High-strength anti-aging PP film for capacitor and preparation method of high-strength anti-aging PP film

By reacting branched boron nitride-skeleton materials with diethylenetriamine and adding divinylbenzene, a high-strength and aging-resistant PP film is prepared, which solves the aging problem of polypropylene films in high-temperature and high-pressure environments and improves the performance of capacitors. stability and longevity.

CN118725384AInactive Publication Date: 2024-10-01扬州博恒新能源材料科技有限公司

Patent Information

Application Number
CN202410959867.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional polypropylene films are prone to aging and fracture in high-temperature and high-pressure environments, resulting in reduced stability and lifespan of capacitors. Existing technologies increase strength by adding reinforcing fillers, but this can easily lead to filler agglomeration and reduced strength.

Method used

The branched boron nitride-skeleton material composite is reacted with diethylenetriamine to generate an aminated boron nitride-skeleton material, and divinylbenzene is added to the polypropylene through a vacuum suction device and a screw melt extrusion system. Prepare high-strength and aging-resistant PP film, and combine it with corona treatment to improve the strength and aging resistance of the film.

Benefits of technology

It improves the strength and aging resistance of the PP film, enhances the dispersion performance and compatibility of boron nitride-framework materials, and extends the service life of the capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of polypropylene films, in particular to a high-strength anti-aging PP film for a capacitor and a preparation method of the high-strength anti-aging PP film. The invention prepares boron nitride with large specific surface area and high strength. Then 2-methylimidazole and zinc nitrate hexahydrate are used, a framework material is loaded on boron nitride, on one hand, the dispersing performance of boron nitride is enhanced through loading of the framework material, on the other hand, the mechanical strength of the prepared boron nitride-framework material compound is enhanced, and the strength of the PP film is improved. And then the boron nitride-framework material compound is subjected to amino treatment, so that the boron nitride-framework material compound has a large number of amino groups, the compatibility and dispersity of the boron nitride-framework material compound in a matrix are enhanced, and the strength and aging resistance of the PP film are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polypropylene films, in particular to a high-strength and aging-resistant PP film for capacitors and a preparation method thereof. Background Art

[0002] In electronic devices and power equipment, capacitors are a key electronic component that is usually used to store and release electrical energy. As one of the important components of capacitors, polypropylene film undertakes important functions such as insulation, support and dielectric. However, traditional polypropylene film is prone to aging, breakage and performance degradation under long-term use and working environments such as high temperature and high pressure, which affects the stability and life of the capacitor. In order to improve the strength, stability and aging resistance of PP film, thereby improving the performance and reliability of capacitors, the prior art usually introduces reinforcing fillers such as nano oxides and carbon nanotubes into PP film, or adds some functional modifiers such as antioxidants and ultraviolet absorbers to improve the mechanical properties and aging resistance of PP film. However, the addition of a large amount of reinforcing fillers will cause filler agglomeration, thereby causing a decrease in the strength of PP film.

[0003] In order to solve the above problems and improve the strength and stability of the PP film, the present invention provides a high-strength and aging-resistant PP film for capacitors and a preparation method thereof. Summary of the invention

[0004] The object of the present invention is to provide a high-strength and aging-resistant PP film for capacitors and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing a high-strength aging-resistant PP film for capacitors comprises the following steps:

[0007] Step 1: Take a branched boron nitride-framework material complex, add diethylenetriamine, and react at 110-112° C. for 10-12 hours to obtain an amino boron nitride-framework material complex;

[0008] Step 2: Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat them until they are melted, add amino boron nitride-skeleton material composite, divinylbenzene, antioxidant, alcohol ester twelve, heat stabilizer, and initiator, stir evenly to obtain raw materials, input them into the screw melt extrusion system through a vacuum suction device, melt them, inject them into the die head, extrude the melt through the lip of the die head, cool the melt to 80-105°C, cast it into a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength and aging-resistant PP film for capacitors.

[0009] More optimally, the high-strength and aging-resistant PP film for capacitors includes the following components, by weight: 200-220 parts of polypropylene, 3-4 parts of polytrimethylene terephthalate, 12-15 parts of maleic anhydride grafted polypropylene, 10-15 parts of amino boron nitride-skeleton material composite, 1-1.5 parts of divinylbenzene, 3-4 parts of antioxidant, 2-3 parts of alcohol ester dodecahydrate, 3-4 parts of heat stabilizer, and 1-1.5 parts of initiator.

[0010] More optimally, the preparation method of the branched boron nitride-framework material complex is: take the boron nitride-framework material complex and succinic anhydride, stir evenly, add diethanolamine under a nitrogen environment, heat to 120-122° C., stir for 5-7 hours, and obtain the branched boron nitride-framework material complex.

[0011] More optimally, the preparation method of the boron nitride-framework material complex is: take 2-methylimidazole and methanol, stir evenly to obtain a 2-methylimidazole solution; take boron nitride and methanol, ultrasonically disperse for 30-40 minutes, add zinc nitrate hexahydrate, ultrasonically disperse for 10-20 minutes, then dropwise add the 2-methylimidazole solution, stir at 25-30°C for 46-50 hours, centrifuge, wash, and dry to obtain a boron nitride-framework material complex.

[0012] More optimally, the preparation method of boron nitride is: take boric acid, melamine, and deionized water, heat to 88-92°C, stir evenly, then cool to 80-82°C, keep warm for 6-7h, cool to 25-30°C, filter, and obtain a precursor; spray deionized water onto the surface of the precursor, then mix evenly, granulate, sieve, and dry to obtain compound A; place compound A at 1100°C and nitrogen atmosphere for reaction for 4-5h, and ball mill to obtain boron nitride.

[0013] More optimally, the antioxidant is any one or more of antioxidant 1010, antioxidant 1076, and antioxidant 164.

[0014] More optimally, the thermal stabilizer is triphenyl phosphate.

[0015] More optimally, the initiator is 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0017] (1) The present invention uses a granulation method to prepare a boron nitride with a large specific surface area and high strength through high-temperature pyrolysis. Then, 2-methylimidazole and zinc nitrate hexahydrate are used to load a skeleton material on the boron nitride. The loading of the skeleton material not only enhances the dispersion performance of the boron nitride, but also enhances the mechanical strength of the prepared boron nitride-skeleton material composite, thereby improving the strength of the PP film.

[0018] (2) First, the boron nitride-framework material composite is subjected to branching treatment, so that a large number of terminal hydroxyl groups are grafted on the boron nitride-framework material composite, and then it is further modified using diethylenetriamine to convert the terminal hydroxyl groups into terminal amino groups, so that the boron nitride-framework material composite has a large number of amino groups. The compatibility and dispersibility of the boron nitride-framework material composite in the matrix are enhanced, and the strength and aging resistance of the PP film are enhanced.

[0019] (3) Adding divinylbenzene to polypropylene, the polypropylene macromolecular free radicals can react with divinylbenzene to generate a long-chain branched structure, thereby improving the strength of polypropylene and thus improving the strength of the PP film. The high-strength aging-resistant PP film for capacitors prepared by the present invention has good aging resistance and high strength. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The purchasers of all raw materials involved in the present invention are not subject to any special restrictions, and exemplary examples include:

[0022] Maleic anhydride grafted polypropylene: can be purchased from Dongguan Dingxin Plastic Raw Materials Co., Ltd., model: B1-1; polypropylene: can be purchased from Shanghai Yuanye Biotechnology Co., Ltd., model: S51655; polytrimethylene terephthalate: can be purchased from DuPont, model: 2261.

[0023] Embodiment 1: A method for preparing a high-strength aging-resistant PP film for capacitors, comprising the following steps:

[0024] Step 1: Preparation of Boron Nitride:

[0025] Take 18g of boric acid, 10g of melamine, and 1000mL of deionized water, heat to 90°C, stir evenly, then cool to 81°C, keep warm for 6.5h, cool to 27°C, filter, and obtain a precursor; spray 50mL of deionized water onto the surface of 500g of the precursor, then mix evenly, granulate, pass through a 20-mesh sieve, and dry to obtain compound A; place compound A at 1100°C and nitrogen atmosphere for reaction for 4.5h, and ball mill to obtain boron nitride;

[0026] Step 2: Preparation of boron nitride-framework material composite:

[0027] Take 2.1g 2-methylimidazole and 100mL methanol, stir evenly to obtain a 2-methylimidazole solution; take 2g boron nitride and 100mL methanol, ultrasonically disperse for 35min, add 4g zinc nitrate hexahydrate, ultrasonically disperse for 15min, then dropwise add the 2-methylimidazole solution, stir at 27°C for 48h, centrifuge, wash, and dry to obtain a boron nitride-framework material composite;

[0028] Step 3: Preparation of amination boron nitride-framework material composite:

[0029] S1: Take 5g of boron nitride-framework material complex and 10g of succinic anhydride, stir evenly, add 16g of diethanolamine under nitrogen environment, heat to 121°C, stir for 6h, and obtain a branched boron nitride-framework material complex;

[0030] S2: Take 5 g of the branched boron nitride-framework material composite, add 16 g of diethylenetriamine, and react at 111° C. for 11 h to obtain an amino boron nitride-framework material composite;

[0031] Step 4: Preparation of high-strength aging-resistant PP film for capacitors:

[0032] Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat them until they are melted, add amino boron nitride-skeleton material composite, divinylbenzene, antioxidant 1010, alcohol ester twelve, heat stabilizer triphenyl phosphate, initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, stir evenly to obtain raw materials, input them into a screw melt extrusion system through a vacuum suction device, melt them, pass through a pre-filter, a metering pump and a candle filter, and then inject them into a T-hanger die head, extrude a sheet melt through the lip of the die head, cool the melt to 90° C., cast a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength and aging-resistant PP film for capacitors;

[0033] The high-strength and aging-resistant PP film for capacitors includes the following components, by weight: 210 parts of polypropylene, 3.5 parts of polytrimethylene terephthalate, 13 parts of maleic anhydride grafted polypropylene, 13 parts of amino boron nitride-skeleton material composite, 1.2 parts of divinylbenzene, 3.5 parts of antioxidant 1010, 2.5 parts of alcohol ester dodecahydrate, 3.5 parts of heat stabilizer triphenyl phosphate, and 1.2 parts of initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

[0034] Embodiment 2: A method for preparing a high-strength aging-resistant PP film for capacitors, comprising the following steps:

[0035] Step 1: Preparation of Boron Nitride:

[0036] Take 18g of boric acid, 10g of melamine, and 1000mL of deionized water, heat to 88°C, stir evenly, then cool to 80°C, keep warm for 6h, cool to 25°C, filter, and obtain a precursor; spray 50mL of deionized water onto the surface of 500g of the precursor, then mix evenly, granulate, pass through a 20-mesh sieve, and dry to obtain compound A; place compound A at 1100°C and nitrogen atmosphere for reaction for 4h, and ball mill to obtain boron nitride;

[0037] Step 2: Preparation of boron nitride-framework material composite:

[0038] Take 2.1g 2-methylimidazole and 100mL methanol, stir evenly to obtain a 2-methylimidazole solution; take 2g boron nitride and 100mL methanol, ultrasonically disperse for 30min, add 4g zinc nitrate hexahydrate, ultrasonically disperse for 10min, then dropwise add the 2-methylimidazole solution, stir at 25°C for 46h, centrifuge, wash, and dry to obtain a boron nitride-framework material composite;

[0039] Step 3: Preparation of amination boron nitride-framework material composite:

[0040] S1: Take 5g of boron nitride-framework material complex and 10g of succinic anhydride, stir evenly, add 16g of diethanolamine under nitrogen environment, heat to 120°C, stir for 5h, and obtain a branched boron nitride-framework material complex;

[0041] S2: Take 5 g of the branched boron nitride-framework material composite, add 16 g of diethylenetriamine, and react at 110° C. for 10 h to obtain an amino boron nitride-framework material composite;

[0042] Step 4: Preparation of high-strength aging-resistant PP film for capacitors:

[0043] Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat them until they are melted, add amino boron nitride-skeleton material composite, divinylbenzene, antioxidant 1010, alcohol ester twelve, heat stabilizer triphenyl phosphate, initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, stir evenly to obtain raw materials, input them into a screw melt extrusion system through a vacuum suction device, melt them, pass through a pre-filter, a metering pump and a candle filter, and then inject them into a T-hanger die head, extrude a sheet melt through the lip of the die head, cool the melt to 80°C, cast a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength and aging-resistant PP film for capacitors;

[0044] The high-strength and aging-resistant PP film for capacitors includes the following components, measured by weight: 200 parts of polypropylene, 3 parts of polytrimethylene terephthalate, 12 parts of maleic anhydride grafted polypropylene, 10 parts of amino boron nitride-skeleton material composite, 1 part of divinylbenzene, 3 parts of antioxidant 1010, 2 parts of alcohol ester dodecahydrate, 3 parts of heat stabilizer triphenyl phosphate, and 1 part of initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

[0045] Embodiment 3: A method for preparing a high-strength aging-resistant PP film for capacitors, comprising the following steps:

[0046] Step 1: Preparation of Boron Nitride:

[0047] Take 18g of boric acid, 10g of melamine, and 1000mL of deionized water, heat to 92°C, stir evenly, then cool to 82°C, keep warm for 7h, cool to 30°C, filter, and obtain a precursor; spray 50mL of deionized water onto the surface of 500g of the precursor, then mix evenly, granulate, pass through a 20-mesh sieve, and dry to obtain compound A; place compound A at 1100°C and nitrogen atmosphere for reaction for 5h, and ball mill to obtain boron nitride;

[0048] Step 2: Preparation of boron nitride-framework material composite:

[0049] Take 2.1g 2-methylimidazole and 100mL methanol, stir evenly to obtain a 2-methylimidazole solution; take 2g boron nitride and 100mL methanol, ultrasonically disperse for 40min, add 4g zinc nitrate hexahydrate, ultrasonically disperse for 20min, then dropwise add the 2-methylimidazole solution, stir at 30°C for 50h, centrifuge, wash, and dry to obtain a boron nitride-framework material composite;

[0050] Step 3: Preparation of amination boron nitride-framework material composite:

[0051] S1: Take 5g of boron nitride-framework material complex and 10g of succinic anhydride, stir evenly, add 16g of diethanolamine under nitrogen environment, heat to 122°C, stir for 7h, and obtain a branched boron nitride-framework material complex;

[0052] S2: Take 5 g of the branched boron nitride-framework material composite, add 16 g of diethylenetriamine, and react at 112° C. for 12 h to obtain an amino boron nitride-framework material composite;

[0053] Step 4: Preparation of high-strength aging-resistant PP film for capacitors:

[0054] Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat them until they are melted, add amino boron nitride-skeleton material composite, divinylbenzene, antioxidant 1010, alcohol ester twelve, heat stabilizer triphenyl phosphate, initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, stir evenly to obtain raw materials, input them into a screw melt extrusion system through a vacuum suction device, melt them, pass through a pre-filter, a metering pump and a candle filter, and then inject them into a T-hanger die head, extrude a sheet melt through the lip of the die head, cool the melt to 105° C., cast a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength and aging-resistant PP film for capacitors;

[0055] The high-strength and aging-resistant PP film for capacitors includes the following components, by weight: 220 parts of polypropylene, 4 parts of polytrimethylene terephthalate, 15 parts of maleic anhydride grafted polypropylene, 15 parts of amino boron nitride-skeleton material composite, 1.5 parts of divinylbenzene, 4 parts of antioxidant 1010, 3 parts of alcohol ester dodecahydrate, 4 parts of heat stabilizer triphenyl phosphate, and 1.5 parts of initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

[0056] Comparative Example 1: No skeleton material is loaded, and the rest is the same as Example 1:

[0057] Step 1: Preparation of Boron Nitride:

[0058] Take 18g of boric acid, 10g of melamine, and 1000mL of deionized water, heat to 90°C, stir evenly, then cool to 81°C, keep warm for 6.5h, cool to 27°C, filter, and obtain a precursor; spray 50mL of deionized water onto the surface of 500g of the precursor, then mix evenly, granulate, pass through a 20-mesh sieve, and dry to obtain compound A; place compound A at 1100°C and nitrogen atmosphere for reaction for 4.5h, and ball mill to obtain boron nitride;

[0059] Step 2: Preparation of amination boron nitride:

[0060] S1: Take 5g of boron nitride and 10g of succinic anhydride, stir evenly, add 16g of diethanolamine under nitrogen environment, heat to 121°C, stir for 6h, and obtain branched boron nitride;

[0061] S2: Take 5 g of branched boron nitride, add 16 g of diethylenetriamine, and react at 111°C for 11 h to obtain amino boron nitride;

[0062] Step 3: Preparation of high-strength aging-resistant PP film for capacitors:

[0063] Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat until melted, add amino boron nitride, divinylbenzene, antioxidant 1010, alcohol ester twelve, heat stabilizer triphenyl phosphate, initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, stir evenly to obtain raw materials, input the raw materials into a screw melt extrusion system through a vacuum suction device, melt, pass through a pre-filter, a metering pump and a candle filter, and then inject into a T-hanger die head, extrude a sheet melt through the lip of the die head, cool the melt to 90° C., cast a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength aging-resistant PP film for capacitors;

[0064] The high-strength and aging-resistant PP film for capacitors includes the following components, by weight: 210 parts of polypropylene, 3.5 parts of polytrimethylene terephthalate, 13 parts of maleic anhydride grafted polypropylene, 13 parts of amino boron nitride, 1.2 parts of divinylbenzene, 3.5 parts of antioxidant 1010, 2.5 parts of alcohol ester dodecahydrate, 3.5 parts of heat stabilizer triphenyl phosphate, and 1.2 parts of initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

[0065] Comparative Example 2: The boron nitride-framework material composite is not subjected to amination treatment, and the rest is the same as Example 1:

[0066] Step 1: Preparation of Boron Nitride:

[0067] Take 18g of boric acid, 10g of melamine, and 1000mL of deionized water, heat to 90°C, stir evenly, then cool to 81°C, keep warm for 6.5h, cool to 27°C, filter, and obtain a precursor; spray 50mL of deionized water onto the surface of 500g of the precursor, then mix evenly, granulate, pass through a 20-mesh sieve, and dry to obtain compound A; place compound A at 1100°C and nitrogen atmosphere for reaction for 4.5h, and ball mill to obtain boron nitride;

[0068] Step 2: Preparation of boron nitride-framework material composite:

[0069] Take 2.1g 2-methylimidazole and 100mL methanol, stir evenly to obtain a 2-methylimidazole solution; take 2g boron nitride and 100mL methanol, ultrasonically disperse for 35min, add 4g zinc nitrate hexahydrate, ultrasonically disperse for 15min, then dropwise add the 2-methylimidazole solution, stir at 27°C for 48h, centrifuge, wash, and dry to obtain a boron nitride-framework material composite;

[0070] Step 3: Preparation of high-strength aging-resistant PP film for capacitors:

[0071] Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat them until they are melted, add boron nitride-skeleton material composite, divinylbenzene, antioxidant 1010, alcohol ester twelve, heat stabilizer triphenyl phosphate, initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane to obtain raw materials, input them into a screw melt extrusion system through a vacuum suction device, melt them, pass through a pre-filter, a metering pump and a candle filter, and then inject them into a T-hanger die head, extrude a sheet melt through the lip of the die head, cool the melt to 90° C., cast a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength and aging-resistant PP film for capacitors;

[0072] The high-strength and aging-resistant PP film for capacitors includes the following components, by weight: 210 parts of polypropylene, 3.5 parts of polytrimethylene terephthalate, 13 parts of maleic anhydride grafted polypropylene, 13 parts of boron nitride-skeleton material composite, 1.2 parts of divinylbenzene, 3.5 parts of antioxidant 1010, 2.5 parts of alcohol ester dodecahydrate, 3.5 parts of heat stabilizer triphenyl phosphate, and 1.2 parts of initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

[0073] Comparative Example 3: No divinylbenzene was added, and the rest was the same as Example 1:

[0074] Step 1: Preparation of Boron Nitride:

[0075] Take 18g of boric acid, 10g of melamine, and 1000mL of deionized water, heat to 90°C, stir evenly, then cool to 81°C, keep warm for 6.5h, cool to 27°C, filter, and obtain a precursor; spray 50mL of deionized water onto the surface of 500g of the precursor, then mix evenly, granulate, pass through a 20-mesh sieve, and dry to obtain compound A; place compound A at 1100°C and nitrogen atmosphere for reaction for 4.5h, and ball mill to obtain boron nitride;

[0076] Step 2: Preparation of boron nitride-framework material composite:

[0077] Take 2.1g 2-methylimidazole and 100mL methanol, stir evenly to obtain a 2-methylimidazole solution; take 2g boron nitride and 100mL methanol, ultrasonically disperse for 35min, add 4g zinc nitrate hexahydrate, ultrasonically disperse for 15min, then dropwise add the 2-methylimidazole solution, stir at 27°C for 48h, centrifuge, wash, and dry to obtain a boron nitride-framework material composite;

[0078] Step 3: Preparation of amination boron nitride-framework material composite:

[0079] S1: Take 5g of boron nitride-framework material complex and 10g of succinic anhydride, stir evenly, add 16g of diethanolamine under nitrogen environment, heat to 121°C, stir for 6h, and obtain a branched boron nitride-framework material complex;

[0080] S2: Take 5 g of the branched boron nitride-framework material composite, add 16 g of diethylenetriamine, and react at 111° C. for 11 h to obtain an amino boron nitride-framework material composite;

[0081] Step 4: Preparation of high-strength aging-resistant PP film for capacitors:

[0082] Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat them until they are melted, add amino boron nitride-skeleton material composite, antioxidant 1010, alcohol ester twelve, heat stabilizer triphenyl phosphate, initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, stir evenly to obtain raw materials, input them into a screw melt extrusion system through a vacuum suction device, melt them, pass through a pre-filter, a metering pump and a candle filter, and then inject them into a T-hanger die head, extrude a sheet melt through the lip of the die head, cool the melt to 90° C., cast a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength and aging-resistant PP film for capacitors;

[0083] The high-strength and aging-resistant PP film for capacitors includes the following components, by weight: 210 parts of polypropylene, 3.5 parts of polytrimethylene terephthalate, 13 parts of maleic anhydride grafted polypropylene, 13 parts of amino boron nitride-skeleton material composite, 3.5 parts of antioxidant 1010, 2.5 parts of alcohol ester dodecahydrate, 3.5 parts of heat stabilizer triphenyl phosphate, and 1.2 parts of initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

[0084] Comparative Example 4: Boron nitride was prepared without using the method provided by the present invention, and the rest was the same as Example 1:

[0085] Step 1: Preparation of boron nitride-framework material composite:

[0086] Take 2.1g 2-methylimidazole and 100mL methanol, stir evenly to obtain a 2-methylimidazole solution; take 2g boron nitride and 100mL methanol, ultrasonically disperse for 35min, add 4g zinc nitrate hexahydrate, ultrasonically disperse for 15min, then dropwise add the 2-methylimidazole solution, stir at 27°C for 48h, centrifuge, wash, and dry to obtain a boron nitride-framework material composite;

[0087] The boron nitride: Model: S40088, can be purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0088] Step 2: Preparation of amination boron nitride-framework material composite:

[0089] S1: Take 5g of boron nitride-framework material complex and 10g of succinic anhydride, stir evenly, add 16g of diethanolamine under nitrogen environment, heat to 121°C, stir for 6h, and obtain a branched boron nitride-framework material complex;

[0090] S2: Take 5 g of the branched boron nitride-framework material composite, add 16 g of diethylenetriamine, and react at 111° C. for 11 h to obtain an amino boron nitride-framework material composite;

[0091] Step 3: Preparation of high-strength aging-resistant PP film for capacitors:

[0092] Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat them until they are melted, add amino boron nitride-skeleton material composite, divinylbenzene, antioxidant 1010, alcohol ester twelve, heat stabilizer triphenyl phosphate, initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, stir evenly to obtain raw materials, input them into a screw melt extrusion system through a vacuum suction device, melt them, pass through a pre-filter, a metering pump and a candle filter, and then inject them into a T-hanger die head, extrude a sheet melt through the lip of the die head, cool the melt to 90° C., cast a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength and aging-resistant PP film for capacitors;

[0093] The high-strength and aging-resistant PP film for capacitors includes the following components, by weight: 210 parts of polypropylene, 3.5 parts of polytrimethylene terephthalate, 13 parts of maleic anhydride grafted polypropylene, 13 parts of amino boron nitride-skeleton material composite, 1.2 parts of divinylbenzene, 3.5 parts of antioxidant 1010, 2.5 parts of alcohol ester dodecahydrate, 3.5 parts of heat stabilizer triphenyl phosphate, and 1.2 parts of initiator 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

[0094] experiment:

[0095] The PP films prepared in Examples 1-3 and Comparative Examples 1-4 were used for performance testing. The tensile strength of the PP films at 30°C was tested using an Instron 1185 universal testing machine with reference to GB / T1040-92. The PP films were then irradiated with UV radiation at a dose of 0.35 W / m 2 (340nm), and then the PP film was immersed in hot water at 80°C for 7 days, taken out, and the treated PP film was obtained. The tensile strength of the treated PP film was tested to characterize its aging resistance. The obtained data are shown below:

[0096]

[0097] Conclusion: Comparative Example 1 does not load the skeleton material, the dispersion performance of boron nitride is poor, the mechanical strength is reduced, and the strength of the PP film is reduced. Comparative Example 2 does not perform an amination treatment on the boron nitride-skeleton material composite, the dispersion of the boron nitride-skeleton material composite in the matrix is ​​poor, and the strength and aging resistance of the PP film are reduced. Comparative Example 3 does not add divinylbenzene, and the aging resistance of the PP film is reduced. Comparative Example 4 does not use the method provided by the present invention to prepare boron nitride, the specific surface area of ​​boron nitride is small, the loaded skeleton material is small, and the strength of the PP film is reduced. Examples 1-3 of the present invention prepare a boron nitride with a large specific surface area and high strength. Then, 2-methylimidazole and zinc nitrate hexahydrate are used to load the skeleton material on the boron nitride. The loading of the skeleton material enhances the dispersion performance of boron nitride on the one hand, and enhances the mechanical strength of the prepared boron nitride-skeleton material composite on the other hand, thereby improving the strength of the PP film. Then, the boron nitride-framework material composite is subjected to amino treatment, so that the boron nitride-framework material composite has a large number of amino groups, which enhances the compatibility and dispersibility of the boron nitride-framework material composite in the matrix, and enhances the strength and aging resistance of the PP film.

[0098] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-strength, aging-resistant PP film for capacitors. Features: The following steps are involved: Step 1: Take a branched boron nitride-framework material complex, add diethylenetriamine, and react at 110-112° C. for 10-12 hours to obtain an amino boron nitride-framework material complex; Step 2: Take polypropylene, polytrimethylene terephthalate, and maleic anhydride grafted polypropylene, heat them until they are melted, add amino boron nitride-skeleton material composite, divinylbenzene, antioxidant, alcohol ester twelve, heat stabilizer, and initiator, stir evenly to obtain raw materials, input them into the screw melt extrusion system through a vacuum suction device, melt them, inject them into the die head, extrude the melt through the lip of the die head, cool the melt to 80-105°C, cast it into a sheet, and then perform synchronous biaxial stretching, and then perform heat and cold setting treatment to obtain a base film, send the base film into a traction device, treat the film surface using a corona treatment method in the traction section, roll it up, perform aging treatment, and slit it to obtain a high-strength and aging-resistant PP film for capacitors.

2. The method for preparing a high-strength aging-resistant PP film for capacitors according to claim 1, Features: The high-strength and aging-resistant PP film for capacitors includes the following components, by weight: 200-220 parts of polypropylene, 3-4 parts of polytrimethylene terephthalate, 12-15 parts of maleic anhydride grafted polypropylene, 10-15 parts of amino boron nitride-skeleton material composite, 1-1.5 parts of divinylbenzene, 3-4 parts of antioxidant, 2-3 parts of alcohol ester dodecahydrate, 3-4 parts of heat stabilizer, and 1-1.5 parts of initiator.

3. The method for preparing a high-strength aging-resistant PP film for capacitors according to claim 1, Features: The preparation method of the branched boron nitride-framework material composite is as follows: take the boron nitride-framework material composite and succinic anhydride, stir them evenly, add diethanolamine under nitrogen environment, heat to 120-122° C., stir for 5-7 hours, and obtain the branched boron nitride-framework material composite.

4. The method for preparing a high-strength aging-resistant PP film for capacitors according to claim 3, Features: The preparation method of the boron nitride-framework material composite comprises: taking 2-methylimidazole and methanol, stirring evenly to obtain a 2-methylimidazole solution; taking boron nitride and methanol, ultrasonically dispersing for 30-40 minutes, adding zinc nitrate hexahydrate, ultrasonically dispersing for 10-20 minutes, then dripping the 2-methylimidazole solution, stirring at 25-30° C. for 46-50 hours, centrifuging, washing, and drying to obtain the boron nitride-framework material composite.

5. The method for preparing a high-strength aging-resistant PP film for capacitors according to claim 4, Features: The preparation method of boron nitride is as follows: taking boric acid, melamine and deionized water, heating them to 88-92° C., stirring them evenly, then cooling them to 80-82° C., keeping them warm for 6-7 hours, cooling them to 25-30° C., filtering them, and obtaining a precursor; spraying deionized water onto the surface of the precursor, then mixing them evenly, granulating, sieving, and drying them, and obtaining compound A; placing compound A at 1100° C. and in a nitrogen atmosphere for reaction for 4-5 hours, and ball milling them, and obtaining boron nitride.

6. The method for preparing a high-strength aging-resistant PP film for capacitors according to claim 2, Features: The antioxidant is any one or more of antioxidant 1010 , antioxidant 1076 , and antioxidant 164 .

7. The method for preparing a high-strength aging-resistant PP film for capacitors according to claim 2, Features: The thermal stabilizer is triphenyl phosphate.

8. The method for preparing a high-strength aging-resistant PP film for capacitors according to claim 2, Features: The initiator is 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane.

9. A high-strength and aging-resistant PP film for capacitors prepared according to the method for preparing a high-strength and aging-resistant PP film for capacitors according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of high-melt strength polypropylene resin with long-chain branched structure characteristic

    CN103804795A

  • Glass fibre modification method and application thereof

    CN105293955A

  • Method for preparing special heat-conducting plastic applied to high-power LED lamp by compounding graphene / boron nitride / metal fiber / polyamide

    CN110540749A

  • Preparation method of high-thermal-conductivity natural rubber composite material

    CN112250917A

  • Composite dielectric film of nano boron nitride modified polypropylene and preparation method thereof

    CN112341654A

Cited By

  • High-bonding-strength flame-retardant composite current collector base film and preparation method thereof

    CN121226899A