3-carbon nanotube composite material is less than 0.1 μm.

[0013] Preferably, in step three, the mass ratio of the V-doped WO3-carbon nanotube composite material, the vinyl silicone rubber and the dispersant is 18-25:100:1-3.

[0014] Preferably, in step three, the dispersant includes a silane coupling agent.

[0015] Preferably, in step three, the silane coupling agent includes a vinyl silane coupling agent.

[0016] Furthermore, the vinyl silane coupling agent is γ-(methacryloyloxy)propyltrimethoxysilane.

[0017] Preferably, in step 3, the stirring and mixing speed is 240-300 r / min; the refining temperature is 160-200° C., and the refining time is 12-15 min.

[0018] Preferably, the hydrogen-sensitive color-changing film based on nanomaterials is prepared by the method for preparing the hydrogen-sensitive color-changing film based on nanomaterials.

[0019] Compared with the prior art, the present invention has the following beneficial effects: In the present invention, sodium tungstate is used as a tungsten source and sodium metavanadate is used as a vanadium source. In an acidic environment, n-propanol is used as an organic inducing agent. Under hydrothermal conditions, the inducing agent and carbon nanotubes react to obtain a V-doped WO3-carbon nanotube composite material precursor. The V-doped WO3-carbon nanotube composite material precursor is calcined in an inert gas atmosphere to obtain a V-doped WO3-carbon nanotube composite material with a unique nanostructure and a higher specific surface area. The V-doped WO3-carbon nanotube composite material is used as a hydrogen-sensitive material, and is stirred and mixed with vinyl silicone rubber and a dispersant vinyl silane coupling agent. After refining and molding, a hydrogen-sensitive color-changing film based on nanomaterials is obtained. The dispersant vinyl silane coupling agent can effectively improve the dispersibility of the V-doped WO3-carbon nanotube composite material, react with the vinyl silicone rubber, and the prepared film has excellent dispersibility and compatibility, and uniform performance.

[0020] The carbon nanotubes in the present invention have a high specific surface area and abundant reaction sites, which can effectively improve the sensitivity and response speed of the composite material, and also have the characteristics of high conductivity and chemical stability. WO3 has a high electron density and oxygen mobility, which can effectively improve the conductivity and hydrogen sensitivity of the composite material. In V-doped WO3, V exists in a +5 valence state, which can replace the tungsten atoms in WO3, generate holes, and enhance the hydrogen sensitivity of WO3. At the same time, since the radius of vanadium is similar to that of tungsten, the crystal structure of WO3 will not be destroyed. V-doped WO3 has a high specific surface area and abundant reaction sites. In addition, V-doped WO3 can also increase the adsorption capacity of hydrogen, improve the selectivity of hydrogen, and has good selectivity. The prepared hydrogen-sensitive color-changing film has the characteristics of high sensitivity and short response time.

[0021] In the present invention, after WO3 reacts with hydrogen, the hydrogen molecules adsorbed on the surface of the hydrogen-sensitive color-changing film are decomposed into hydrogen atoms under the action of the catalytic layer. The hydrogen atoms diffuse into the film along the surface of the film holes. During the diffusion process, two hydrogen atoms combine with one oxygen atom at the boundary of the WO3 grain to form water, thereby forming oxygen vacancies in the WO3 grain body. The oxygen vacancies diffuse into the grain body to form color centers, resulting in the color change of the film and generating a blue bronze structure: 0.5xH2+WO3→HxWO4, the electrons in W 6+ With W 5+ Due to the transition between the two, the color of the hydrogen-sensitive color-changing film will change from transparent to blue after the reaction.

[0022] The carbon nanotubes in the present invention have the advantages of small size, large specific surface area, strong adsorption capacity, high conductivity and low operating temperature. Since the high surface area carbon nanotubes can adsorb a large amount of gas, the sensitivity and response time to hydrogen are effectively improved. V-doped WO3 grows on the carbon nanotubes, the growth density is large, the specific surface area of ​​the material is improved, and it has good hydrogen response ability and fast color change time. At the same time, the carbon nanotubes have excellent mechanical properties, and the vinyl silicone rubber has excellent elasticity and mechanical properties, which effectively improves the mechanical properties of the film. At the same time, the vinyl silicone rubber also protects the hydrogen-sensitive material and improves the stability, safety and service life of the film. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A method for preparing a hydrogen-sensitive color-changing film based on nanomaterials comprises the following steps: Step 1: dissolve sodium tungstate in deionized water, mix well, add sodium metavanadate, adjust the pH to 1.6 with 0.3 mol / L hydrochloric acid aqueous solution, add n-propanol, stir and mix, and add a carbon nanotube dispersion with a concentration of 50 g / L to obtain a mixed solution, wherein the mixed solution is obtained by mixing sodium tungstate, deionized water, sodium metavanadate, n-propanol and carbon nanotube dispersion in a mass ratio of 100:130:0.2:1:18, transfer the mixed solution to a reactor, and perform a hydrothermal reaction at a temperature of 150°C for 12 hours. After the reaction is completed, cool and centrifuge at a rate of 6000 r / min for 6 minutes. The solid product obtained by centrifugation is washed with deionized water and anhydrous ethanol until neutral, and then vacuum dried in a vacuum drying oven at 60°C for 12 hours to obtain a V-doped WO3-carbon nanotube composite material precursor; The carbon nanotube dispersion is an aqueous solution of carbon nanotubes after acidification, and the preparation steps of the carbon nanotubes after acidification are as follows: adding multi-walled carbon nanotubes to a 37wt% hydrochloric acid solution, the mass ratio of the multi-walled carbon nanotubes to the 37wt% hydrochloric acid solution is 1:5, stirring for 1h, and then ultrasonically dispersing, the ultrasonic dispersion temperature is 70°C, the ultrasonic dispersion time is 4h, suction filtering, washing with deionized water to neutrality, and vacuum drying at 60°C for 6h to obtain the carbon nanotubes after acidification; Step 2: placing the V-doped WO3-carbon nanotube composite material precursor in a muffle furnace, and calcining it in an argon atmosphere at a temperature of 450° C. for 3 hours. After the calcination, cooling it to room temperature in an argon atmosphere, grinding and sieving, to obtain a V-doped WO3-carbon nanotube composite material with an average particle size of less than 0.1 μm; Step 3: Place the V-doped WO3-carbon nanotube composite material, vinyl silicone rubber and dispersant γ-(methacryloyloxy)propyltrimethoxysilane in a mass ratio of 18:100:1 into a mixer and stir and mix them evenly at a speed of 240 r / min. Then, refine them in an open mill at a temperature of 160°C and a time of 15 min. Then, mold them in a molding machine to obtain a hydrogen-sensitive color-changing film based on nanomaterials.

[0026] Example 2

[0027] A method for preparing a hydrogen-sensitive color-changing film based on nanomaterials comprises the following steps: Step 1: dissolve sodium tungstate in deionized water, mix well, add sodium metavanadate, adjust the pH to 2 with 0.3 mol / L hydrochloric acid aqueous solution, add n-propanol, stir and mix, and add a carbon nanotube dispersion with a concentration of 50 g / L to obtain a mixed solution, wherein the mixed solution is obtained by mixing sodium tungstate, deionized water, sodium metavanadate, n-propanol and carbon nanotube dispersion in a mass ratio of 100:138:0.4:1.8:22, transfer the mixed solution to a reactor, and perform a hydrothermal reaction at a temperature of 160°C for 9 hours. After the reaction is completed, cool and centrifuge at a rate of 6000 r / min for 6 minutes. The solid product obtained by centrifugation is washed with deionized water and anhydrous ethanol until neutral, and then vacuum dried in a vacuum drying oven at 60°C for 12 hours to obtain a V-doped WO3-carbon nanotube composite material precursor; The carbon nanotube dispersion is an aqueous solution of carbon nanotubes after acidification, and the preparation steps of the carbon nanotubes after acidification are as follows: adding multi-walled carbon nanotubes to a 37wt% hydrochloric acid solution, the mass ratio of the multi-walled carbon nanotubes to the 37wt% hydrochloric acid solution is 1:5, stirring for 1h, and then ultrasonically dispersing, the ultrasonic dispersion temperature is 75°C, the ultrasonic dispersion time is 3.5h, filtering, washing with deionized water to neutrality, and vacuum drying at 60°C for 6h to obtain the carbon nanotubes after acidification; Step 2: placing the V-doped WO3-carbon nanotube composite material precursor in a muffle furnace, and calcining it in an argon atmosphere at a temperature of 480° C. for 2.5 hours. After the calcination, cooling it to room temperature in an argon atmosphere, grinding and sieving, to obtain a V-doped WO3-carbon nanotube composite material with an average particle size of less than 0.1 μm; Step 3: Place the V-doped WO3-carbon nanotube composite material, vinyl silicone rubber and dispersant γ-(methacryloyloxy)propyltrimethoxysilane in a mass ratio of 21:100:2 into a mixer and stir at a speed of 260 r / min to mix evenly, and then refine in an open mill at a refining temperature of 175°C for 13 min. Then, mold in a molding machine to obtain a hydrogen-sensitive color-changing film based on nanomaterials.

[0028] Example 3

[0029] A method for preparing a hydrogen-sensitive color-changing film based on nanomaterials comprises the following steps: Step 1: dissolve sodium tungstate in deionized water, mix well, add sodium metavanadate, adjust the pH to 2 with 0.3 mol / L hydrochloric acid aqueous solution, add n-propanol, stir and mix, and add 50 g / L carbon nanotube dispersion to obtain a mixed solution, wherein the mixed solution is obtained by mixing sodium tungstate, deionized water, sodium metavanadate, n-propanol and carbon nanotube dispersion in a mass ratio of 100:145:0.6:2.5:26, transfer the mixed solution to a reactor, and perform a hydrothermal reaction at a temperature of 170°C for 10 hours. After the reaction is completed, cool and centrifuge at a rate of 6000 r / min for 6 minutes. The solid product obtained by centrifugation is washed with deionized water and anhydrous ethanol until neutral, and then vacuum dried in a vacuum drying oven at 60°C for 12 hours to obtain a V-doped WO3-carbon nanotube composite material precursor; The carbon nanotube dispersion is an aqueous solution of carbon nanotubes after acidification, and the preparation steps of the carbon nanotubes after acidification are as follows: adding multi-walled carbon nanotubes to a 37wt% hydrochloric acid solution, the mass ratio of the multi-walled carbon nanotubes to the 37wt% hydrochloric acid solution is 1:5, stirring for 1h, and then ultrasonically dispersing, the ultrasonic dispersion temperature is 75°C, the ultrasonic dispersion time is 3.5h, filtering, washing with deionized water to neutrality, and vacuum drying at 60°C for 6h to obtain the carbon nanotubes after acidification; Step 2: placing the V-doped WO3-carbon nanotube composite material precursor in a muffle furnace, and calcining it in an argon atmosphere at a temperature of 500° C. for 2.5 hours. After the calcination, cooling it to room temperature in an argon atmosphere, grinding and sieving, to obtain a V-doped WO3-carbon nanotube composite material with an average particle size of less than 0.1 μm; Step 3: Place the V-doped WO3-carbon nanotube composite material, vinyl silicone rubber and dispersant γ-(methacryloyloxy)propyltrimethoxysilane in a mass ratio of 24:100:2.5 into a mixer and stir and mix them evenly at a speed of 280 r / min. Then, refine them in an open mill at a temperature of 185°C and a time of 14 min. Then, mold them in a molding machine to obtain a hydrogen-sensitive color-changing film based on nanomaterials.

[0030] Example 4

[0031] A method for preparing a hydrogen-sensitive color-changing film based on nanomaterials comprises the following steps: Step 1: dissolve sodium tungstate in deionized water, mix well, add sodium metavanadate, adjust the pH to 2.4 with 0.3 mol / L hydrochloric acid aqueous solution, add n-propanol, stir and mix, and add a carbon nanotube dispersion with a concentration of 50 g / L to obtain a mixed solution, wherein the mixed solution is obtained by mixing sodium tungstate, deionized water, sodium metavanadate, n-propanol and carbon nanotube dispersion in a mass ratio of 100:150:0.7:3:30, transfer the mixed solution to a reactor, and perform a hydrothermal reaction at a temperature of 180°C for 8 hours. After the reaction is completed, cool and centrifuge at a rate of 6000 r / min for 6 minutes. The solid product obtained by centrifugation is washed with deionized water and anhydrous ethanol until neutral, and then vacuum dried in a vacuum drying oven at 60°C for 12 hours to obtain a V-doped WO3-carbon nanotube composite material precursor; The carbon nanotube dispersion is an aqueous solution of carbon nanotubes after acidification, and the preparation steps of the carbon nanotubes after acidification are as follows: adding multi-walled carbon nanotubes to a 37wt% hydrochloric acid solution, the mass ratio of the multi-walled carbon nanotubes to the 37wt% hydrochloric acid solution is 1:5, stirring for 1h, and then ultrasonically dispersing, the ultrasonic dispersion temperature is 80°C, the ultrasonic dispersion time is 3h, suction filtering, washing with deionized water to neutrality, and vacuum drying at 60°C for 6h to obtain the carbon nanotubes after acidification; Step 2: placing the V-doped WO3-carbon nanotube composite material precursor in a muffle furnace, and calcining it in an argon atmosphere at a temperature of 520° C. for 2 hours. After the calcination, cooling it to room temperature in an argon atmosphere, grinding and sieving, to obtain a V-doped WO3-carbon nanotube composite material with an average particle size of less than 0.1 μm; Step 3: Place the V-doped WO3-carbon nanotube composite material, vinyl silicone rubber and dispersant γ-(methacryloyloxy)propyltrimethoxysilane in a mass ratio of 25:100:3 into a mixer and stir at a speed of 300 r / min to mix evenly, then refine in an open mill at a temperature of 200°C for 12 min, and then mold in a molding machine to obtain a hydrogen-sensitive color-changing film based on nanomaterials.

[0032] Comparative Example 1 A method for preparing a hydrogen-sensitive color-changing film comprises the following steps: Step 1: dissolve sodium tungstate in deionized water, mix well, add sodium metavanadate, adjust the pH to 2 with 0.3 mol / L hydrochloric acid aqueous solution, add n-propanol, stir and mix to obtain a mixed solution, wherein the mixed solution is obtained by mixing sodium tungstate, deionized water, sodium metavanadate and n-propanol in a mass ratio of 100:145:0.6:2.5, transfer the mixed solution to a reactor, and undergo a hydrothermal reaction at a temperature of 170°C for 10 hours. After the reaction is completed, cool and centrifuge at a rate of 6000 r / min for 6 minutes. The solid product obtained by centrifugation is washed with deionized water and anhydrous ethanol until neutral, and then vacuum dried in a 60°C vacuum drying oven for 12 hours to obtain a V-doped WO3 composite material precursor; Step 2: placing the V-doped WO3 precursor in a muffle furnace and calcining it in an argon atmosphere at a temperature of 500° C. for 2.5 hours. After the calcination, cooling it to room temperature in an argon atmosphere, grinding and sieving it to obtain V-doped WO3 with an average particle size of less than 0.1 μm; Step 3: Put V-doped WO3, vinyl silicone rubber and dispersant γ-(methacryloyloxy)propyltrimethoxysilane in a mass ratio of 24:100:2.5 into a mixer and stir at a speed of 280 r / min to mix evenly, and then refine in an open mill at a temperature of 185°C and a time of 14 min. Then, mold in a molding machine to obtain a hydrogen-sensitive color-changing film.

[0033] Comparative Example 2 A method for preparing a hydrogen-sensitive color-changing film comprises the following steps: Step 1: dissolve sodium tungstate in deionized water, mix well, adjust the pH to 2 with 0.3 mol / L hydrochloric acid aqueous solution, add n-propanol, stir and mix, and then add 50 g / L carbon nanotube dispersion to obtain a mixed solution, wherein the mixed solution is obtained by mixing sodium tungstate, deionized water, n-propanol and carbon nanotube dispersion in a mass ratio of 100:145:2.5:26. Transfer the mixed solution to a reactor for hydrothermal reaction at a temperature of 170°C for 10 hours. After the reaction is completed, cool and centrifuge at a rate of 6000 r / min for 6 minutes. The solid product obtained by centrifugation is washed with deionized water and anhydrous ethanol until neutral, and then vacuum dried in a vacuum drying oven at 60°C for 12 hours to obtain a WO3-carbon nanotube composite material precursor. The carbon nanotube dispersion is an aqueous solution of carbon nanotubes after acidification, and the preparation steps of the carbon nanotubes after acidification are as follows: adding multi-walled carbon nanotubes to a 37wt% hydrochloric acid solution, the mass ratio of the multi-walled carbon nanotubes to the 37wt% hydrochloric acid solution is 1:5, stirring for 1h, and then ultrasonically dispersing, the ultrasonic dispersion temperature is 75°C, the ultrasonic dispersion time is 3.5h, filtering, washing with deionized water to neutrality, and vacuum drying at 60°C for 6h to obtain the carbon nanotubes after acidification; Step 2: placing the WO3-carbon nanotube composite material precursor in a muffle furnace and calcining it in an argon atmosphere at a temperature of 500°C for 2.5 hours. After the calcination, cooling it to room temperature in an argon atmosphere, grinding and sieving it to obtain a WO3-carbon nanotube composite material with an average particle size of less than 0.1 μm; Step 3: Place the WO3-carbon nanotube composite material, vinyl silicone rubber and dispersant γ-(methacryloyloxy)propyltrimethoxysilane in a mass ratio of 24:100:2.5 into a mixer and stir at a speed of 280 r / min to mix evenly, and then refine in an open mill at a temperature of 185°C for 14 min, and then mold in a molding machine to obtain a hydrogen-sensitive color-changing film.

[0034] The multi-walled carbon nanotubes used in the embodiments and comparative examples of the present invention were purchased from Xianfeng Nanomaterial Technology Co., Ltd., with a purity of >98%, a diameter of 4-6 nm, and a length of 0.5-2 μm; the vinyl silicone rubber is high-strength H-110-3 methyl vinyl silicone resin purchased from Zhejiang Hengyecheng Silicone Co., Ltd.; other reagents are commercially available.

[0035] Corresponding tests were performed on the hydrogen-sensitive color-changing films in Examples 1-4 and Comparative Examples 1-2, and the test results are as follows: (1) Color change experiment: The hydrogen-sensitive color-changing films in Examples 1-4 and Comparative Examples 1-2 were placed in different test tubes, and 10% hydrogen (90% nitrogen) was introduced at a distance of 10 cm from the sample. The purge flow rate was 10 L / min. During the test, the temperature was 23±2°C and the humidity was 50±10%. Color change occurred during the test, and the substrate turned blue. The color change time was recorded. The test results are shown in Table 1: (2) Mechanical property test: Mechanical property test was performed on the hydrogen-sensitive color-changing films in Examples 1-4 and Comparative Examples 1-2, wherein the Shore hardness test was performed according to ASTM D2240-2015 standard, type Shore A; the tensile property test was performed according to GB / T 528-2009 standard, with a tensile rate of 50 mm / min; the test results were recorded respectively; the test results are shown in Table 1: Table 1 Test items Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Color change time (s) 56 50 47 46 68 65 Shore Hardness 69 73 74 74 55 70 Tensile strength (MPa) 11.5 12.3 12.7 12.5 8.4 11.2 Elongation at break (%) 261 272 278 281 219 263 According to the test results of Table 1, it can be seen that embodiments 1-4 have excellent hydrogen response ability, fast color change time, high hardness and good mechanical properties. Carbon nanotubes have high specific surface area and abundant reaction sites, which can effectively improve the sensitivity and response speed of composite materials. WO3 has high electron density and oxygen mobility, which can effectively improve the conductivity and hydrogen-sensitive performance of composite materials. In V-doped WO3, V exists in +5 valence state, which can replace the tungsten atoms in WO3, generate holes, and enhance the hydrogen-sensitive performance of WO3. At the same time, since the radius of vanadium is close to the radius of tungsten, the crystal structure of WO3 will not be destroyed. V-doped WO3 has high specific surface area and abundant reaction sites. In addition, V-doped WO3 can also increase the adsorption capacity of hydrogen and improve the selectivity of hydrogen. The prepared hydrogen-sensitive color-changing film has the characteristics of high sensitivity and short response time. Therefore, the color change time of the hydrogen-sensitive color-changing film corresponding to embodiment 4 is 46s, and the Shore hardness corresponding to embodiment 3 is 74, the tensile strength is 12.7MPa, and the elongation at break is 278%. In comparative example 1, no carbon nanotubes were added, the discoloration time was prolonged, and the Shore hardness and mechanical properties were greatly reduced; in comparative example 2, no V atoms were added to WO3, the discoloration time was prolonged, and the Shore hardness and mechanical properties were affected, but the effect was small.

[0036] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a hydrogen-sensitive color-changing film based on nanomaterials, characterized in that: The following steps are involved: Step 1: dissolve sodium tungstate in deionized water, mix well, add sodium metavanadate, adjust the pH to 1.6-2.4 with aqueous hydrochloric acid, add n-propanol, stir and mix, add carbon nanotube dispersion to obtain a mixed solution, transfer the mixed solution to a reactor, and perform a hydrothermal reaction. After the reaction is completed, cool and centrifuge, wash and dry the solid product obtained by centrifugation to obtain a V-doped WO3-carbon nanotube composite material precursor; Step 2: placing the V-doped WO3-carbon nanotube composite material precursor in a muffle furnace, and calcining it in an inert gas atmosphere. After the calcination, cooling it to room temperature in an inert gas atmosphere, grinding and sieving it, to obtain a V-doped WO3-carbon nanotube composite material; Step 3: Stir and mix the V-doped WO3-carbon nanotube composite material, vinyl silicone rubber and dispersant, and then refine and shape them to obtain a hydrogen-sensitive color-changing film based on nanomaterials.

2. The method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to claim 1, characterized in that: In the step 1, the mass ratio of sodium tungstate, deionized water, sodium metavanadate, n-propanol and carbon nanotube dispersion is 100:130-150:0.2-0.7:1-3:18-30.

3. The method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to claim 1, characterized in that: In the step 1, the temperature of the hydrothermal reaction is 150-180° C., and the time of the hydrothermal reaction is 8-12 hours.

4. The method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to claim 1, characterized in that: In the step 1, the concentration of the carbon nanotube dispersion is 50 g / L, and the carbon nanotube dispersion is an aqueous solution of carbon nanotubes after acidification; The steps for preparing the acid-treated carbon nanotubes are as follows: The multi-walled carbon nanotubes were added into a 37wt% hydrochloric acid solution in a mass ratio of 1:

5. The mixture was stirred for 1 hour and then ultrasonically dispersed at a temperature of 70-80°C for 3-4 hours. The mixture was filtered and washed with deionizer until neutral. The mixture was vacuum dried at 60°C for 6 hours to obtain the acidified carbon nanotubes.

5. The method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to claim 1, characterized in that: In the step 2, the calcination temperature is 450-520° C., and the calcination time is 2-3 hours.

6. The method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to claim 1, characterized in that: In the step 2, the average particle size of the V-doped WO3-carbon nanotube composite material is less than 0.1 μm.

7. The method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to claim 1, characterized in that: In the step 3, the mass ratio of the V-doped WO3-carbon nanotube composite material, the vinyl silicone rubber and the dispersant is 18-25:100:1-3.

8. The method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to claim 1, characterized in that: In the step three, the dispersant includes a silane coupling agent.

9. The method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to claim 1, characterized in that: In the step 3, the rotation speed of the stirring and mixing is 240-300 r / min; the temperature of the refining is 160-200° C., and the refining time is 12-15 min.

10. A hydrogen-sensitive color-changing film based on nanomaterials prepared by the method for preparing a hydrogen-sensitive color-changing film based on nanomaterials according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Vanadium-doped crystalline tungsten trioxide electrochromic film and preparation method thereof

    CN114180850A

  • Preparation method of nickel-plated carbon nanotube enhanced PDMS composite film with conductivity and product thereof

    CN112980191A

  • Hydrogen sensor and intelligent monitoring system

    CN115963151A

  • Hydrogen gas sensing film and hydrogen gas sensor

    JP2005331364A

Cited By

  • Preparation method of vanadium-containing modified tungsten oxide-titanium dioxide composite hydrogen-sensitive color-changing material

    CN121801555A