Method for continuously producing depolymerized cellulose ether

By performing humidity control, heating and depolymerization processes in a continuous reactor, combined with the neutralization process, the problems of cellulose ether powder adhesion and foreign matter generation in the batch reactor are solved, and efficient and stable low-polymerization fibers are achieved. The production of plain ether reduces production costs and product foreign matter content.

CN118725404APending Publication Date: 2024-10-01SHIN ETSU CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410375560.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When existing batch reactors are used to produce low-polymerization cellulose ethers on an industrial scale, there are problems such as increased reactor space and investment costs, and the adhesion of cellulose ether powder leads to deterioration of heat transfer characteristics, unstable viscosity and the generation of foreign matter, which affects product quality.

Method used

Using a continuous reactor, the raw cellulose ether is brought into contact with water vapor through the humidity control process, heated during the temperature raising process, hydrogen chloride is used for depolymerization in the depolymerization process, and alkaline compounds are added in the neutralization process to control the process temperature and speed. To reduce adhesion and foreign matter generation.

Benefits of technology

It realizes the efficient production of low-polymerization cellulose ether that saves space and investment, reduces the adhesion of cellulose ether powder, suppresses the generation of yellowness and foreign matter, and improves the quality stability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725404A_ABST
    Figure CN118725404A_ABST
Patent Text Reader

Abstract

Provided is a method for producing a depolymerized cellulose ether with which it is possible to reduce adhesion of a cellulose ether powder to a reactor and with which it is possible to obtain a depolymerized cellulose ether in which yellowness and the amount of foreign matter generation are suppressed, while saving space and having high productivity. A method for continuously producing a depolymerized cellulose ether, which comprises at least: a) a humidifying step for obtaining a humidified cellulose ether by bringing a starting material cellulose ether (A), which is continuously supplied from a starting material tank (1) to a humidifying tank (2) and has a temperature of 3 DEG C or more and less than 40 DEG C, into contact with water vapor (B); b) a heating process: heating the humidified cellulose ether to obtain heated cellulose ether; c) a depolymerization step for obtaining a depolymerized cellulose ether product by continuously contacting gaseous hydrogen chloride (C) with the heated cellulose ether; and d) a neutralization step for obtaining a depolymerized cellulose ether (F) by mixing and neutralizing the depolymerized cellulose ether product with a basic compound (E).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a process for continuously producing depolymerized cellulose ethers. Background Art

[0002] Low-polymerization cellulose ethers are used for film coatings in solid preparations such as tablets. Such film coatings are used to mask the unpleasant taste of the drug while preventing the modification of the contained drug and controlling the dissolution behavior in the digestive organs after administration. In addition, films obtained by drying solutions of low-polymerization cellulose ethers are widely used as bases for film preparations or hard capsules.

[0003] Generally, low-polymerization cellulose ether is obtained by depolymerizing high-polymerization cellulose ether. As a depolymerization method, a depolymerization method in which a powdered high-polymerization cellulose ether is brought into contact with an acid such as hydrogen chloride and heated is widely used. As an apparatus for depolymerizing high-polymerization cellulose ether, as described in Patent Documents 1 and 2, a batch reactor such as a conical mixer is generally used in which the reactor itself rotates.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 08-301901

[0007] Patent Document 2: Japanese Patent Application No. 2020-531599 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] However, the methods described in Patent Documents 1 and 2 require a large batch reactor when attempting to industrially mass-produce low-polymerization-degree cellulose ether. This has the disadvantage of increasing the reactor installation space and investment cost.

[0010] In addition, when low-polymerization degree cellulose ether is produced using a batch reactor on an industrial scale, there is a problem that the adhesion of cellulose ether powder to the inside of the device increases over time as the number of production increases. When the adhesion of cellulose ether powder to the device increases, there are problems such as deterioration of heat transfer characteristics from the jacket of the reactor to the cellulose ether powder, instability of the viscosity of the low-polymerization degree cellulose ether obtained in each batch, and poor discharge of the low-polymerization degree cellulose ether from the reactor. In addition, there is a problem that black foreign matter is generated when the attached cellulose ether powder is peeled off from the device, and mixed into the product, thereby damaging the commercial value of the low-polymerization degree cellulose ether.

[0011] In order to remove the adhesion of the cellulose ether powder, when a low-polymerization-degree cellulose ether is produced industrially using a batch reactor, it is necessary to frequently perform a cleaning operation of the reactor between batches.

[0012] It is thought that if a continuous reactor is used instead of a batch reactor, the reactor can be miniaturized, thereby reducing the reactor installation space and investment cost, and producing low-polymerization-degree cellulose ether efficiently on an industrial scale. However, in a continuous reactor, since the reactor cannot be cleaned between batches as in a batch reactor, it is difficult to remove cellulose ether powder once it adheres. In addition, since it is difficult to prevent adhesion, it is not possible to produce low-polymerization-degree cellulose ether continuously.

[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for continuously producing depolymerized cellulose ether, which method can save space and has high productivity, and can reduce adhesion of cellulose ether powder to a reactor, and can obtain depolymerized cellulose ether with suppressed yellowness and generation of foreign matter.

[0014] Solutions for solving problems

[0015] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that by adjusting the temperature of the raw material cellulose ether supplied from the raw material tank to the humidity control tank to less than 40° C. and providing a humidity control step in which the supplied raw material cellulose ether is brought into contact with water vapor, adhesion of cellulose ether powder to the reactor can be reduced, and depolymerized cellulose ether with suppressed yellowness and foreign matter generation can be continuously produced, thereby completing the present invention.

[0016] That is, the present invention provides the following method for continuously producing depolymerized cellulose ether.

[0017] [1]. A method for continuously producing depolymerized cellulose ether, characterized in that:

[0018] The method at least comprises the following steps:

[0019] a) a humidity conditioning step, wherein the raw material cellulose ether continuously supplied from the raw material tank to the humidity conditioning tank is contacted with water vapor to obtain the humidity-conditioned cellulose ether;

[0020] b) a temperature raising step of heating the humidity-controlled cellulose ether continuously supplied from the humidity controlling step to obtain the temperature-raised cellulose ether;

[0021] c) a depolymerization step of continuously contacting gaseous hydrogen chloride with the heated cellulose ether to depolymerize the cellulose ether, thereby obtaining a depolymerized cellulose ether product; and

[0022] d) a neutralization step of mixing the depolymerized cellulose ether product with a basic compound to neutralize the product to obtain the depolymerized cellulose ether,

[0023] Furthermore, the temperature of the raw material cellulose ether continuously supplied from the raw material tank to the humidity control tank is 3°C or higher and lower than 40°C.

[0024] [2] The method for continuously producing depolymerized cellulose ether as described in [1], wherein:

[0025] The method comprises a washing step between the depolymerization step and the neutralization step, wherein hydrogen chloride and water are removed from the depolymerized cellulose ether product continuously supplied from the depolymerization step to obtain a washed depolymerized cellulose ether product.

[0026] [3] The method for continuously producing depolymerized cellulose ether according to [1] or [2], wherein:

[0027] The ratio of the supply rate of the humidity-controlled cellulose ether from the humidity-control step to the temperature-raising step to the discharge rate of the depolymerized cellulose ether product discharged from the depolymerization step is in the range of 0.9 to 1.1.

[0028] [4] The method for continuously producing depolymerized cellulose ether according to any one of [1] to [3], wherein

[0029] The method comprises a cooling step after the neutralization step, wherein the depolymerized cellulose ether is cooled.

[0030] [5] The method for continuously producing depolymerized cellulose ether according to any one of [1] to [4], wherein

[0031] The temperature of the humidity-controlled cellulose ether continuously supplied from the humidity-control step to the temperature-raising step is 50°C to 90°C.

[0032] [6] The method for continuously producing depolymerized cellulose ether according to any one of [1] to [5], wherein

[0033] In the humidity control step, the jacket temperature of the humidity control tank is 20°C to 120°C.

[0034] [7] The method for continuously producing depolymerized cellulose ether according to any one of [1] to [6], wherein

[0035] The raw material cellulose ether is at least one selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose and hydroxyalkyl alkyl cellulose.

[0036] The depolymerized cellulose ether also includes a low-polymerization-degree cellulose ether having a lower degree of polymerization than the cellulose ether before depolymerization and used for film coating of solid preparations such as tablets.

[0037] Effects of the Invention

[0038] According to the present invention, a low-polymerization-degree cellulose ether with suppressed yellowness and reduced generation of foreign matter can be produced by a space-saving and highly productive continuous production method. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a diagram showing an example of a production system used in the production method of the present invention.

[0040] Figure 2 It is a diagram showing another example of the production system used in the production method of the present invention. DETAILED DESCRIPTION

[0041] Depolymerized cellulose ether can be produced by a space-saving and highly productive continuous production method, the continuous production method comprising at least the following steps: a humidity control step of bringing a raw material cellulose ether continuously supplied from a raw material tank into contact with water vapor to obtain humidity-controlled cellulose ether; a temperature raising step of heating the humidity-controlled cellulose ether continuously supplied from the humidity control step to obtain temperature-raised cellulose ether; a depolymerization step of bringing gaseous hydrogen chloride into contact with the temperature-raised cellulose ether to depolymerize it and obtain a depolymerized cellulose ether product; and a neutralization step of neutralizing the depolymerized cellulose ether product by mixing it with an alkaline compound to obtain the depolymerized cellulose ether, wherein the temperature of the raw material cellulose ether continuously supplied from the raw material tank into the humidity control tank is 3° C. or higher and lower than 40° C.

[0042] The continuous method for producing depolymerized cellulose ether is described. In the following description, the term "continuous method" means a method in which powder is continuously supplied from the previous process to the next process during production, and is distinguished from an intermittent method in which the supply and discharge of raw materials (powder) to each process are discontinuous.

[0043] In addition, the devices used in each step are connected by piping. Preferably, rotary valves are provided at the powder supply port and discharge port of the device used in each step to quantitatively supply and discharge the powder.

[0044] First, the raw material cellulose ether will be described. Examples of the raw material cellulose ether include cellulose ethers having a high degree of polymerization, such as hydroxyalkyl alkyl cellulose, alkyl cellulose, and hydroxyalkyl cellulose.

[0045] Examples of the hydroxyalkyl alkyl cellulose include hydroxypropyl methylcellulose (hereinafter also referred to as "HPMC"), in which the hydroxypropoxy group is preferably 4.0 to 13.0% by mass and the methoxy group is preferably 19.0 to 32.0% by mass; hydroxyethyl methylcellulose, in which the hydroxyethoxy group is preferably 4.0 to 15.0% by mass and the methoxy group is preferably 20.0 to 26.0% by mass; and hydroxyethyl ethyl cellulose, in which the hydroxyethoxy group is preferably 8.0 to 20.0% by mass and the ethoxy group is preferably 20.0 to 38.0% by mass.

[0046] Examples of the alkyl cellulose include methyl cellulose (hereinafter also referred to as "MC") having a methoxy group content of preferably 18.0 to 36.0% by mass, and ethyl cellulose having an ethoxy group content of preferably 40.0 to 50.0% by mass.

[0047] Examples of the hydroxyalkyl cellulose include hydroxyethyl cellulose having a hydroxyethoxy group content of preferably 2.0 to 70.0% by mass, and hydroxypropyl cellulose having a hydroxypropoxy group content of preferably 2.0 to 70.0% by mass.

[0048] The contents of alkoxy groups and hydroxyalkoxy groups in alkyl cellulose, hydroxyalkyl cellulose and hydroxyalkyl alkyl cellulose can be determined according to the analytical method for hypromellose in the 18th revised edition of the Japanese Pharmacopoeia.

[0049] From the viewpoint of the cleansing properties of the raw material cellulose ether, the viscosity of a 2 mass % aqueous solution of the raw material cellulose ether at 20° C. is preferably 400 to 200,000 mPa·s, more preferably 400 to 150,000 mPa·s, and even more preferably 400 to 100,000 mPa·s.

[0050] The viscosity of a 2% by mass aqueous solution of the raw material cellulose ether at 20° C. can be measured using a single cylinder type rotational viscometer in accordance with the rotational viscometer method of the viscosity measurement method of the general test methods described in the 18th revised edition of the Japanese Pharmacopoeia, when the viscosity is 600 mPa·s or more. On the other hand, when the viscosity is lower than 600 mPa·s, it can be measured using an Ubbelohde viscometer in accordance with the capillary viscometer method of the viscosity measurement method of the general test methods described in the 18th revised edition of the Japanese Pharmacopoeia, when the viscosity is lower than 600 mPa·s.

[0051] The raw material cellulose ether can be produced by a known method.

[0052] For example, it can be obtained by a production method comprising at least the following steps: a step of bringing an alkali metal hydroxide solution into contact with pulp to obtain alkali cellulose; a step of reacting the alkali cellulose with an etherifying agent to obtain a cellulose ether product; a step of washing and drying the cellulose ether product; and a step of pulverizing as required.

[0053] The alkali metal hydroxide solution is not particularly limited, but an alkali metal hydroxide aqueous solution is preferred from an economical viewpoint.

[0054] The alkali metal hydroxide aqueous solution is not particularly limited, but a sodium hydroxide aqueous solution is preferred from an economical viewpoint.

[0055] The etherifying agent is not particularly limited, and examples thereof include alkyl halides such as methyl chloride and ethyl chloride; and alkyl oxides such as ethylene oxide and propylene oxide.

[0056] Then, the cellulose ether product is washed, dried, and pulverized as necessary to produce the raw material cellulose ether.

[0057] From the viewpoint of preventing the raw material cellulose ether from agglomerating, the water content of the raw material cellulose ether is preferably greater than 0% by mass and 2.00% by mass or less, and more preferably 0.1 to 1.50% by mass.

[0058] The moisture content is defined as {(total mass of cellulose ether-absolute dry mass of cellulose ether) / (total mass of cellulose ether)}×100%.

[0059] Here, the "total mass of cellulose ether" refers to the mass of the raw material cellulose ether before drying when accurately weighed according to the "loss on drying test method" of the 18th revised edition of the Japanese Pharmacopoeia. In addition, the "absolute dry mass of cellulose ether" refers to the mass of the raw material cellulose ether after drying according to the "loss on drying test method" of the 18th revised edition of the Japanese Pharmacopoeia.

[0060] The temperature (product temperature) of the raw material cellulose ether is 3°C or higher and lower than 40°C, preferably 5°C to 38°C, more preferably 7°C to 35°C, and even more preferably 10°C to 30°C. If the temperature (product temperature) of the raw material cellulose ether is 40°C or higher, cellulose ether powder may adhere to the device in the humidity control step and the temperature increase step. If the temperature (product temperature) of the raw material cellulose ether is lower than 3°C, the temperature increase in the temperature increase step may be large, resulting in an increase in the size of the device and a large amount of energy consumption.

[0061] There are no particular limitations on the method for adjusting the temperature of the raw material cellulose ether. Examples thereof include a method in which the temperature of the raw material cellulose ether is adjusted by adding cellulose ether to a jacketed container and flowing a fluid such as water through the jacket to adjust the jacket temperature; a method in which the cellulose ether is added to a jacketed screw conveyor and the jacket temperature is adjusted to continuously adjust the temperature of the raw material cellulose ether while conveying the raw material cellulose ether; a method in which air or nitrogen at a specified temperature is passed into the cellulose ether to adjust the temperature of the raw material cellulose ether; and the like.

[0062] The temperature of the raw material cellulose ether can be measured by a thermometer provided in the raw material tank or in a pipe for conveying the raw material cellulose ether from the raw material tank to the humidity control step.

[0063] a) Humidity Control Process

[0064] Next, the humidity control step will be described.

[0065] In the humidity control step, the raw material cellulose ether is brought into contact with water vapor in a humidity control tank, thereby obtaining the humidity controlled cellulose ether. A continuous humidity control tank is used as the humidity control tank, and the humidity control tank has at least one supply port and at least one discharge port. The supply port of the humidity control tank is connected to the discharge port of the raw material tank having the raw material cellulose ether through a pipe, and the discharge port of the humidity control tank is connected to the supply port of the temperature increasing device described later through a pipe. In addition, the humidity control tank has a water vapor supply port.

[0066] As a continuous humidity-conditioning tank, a vertical high-speed stirring mixer, a horizontal mixer, and a continuous mixing mixer can be cited. As a vertical high-speed stirring mixer, an axial mixer (manufactured by Sugiyama Heavy Industries, Japan) can be cited. As a horizontal mixer, a Pam Apex mixer WA type (manufactured by Ohira Machinery Co., Ltd., Japan) can be cited. As a continuous mixing mixer, a flexible mixer (manufactured by Hosokawa Micron) and a Tabular (manufactured by Hosokawa Micron) can be cited.

[0067] In the humidity control tank, the raw material cellulose ether is stirred while being brought into contact with water vapor. Here, the water vapor refers to saturated water vapor and superheated water vapor. Saturated water vapor refers to gaseous water existing in equilibrium with liquid water, and superheated water vapor refers to gaseous water existing at a temperature higher than the boiling point of water under a specified pressure condition.

[0068] From the viewpoint of efficiently adjusting the humidity of the raw material cellulose ether, it is preferred to use saturated steam.

[0069] The temperature of the water vapor is preferably 100° C. to 150° C. from the viewpoint of efficiently controlling the humidity of the raw material cellulose ether and the quality of the obtained depolymerized cellulose ether.

[0070] From the viewpoint of preventing the adhesion of cellulose ether powder to the apparatus and the viewpoint of the quality of the obtained depolymerized cellulose ether, the ratio of the amount of water vapor supplied to the humidity controlling tank in the humidity controlling step to the amount of the raw material cellulose ether supplied ([amount of water vapor supplied] / [amount of raw material cellulose ether supplied]) is preferably 0.02 to 0.1, more preferably 0.025 to 0.08, and most preferably 0.027 to 0.05 in terms of weight ratio.

[0071] From the viewpoint of preventing the internal pressure of the humidity control tank from rising and condensation, it is preferred to install a bag filter in the humidity control tank to discharge the remaining water vapor not absorbed by the raw material cellulose ether to the outside of the humidity control tank. For the purpose of discharging the remaining water vapor to the outside of the humidity control tank, an inert gas such as nitrogen may be flowed into the humidity control tank.

[0072] The inert gas such as nitrogen may be mixed with water vapor in advance and supplied to the humidity controlling tank as a mixture of water vapor and inert gas, or may be supplied into the humidity controlling tank from a supply port different from that for water vapor.

[0073] From the viewpoint of preventing the cellulose ether powder from adhering to the humidity control tank and the temperature increasing device described later, the jacket temperature of the humidity control tank is preferably 20° C. to 120° C., more preferably 30° C. to 100° C., and even more preferably 35° C. to 85° C. The jacket temperature of the humidity control tank can be controlled by adjusting the temperature of the fluid flowing in the jacket of the humidity control tank.

[0074] In order to mix the raw material cellulose ether and water vapor, the humidity control tank may have either a main shaft or a chopper or both. From the viewpoint of fully mixing the raw material cellulose ether and water vapor, the rotation speed of the main shaft is preferably 10 rpm to 1000 rpm; from the viewpoint of fully mixing the raw material cellulose ether and water vapor, the rotation speed of the chopper is preferably 10 rpm to 5000 rpm.

[0075] From the viewpoint of preventing the adhesion of cellulose ether powder to the device after the temperature raising step and the viewpoint of the quality of the obtained depolymerized cellulose ether, the temperature of the humidity-controlled cellulose ether at the outlet of the humidity-controlled tank is preferably 30 to 100° C., more preferably 50 to 90° C. In the present specification, the “temperature of the humidity-controlled cellulose ether” refers to the temperature of the humidity-controlled cellulose ether at the outlet of the humidity-controlled tank.

[0076] From the viewpoint of preventing the adhesion of cellulose ether powder to the device after the temperature raising step and the viewpoint of the quality of the obtained depolymerized cellulose ether, the moisture content of the humidity-conditioned cellulose ether at the outlet of the humidity-conditioning tank is preferably 1.5 to 6% by mass, more preferably 2.0 to 4.0% by mass. It should be noted that in this specification, the "moisture content of the humidity-conditioned cellulose ether" refers to the moisture content of the humidity-conditioned cellulose ether at the outlet of the humidity-conditioning tank.

[0077] b) Heating process

[0078] Next, the temperature raising step will be described.

[0079] In the temperature raising step, the humidity-controlled cellulose ether is raised in a temperature raising device to obtain the temperature-raised cellulose ether.

[0080] The temperature raising process is performed using a continuous temperature raising device having at least one supply port and at least one discharge port. The supply port of the temperature raising device is connected to the discharge port of the humidity control tank via a pipe, and the discharge port of the temperature raising device is connected to the supply port of the depolymerization device described later via a pipe.

[0081] Examples of the continuous temperature-raising device include a jacketed screw conveyor and a jacketed continuous mixer.

[0082] From the viewpoint of preventing the cellulose ether powder from adhering to the temperature increasing device, the jacket temperature of the temperature increasing device is preferably 20° C. to 120° C. The jacket temperature of the temperature increasing device can be controlled by adjusting the temperature of the fluid flowing through the jacket of the temperature increasing device.

[0083] From the viewpoint of controlling the viscosity of the obtained depolymerized cellulose ether and preventing the adhesion of cellulose ether powder to the device, the temperature of the heated cellulose ether at the discharge outlet of the heating device is preferably 55 to 90° C., more preferably 60 to 88° C., and even more preferably 63 to 85° C. In the present specification, the “temperature of the heated cellulose ether” refers to the temperature of the heated cellulose ether at the discharge outlet of the heating device.

[0084] From the viewpoint of preventing the cellulose ether powder from adhering to the device after the depolymerization step and from the viewpoint of the quality of the depolymerized cellulose ether obtained, the water content of the heated cellulose ether at the outlet of the heating vessel is preferably 1.5 to 6% by mass, more preferably 2.0 to 4.0% by mass. It should be noted that in the present specification, the "water content of the heated cellulose ether" refers to the water content of the heated cellulose ether at the outlet of the heating device.

[0085] c) Depolymerization process

[0086] Next, the depolymerization step will be described.

[0087] In the depolymerization step, the cellulose ether is continuously contacted with gaseous hydrogen chloride (hydrogen chloride gas) in a continuous depolymerization device to depolymerize the cellulose ether, thereby obtaining a depolymerized cellulose ether product. The depolymerization device has at least one supply port and at least one discharge port. The supply port of the depolymerization device is connected to the discharge port of the temperature-elevating device through a pipe, and the discharge port of the depolymerization device is connected to the supply port of the neutralization tank or the cleaning device described later through a pipe.

[0088] As continuous depolymerization apparatus, there can be mentioned a vertical high-speed stirring mixer, a horizontal mixer, a continuous mixing mixer, and a jacketed screw conveyor. As a vertical high-speed stirring mixer, there can be mentioned an axial mixer (manufactured by Sugiyama Heavy Industries, Ltd., Japan), etc. As a horizontal mixer, there can be mentioned a Pam Apex mixer WA type (manufactured by Ohira Machinery Co., Ltd., Japan), etc. As a continuous mixing mixer, there can be mentioned a flexible mixer (manufactured by Hosokawa Micron), Tabular (manufactured by Hosokawa Micron), etc.

[0089] In the depolymerization step, from the viewpoint of uniformly performing depolymerization, it is preferred to use two or more continuous depolymerization apparatuses selected from the above-mentioned continuous depolymerization apparatuses in combination.

[0090] For example, when two continuous depolymerization devices are used in combination, if the depolymerization device connected to the temperature raising device is used as the first depolymerization device, and the depolymerization device connected to the first depolymerization device is used as the second depolymerization device, the supply port of the first depolymerization device is connected to the discharge port of the temperature raising device through a pipe, the discharge port of the first depolymerization device is connected to the supply port of the second depolymerization device through a pipe, and the discharge port of the second depolymerization device is connected to the supply port of the neutralization tank or the cleaning device described later through a pipe. In addition, the supply port of the hydrogen chloride gas (hydrogen chloride gas) is preferably provided in the first depolymerization device, but it is not limited thereto. The same is true when the number of depolymerization devices is increased to three or more.

[0091] More preferably, one selected from a vertical high-speed stirring mixer, a horizontal mixer and a continuous mixing mixer is used as the first depolymerization device, and a jacketed screw conveyor is used in combination in this order as the second depolymerization device.

[0092] From the viewpoint of controlling the viscosity of the obtained depolymerized cellulose ether, the jacket temperature of the depolymerization device is preferably 20 to 120° C., more preferably 30 to 90° C., and even more preferably 50 to 85° C. The jacket temperature of the depolymerization device can be controlled by adjusting the temperature of the fluid flowing through the jacket of the depolymerization device.

[0093] From the viewpoint of preventing the hydrogen chloride gas from leaking out of the depolymerization device, the internal pressure of the depolymerization device is preferably -40 to 0 kPaG.

[0094] In order to fully mix the heated cellulose ether and the hydrogen chloride gas, the depolymerization device may have either a main shaft or a chopper or both. From the viewpoint of fully mixing the heated cellulose ether and the hydrogen chloride gas, the rotation speed of the main shaft is preferably 10 rpm to 1000 rpm. From the viewpoint of fully mixing the heated cellulose ether and the hydrogen chloride gas, the rotation speed of the chopper is preferably 10 rpm to 5000 rpm.

[0095] From the viewpoint of preventing the cellulose ether from adhering to the equipment and enabling continuous production, and from the viewpoint of suppressing the generation of black foreign matter in the product, the acid to be brought into contact with the heated cellulose ether is preferably gaseous hydrogen chloride.

[0096] From the viewpoint of controlling the viscosity of the obtained depolymerized cellulose ether, the ratio of the amount of hydrogen chloride supplied in gas to the amount of cellulose ether supplied at elevated temperature ([amount of hydrogen chloride supplied in gas] / [amount of cellulose ether supplied at elevated temperature]) is preferably 0.0001 to 0.01, more preferably 0.001 to 0.008 in terms of weight ratio.

[0097] The product temperature of the depolymerized cellulose ether in the depolymerization step is preferably 55 to 90°C, more preferably 60 to 88°C, and even more preferably 63 to 85°C from the viewpoint of controlling the viscosity of the obtained depolymerized cellulose ether.

[0098] The depolymerization time in the depolymerization step is not particularly limited as long as the depolymerized cellulose ether reaches a desired viscosity, but from the viewpoint of obtaining a depolymerized cellulose ether with low yellowness, the depolymerization time is preferably 0.1 to 4.0 hours, more preferably 0.2 to 2.0 hours. Here, the depolymerization time refers to the time from when the heated cellulose ether is supplied to the depolymerization device to when the depolymerized cellulose ether product is discharged from the depolymerization device. When two or more depolymerization devices are used in combination in the depolymerization step, the total of the depolymerization times in the depolymerization devices is taken as the depolymerization time in the depolymerization step. The depolymerization time can be obtained by dividing the retention amount (kg) of the cellulose ether powder in the depolymerization device in terms of anhydrous cellulose ether by the discharge rate (kg / hr) of the depolymerized cellulose ether product at the discharge port of the depolymerization device in terms of anhydrous cellulose ether.

[0099] From the viewpoint of continuously producing the depolymerized cellulose ether in a stable state, the ratio of the supply rate of the humidity-conditioned cellulose ether from the humidity-conditioning step to the temperature-raising step to the discharge rate of the depolymerized cellulose ether product from the depolymerization step ([supply rate of the humidity-conditioned cellulose ether from the humidity-conditioning step to the temperature-raising step] / [discharge rate of the depolymerized cellulose ether product from the depolymerization step]) is 0.9 to 1.1, preferably 0.95 to 1.05, and more preferably 0.98 to 1.02.

[0100] After the depolymerization step, in order to reduce the residual amount of hydrogen chloride in the depolymerized cellulose ether product, a washing step may be further included in which hydrogen chloride is removed from the depolymerized cellulose ether product under reduced pressure to obtain a washed depolymerized cellulose ether product. In the washing step, hydrogen chloride (hydrogen chloride gas or hydrochloric acid aqueous solution) and water (water vapor or liquid) can be removed from the depolymerized cellulose ether product.

[0101] The cleaning process can be performed using a cleaning device. Since the previous and subsequent processes (depolymerization process and neutralization process) are continuous, the cleaning device is preferably continuous. The continuous cleaning device has at least one supply port and at least one discharge port. The supply port of the cleaning device is connected to the discharge port of the depolymerization device through a pipe, and the discharge port of the cleaning device is connected to the supply port of the neutralization tank described later through a pipe. In addition, the cleaning device has a discharge port that can discharge hydrogen chloride and water to the outside of the system through the cleaning process.

[0102] As continuous cleaning devices, there can be mentioned a jacketed screw conveyor, a jacketed continuous mixer, a continuous vibration vacuum dryer (manufactured by Chuo Kakoki, Japan), a belt vacuum dryer (manufactured by Nisaka Seisakusho, Japan), etc. As a jacketed continuous mixer, there can be mentioned the same mixer as the humidity control tank.

[0103] From the viewpoint of efficiently removing hydrogen chloride from the depolymerized cellulose ether product, the internal pressure of the cleaning apparatus in the cleaning step is preferably -99 to -60 kPaG.

[0104] From the viewpoint of efficiently removing hydrogen chloride from the depolymerized cellulose ether product, the jacket temperature of the cleaning apparatus in the cleaning step is preferably 20 to 120°C.

[0105] d) Neutralization process

[0106] Next, the neutralization step will be described.

[0107] In the neutralization step, a basic compound and a depolymerized cellulose ether product are mixed in a neutralization tank to obtain depolymerized cellulose ether.

[0108] As the neutralization tank, a continuous mixer similar to the humidity control tank can be used, and the neutralization tank has at least one supply port and at least one discharge port. The supply port of the neutralization tank is connected to the discharge port of the depolymerization device or the cleaning device through a pipe, and the discharge port of the neutralization tank is connected to the supply port of the product tank or the cooling device described later through a pipe. In addition, the neutralization tank has a supply port for the alkaline compound.

[0109] In order to mix the depolymerized cellulose ether product and the alkaline compound, the neutralization tank may have either a main shaft or a chopper or both. From the viewpoint of sufficiently mixing the depolymerized cellulose ether product and the alkaline compound, the rotation speed of the main shaft is preferably 10 rpm to 1000 rpm. From the viewpoint of sufficiently mixing the depolymerized cellulose ether product and the alkaline compound, the rotation speed of the chopper is preferably 10 rpm to 5000 rpm.

[0110] From the viewpoint of efficiently performing neutralization, the jacket temperature of the neutralization tank is preferably 30°C to 120°C.

[0111] Examples of the basic compound include weakly basic compounds such as sodium hydrogen carbonate and sodium carbonate.

[0112] The amount of the basic compound added is not particularly limited as long as the acid is neutralized, but the ratio of the amount of the basic compound supplied to the amount of the depolymerized cellulose ether product supplied ([amount of the basic compound supplied] / [amount of the depolymerized cellulose ether product supplied]) is preferably 0.001 to 0.01 in terms of weight ratio.

[0113] From the viewpoint of efficiently performing neutralization, the temperature of the depolymerized cellulose ether at the outlet of the neutralization tank is preferably 30 to 100°C, more preferably 40 to 90°C, and even more preferably 50 to 85°C.

[0114] After the neutralization step, a cooling step of cooling the depolymerized cellulose ether may be further included. By providing the cooling step, the temperature of the depolymerized cellulose ether supplied to the product tank is reduced, and condensation in the product tank and foreign matter caused by condensation entering the product or corrosion of the product tank can be prevented.

[0115] The cooling process can be carried out in a continuous cooling device. As the cooling device, the same device as the temperature raising device and the depolymerization device can be used. By making the jacket temperature of the cooling device lower than the temperature of the depolymerized cellulose ether, the depolymerized cellulose ether can be cooled. The cooling device has at least one supply port and at least one discharge port. The supply port of the cooling device is connected to the discharge port of the neutralization tank through a pipe, and the discharge port of the cooling device is connected to the supply port of the product tank described later through a pipe.

[0116] From the viewpoint of efficiently cooling the depolymerized cellulose ether, the jacket temperature of the cooling device is preferably 5°C to 60°C.

[0117] The product temperature of the depolymerized cellulose ether at the outlet of the cooling device is preferably 20°C to 70°C from the viewpoint of preventing condensation in the product tank and foreign matter from being mixed into the product due to condensation or corrosion of the product tank.

[0118] The depolymerized cellulose ether can be dried, crushed and sieved with a sieve of any mesh size as required. There is no particular limitation on the apparatus for drying, crushing and sieving, but a continuous apparatus is preferred.

[0119] From the viewpoint of obtaining depolymerized cellulose ether with low yellowness, the viscosity reduction rate of the depolymerized cellulose ether is preferably 40.0 to 99.99%, more preferably 50.0 to 99.99%, and even more preferably 60.0 to 99.99% relative to the raw material cellulose ether.

[0120] Here, the viscosity reduction rate refers to the ratio of the difference between the viscosity of a 2 mass % aqueous solution of the raw material cellulose ether at 20°C (viscosity before depolymerization) and the viscosity of a 2 mass % aqueous solution of the depolymerized cellulose ether at 20°C (viscosity after depolymerization) to (viscosity before depolymerization), and is defined as {(viscosity before depolymerization - viscosity after depolymerization) / viscosity before depolymerization}×100.

[0121] From the viewpoint of maintaining a low solution viscosity during film coating, the viscosity of a 2 mass % aqueous solution of the depolymerized cellulose ether at 20° C. is preferably 1.0 to 20.0 mPa·s, more preferably 2.0 to 20.0 mPa·s, and even more preferably 3.0 to 15.0 mPa·s. The viscosity of a 2 mass % aqueous solution of the depolymerized cellulose ether at 20° C. is a value measured by the same method as the viscosity of a 2 mass % aqueous solution of the raw material cellulose ether at 20° C.

[0122] [Example]

[0123] Hereinafter, the present invention will be described in detail by way of Examples and Comparative Examples, but the present invention is not limited to these Examples at all.

[0124] In addition, the yellowness was measured, the amount of black foreign matter was evaluated, and the #100 pass rate was evaluated by the following methods.

[0125] <Determination of yellowness>

[0126] A 2 mass % aqueous solution of depolymerized cellulose ether at 20° C. was prepared, and the yellowness was measured using an SM color computer (trade name “SM-4”, manufactured by Suga Test Instruments Co., Ltd.).

[0127] <Evaluation of the amount of black foreign matter generated>

[0128] 200 g of depolymerized cellulose ether was supplied to a sieve having a first layer of 18 mesh (effective sieve area of ​​0.0314 m 2After using a rotary hammer (Ro-Tap) type vibrating sieve machine (manufactured by Takeda Rika Kogyo Co., Ltd., Japan) with a mesh size of 0.85 mm, ...

[0129] <#100pass rate evaluation>

[0130] 200 g of depolymerized cellulose ether was supplied to a sieve having a 100-mesh sieve (effective sieve area of ​​0.0314 m 2 After using a rotary hammer type vibrating sieve machine (manufactured by Takeda Rika Kogyo Co., Ltd., Japan) with a mesh size of 0.15 mm, ...

[0131] A schematic diagram of a production system 10 used in the continuous production method of depolymerized cellulose ether of the present invention is shown in Figure 1 .exist Figure 1 In the manufacturing system 10 shown, the discharge outlet of the raw material tank 1 is connected to the supply port of the humidity control tank 2 through a pipe, the discharge outlet of the humidity control tank 2 is connected to the supply port of the temperature increasing device 3 through a pipe, the discharge outlet of the temperature increasing device 3 is connected to the supply port of the depolymerization device 4 through a pipe, the discharge outlet of the depolymerization device 4 is connected to the supply port of the neutralization tank 6 through a pipe, and the discharge outlet of the neutralization tank 6 is connected to the supply port of the product tank 8 through a pipe.

[0132] The raw material tank 1 has a supply port for the raw material cellulose ether A, the humidity control tank 2 has a supply port for water vapor B, the depolymerization device 4 has a supply port for gaseous hydrogen chloride (hydrogen chloride gas) C, and the neutralization tank 6 has a supply port for the basic compound E.

[0133] Example 1

[0134] will be with Figure 1A schematic diagram of a production system 20 used in the continuous production method of depolymerized cellulose ether of the present invention is shown in FIG. Figure 2 .

[0135] In the following examples, using Figure 2 The manufacturing system shown. Figure 2 In the manufacturing system 20 shown, the discharge outlet of the raw material tank 1 is connected to the supply port of the humidity control tank 2 through a pipe, the discharge outlet of the humidity control tank 2 is connected to the supply port of the temperature increasing device 3 through a pipe, the discharge outlet of the temperature increasing device 3 is connected to the supply port of the depolymerization device (1) 41 through a pipe, the discharge outlet of the depolymerization device (1) 41 is connected to the supply port of the depolymerization device (2) 42 through a pipe, the discharge outlet of the depolymerization device (2) 42 is connected to the supply port of the cleaning device 5 through a pipe, the discharge outlet of the cleaning device 5 is connected to the supply port of the neutralization tank 6 through a pipe, the discharge outlet of the neutralization tank 6 is connected to the supply port of the cooling device 7 through a pipe, and the discharge outlet of the cooling device 7 is connected to the supply port of the product tank 8 through a pipe.

[0136] In addition, the raw material tank 1 has a supply port for the raw material cellulose ether A, the humidity control tank 2 has a supply port for water vapor B, the depolymerization device (1) 41 has a supply port for gaseous hydrogen chloride (hydrogen chloride gas) C, the cleaning device 5 has a discharge port for hydrogen chloride and water D, and the neutralization tank 6 has a supply port for the alkaline compound E.

[0137] Each device is described.

[0138] (1) Humidity Control Tank

[0139] The humidity control tank used was a device with an effective volume of 50L and a jacketed vertical high-speed stirring mixer with a main shaft and a chopper. A supply port with a rotary valve was provided on the top plate of the humidity control tank, and the raw material cellulose ether could be continuously supplied at a certain speed. A discharge port with a rotary valve was provided on the wall surface of the humidity control tank, and the humidity-controlled cellulose ether in the tank could be continuously discharged at a certain speed. In addition, a bag filter was provided on the top plate.

[0140] (2) Heating device

[0141] The temperature increasing device used was a temperature increasing device having a jacketed screw conveyor having a screw diameter of 120 mm, a shaft diameter of 80 mm, a screw length of 5 m, and a pitch of 100 mm.

[0142] (3) Depolymerization device (1)

[0143] The depolymerization device (1) used was a device having an effective volume of 50 L and equipped with a jacketed vertical high-speed stirring mixer having a main shaft and a chopper. A supply port with a rotary valve was provided on the top plate of the depolymerization device (1) to continuously supply the heated cellulose ether at a constant speed. A discharge port with a rotary valve was provided on the wall surface of the depolymerization device (1) to continuously discharge the depolymerized cellulose ether in the tank at a constant speed.

[0144] (4) Depolymerization device (2)

[0145] The depolymerization device used was a depolymerization device having a jacketed screw conveyor having a screw diameter of 120 mm, a shaft diameter of 80 mm, a screw length of 100 m, and a pitch of 100 mm.

[0146] (5) Cleaning device

[0147] The cleaning device used was a cleaning device having a jacketed screw conveyor having a screw diameter of 120 mm, a shaft diameter of 80 mm, a screw length of 40 m, and a pitch of 100 mm.

[0148] (6) Neutralization tank

[0149] The neutralization tank used was a device with an effective volume of 50 L and equipped with a jacketed vertical high-speed stirring mixer having a main shaft and a chopper. A supply port with a rotary valve was provided on the top plate of the neutralization tank, and the depolymerized cellulose ether product could be continuously supplied at a constant speed. In addition, a discharge port with a rotary valve was provided on the wall surface of the neutralization tank, and the depolymerized cellulose ether in the tank could be continuously discharged at a constant speed.

[0150] (7) Cooling device

[0151] The cooling device used was a cooling device having a jacketed screw conveyor having a screw diameter of 120 mm, a shaft diameter of 80 mm, a screw length of 5 m, and a pitch of 100 mm.

[0152] Low-polymerization-degree cellulose ether was continuously produced under the following operating conditions.

[0153] (i) Humidity Control Process

[0154] The raw material cellulose ether (29.0% by mass of methoxyl group, 9.1% by mass of hydroxypropoxyl group, 1000 mPa·s viscosity of 2% by mass aqueous solution, and 0.5% by mass of HPMC) at 20° C. was continuously supplied from the raw material tank to the humidity control tank at a rate of 180 kg / hr converted to anhydrous cellulose ether. The humidity control tank was operated under the conditions of a main shaft speed of 250 rpm, a chopper speed of 1000 rpm, and a jacket temperature of 80° C. In addition, nitrogen was supplied to the humidity control tank.

[0155] Water vapor at 110° C. was continuously supplied from the water vapor supply port of the humidity control tank to the powder layer of the raw material cellulose ether at a supply rate of 0.040 in weight ratio to the supply rate of the raw material cellulose ether, so as to contact the raw material cellulose ether, thereby obtaining humidity-controlled cellulose ether. While the raw material cellulose ether was continuously supplied, the humidity-controlled cellulose ether was continuously discharged from the discharge port of the humidity control tank at a rate of 180 kg / hr in terms of anhydrous cellulose ether. The humidity-controlled cellulose ether discharged from the humidity control tank had a product temperature of 70° C. and a water content of 2.9% by mass.

[0156] The apparatus used as the humidity controlling tank, the jacket temperature of the humidity controlling tank, the form of water, the amount of water supplied relative to the amount of raw material cellulose ether supplied (water supply amount / raw material cellulose ether supply amount), the temperature of the raw material cellulose ether, the temperature of the humidity-controlled cellulose ether, and the water content of the humidity-controlled cellulose ether are shown in Table 1 a) in the humidity controlling step.

[0157] (ii) Heating process

[0158] The humidity-adjusted cellulose ether was continuously supplied to the temperature-elevating device at a rate of 180 kg / hr in terms of anhydrous cellulose ether. Hot water at 90° C. was circulated in the jacket of the temperature-elevating device. The screw of the temperature-elevating device was rotated at a rate of 20 rpm. The temperature-elevated cellulose ether was discharged from the outlet of the temperature-elevating device at a rate of 180 kg / hr in terms of anhydrous cellulose ether. The product temperature of the temperature-elevated cellulose ether when discharged from the temperature-elevating device was 80° C. and the water content was 2.8% by mass.

[0159] The temperature increasing device, the jacket temperature of the temperature increasing device, the temperature of the humidity-controlled cellulose ether, the temperature of the temperature-increasing cellulose ether, and the water content of the temperature-increasing cellulose ether are shown in Table 1 in b) the temperature increasing step.

[0160] (iii) Depolymerization process

[0161] The above-mentioned heated cellulose ether was continuously supplied to the depolymerization device (1) at a rate of 180 kg / hr in terms of anhydrous cellulose ether. The depolymerization device (1) was operated under the conditions of a main shaft speed of 250 rpm, a chopper speed of 1000 rpm, a jacket temperature of 80°C, and an internal pressure of -30 kPaG. Hydrogen chloride gas was continuously supplied from the hydrogen chloride supply port of the depolymerization device (1) to the powder layer of the heated cellulose ether at a supply rate of 0.0040 in weight ratio to the supply rate of the heated cellulose ether, so as to contact the heated cellulose ether. While the heated cellulose ether was continuously supplied, the depolymerized cellulose ether product was continuously supplied from the discharge port of the depolymerization device (1) to the depolymerization device (2).

[0162] The jacket temperature of the depolymerization device (2) was 80°C and the internal pressure was -5 kPaG. The screw of the depolymerization device (2) was rotated at 20 rpm.

[0163] The depolymerization time of the depolymerized cellulose ether product in the depolymerization device (1) was 0.1 hour, and the depolymerization time of the depolymerized cellulose ether product in the depolymerization device (2) was 1 hour, and the total depolymerization time was 1.1 hours. The depolymerized cellulose ether product was continuously discharged from the discharge port of the depolymerization device (2) at a flow rate of 180 kg / hr in terms of anhydrous cellulose ether. The temperature of the depolymerized cellulose ether product was 80° C.

[0164] (iv) Cleaning process

[0165] The depolymerized cellulose ether product was continuously supplied to the cleaning device at a rate of 180 kg / hr in terms of anhydrous cellulose ether. The jacket temperature of the cleaning device was 80° C. The screw of the cleaning device rotated at 20 rpm. In addition, the pressure in the cleaning device was maintained at -98 kPaG by a vacuum pump, and hydrogen chloride gas, water vapor and a portion of the hydrochloric acid aqueous solution were removed from the hydrogen chloride and water outlets of the cleaning device. The depolymerized cellulose ether product was continuously discharged from the outlet of the cleaning device at a flow rate of 180 kg / hr in terms of anhydrous cellulose ether.

[0166] (V) Neutralization process

[0167] The washed depolymerized cellulose ether product was continuously supplied to the neutralization tank at a rate of 180 kg / hr in terms of anhydrous cellulose ether. The neutralization tank was operated under the conditions of a main shaft speed of 250 rpm, a chopper speed of 1000 rpm, and a jacket temperature of 80°C. Sodium bicarbonate powder was continuously supplied from the supply port of the alkaline compound of the neutralization tank at a supply rate of 0.0040 in weight ratio to the supply rate of the depolymerized cellulose ether product, and mixed with the cellulose ether product to obtain depolymerized cellulose ether. While the depolymerized cellulose ether product was continuously supplied, the depolymerized cellulose ether was continuously discharged directly from the discharge port of the neutralization device at a flow rate of 180 kg / hr in terms of anhydrous cellulose ether. The temperature of the depolymerized cellulose ether when discharged from the neutralization tank was 80°C.

[0168] (Vi) Cooling process

[0169] The depolymerized cellulose ether was continuously supplied to the cooling device at a rate of 180 kg / hr in terms of anhydrous cellulose ether. Water at 10° C. was circulated in the jacket of the cooling device. The screw of the cooling device was rotated at 20 rpm. The depolymerized cellulose ether was continuously discharged from the discharge port of the cooling device to the product tank at a flow rate of 180 kg / hr in terms of anhydrous cellulose ether. It should be noted that the temperature of the depolymerized cellulose ether when discharged from the cooling device was 30° C.

[0170] Under the above conditions, depolymerized cellulose ether was produced continuously for 24 hours, and a total of 4320 kg of depolymerized cellulose ether was produced in terms of anhydrous cellulose ether. The depolymerized cellulose ether was sampled from the product tank and analyzed.

[0171] After the production was continued for 24 hours, the humidity control tank and the temperature raising device were visually checked to confirm the occurrence of adhesion and the like.

[0172] The viscosity of a 2 mass % aqueous solution of each of the obtained depolymerized cellulose ethers at 20° C. was measured by the above-mentioned method, and the viscosity reduction rate was calculated from the value of the viscosity of the raw material cellulose ether.

[0173] In addition, the yellowness of the obtained depolymerized cellulose ether was measured, the amount of black foreign matter was evaluated, and the #100 pass rate was calculated by the above-mentioned methods.

[0174] The results are shown in Tables 2 and 3.

[0175] Example 2

[0176] Depolymerized cellulose ether was produced in the same manner as in Example 1 except that the jacket temperature of the humidity control tank was 25° C. and the jacket temperature of the temperature increasing device was 100° C. in the temperature increasing step.

[0177] Comparative Example 1

[0178] Depolymerized cellulose ether was produced in the same manner as in Example 1 except that the jacket temperature of the raw material tank was set to 100° C., the temperature of the raw material cellulose ether in the raw material tank was adjusted, the temperature of the raw material cellulose ether supplied to the humidity control step was set to 80° C., and the temperature of the heated cellulose ether was set to 80° C., which was the same as those in Examples 1 and 2. The results are shown in Tables 2 and 3.

[0179] Comparative Example 2

[0180] The same method as in Example 1 was attempted to produce depolymerized cellulose ether, except that the jacket temperature of the raw material tank was set to 100°C, the temperature of the raw material cellulose ether in the raw material tank was adjusted, the temperature of the raw material cellulose ether supplied to the humidity control step was set to 80°C, and 110°C water vapor was supplied to the raw material cellulose ether at a supply rate of 0.150 in weight ratio to the supply rate of the raw material cellulose ether. However, a large amount of adhesion occurred at the discharge port of the humidity control tank, etc., and clogging occurred, so that continuous operation could not be performed, and further the steps after the temperature raising step could not be performed. The results are shown in Tables 2 and 3.

[0181] Comparative Example 3

[0182] Depolymerized cellulose ether was produced in the same manner as in Example 1 except that the jacket temperature of the humidity control tank was 25°C, liquid water at 20°C was brought into contact with the raw material cellulose ether in place of water vapor in the humidity control step, and the jacket temperature of the temperature raising device was set to 130°C in the temperature raising step so that the temperature of the raised cellulose ether was 80°C, which was the same as those in Examples 1 and 2. The results are shown in Tables 2 and 3.

[0183] [Table 1]

[0184]

[0185] [Table 2]

[0186]

[0187] ○: No adhesion observed A: No adhesion observed

[0188] △: Adhesion occurred B: Adhesion occurred

[0189] ×: A large amount of adhesion occurred. C: Due to a large amount of adhesion and clogging, continuous operation could not be performed.

[0191] [Table 3]

[0192]

[0193] In Examples 1 and 2, in which the temperature of the raw material cellulose ether supplied to the humidity control tank was 20°C, the cellulose ether powder did not significantly adhere to the equipment in the humidity control step and the temperature increase step, and the depolymerized cellulose ether could be continuously produced. In addition, the yellowness of the obtained depolymerized cellulose ether was low, and no black foreign matter was generated. In particular, in Example 1, in which the jacket temperature of the humidity control tank was 80°C, the cellulose ether powder did not adhere to the equipment in either the humidity control step or the temperature increase step.

[0194] In Comparative Example 1, in which the temperature of the raw material cellulose ether supplied to the humidity-controlling tank was 80° C., the moisture content of the humidity-controlled cellulose ether decreased even when the same amount of water vapor as in Example 1 was supplied, and as a result, the yellowness of the obtained depolymerized cellulose ether increased. In Comparative Example 2, in which the amount of water vapor supplied was increased in the humidity-controlling step, although the moisture content of the humidity-controlled cellulose ether increased, the powder of the cellulose ether in the humidity-controlling tank adhered significantly, and clogging occurred at the discharge port of the humidity-controlling tank, resulting in an unstable discharge amount of the humidity-controlled cellulose ether, and the depolymerized cellulose ether could not be produced continuously.

[0195] In Comparative Example 3, in which liquid water at 20° C. was used in the humidity control step, adhesion occurred on the humidity control tank and the temperature raising device. In addition, the amount of black foreign matter in the obtained depolymerized cellulose ether increased, which impaired the product value. In addition, the amount of aggregates increased, resulting in a decrease in the #100 pass rate and a decrease in the yield.

[0196] Description of Reference Numerals

[0197] 10.20- Manufacturing System

[0198] 1-Raw material tank

[0199] 2-Humidity conditioning tank

[0200] 3- Heating device

[0201] 4-Depolymerization device

[0202] 41-Depolymerization device (1)

[0203] 42-Depolymerization device (2)

[0204] 5-Cleaning device

[0205] 6-Neutralization tank

[0206] 7-Cooling device

[0207] 8-Product tank

[0208] A-Raw material cellulose ether

[0209] B-Water vapor

[0210] C-Hydrogen chloride gas

[0211] D-hydrogen chloride and water

[0212] E-Basic compounds

[0213] F-depolymerized cellulose ether

Claims

1. A method for continuously producing depolymerized cellulose ether, characterized in that: The method at least comprises the following steps: a) a humidity conditioning step, wherein the raw material cellulose ether continuously supplied from the raw material tank to the humidity conditioning tank is contacted with water vapor to obtain the humidity-conditioned cellulose ether; b) a temperature raising step of heating the humidity-controlled cellulose ether continuously supplied from the humidity-controlling step to obtain the temperature-raised cellulose ether; c) a depolymerization step of continuously contacting gaseous hydrogen chloride with the heated cellulose ether to depolymerize the cellulose ether, thereby obtaining a depolymerized cellulose ether product; as well as d) a neutralization step of mixing the depolymerized cellulose ether product with a basic compound to neutralize the product to obtain the depolymerized cellulose ether, Furthermore, the temperature of the raw material cellulose ether continuously supplied from the raw material tank to the humidity control tank is 3°C or higher and lower than 40°C.

2. The method for continuously producing depolymerized cellulose ether according to claim 1, wherein: The method comprises a washing step between the depolymerization step and the neutralization step, wherein hydrogen chloride and water are removed from the depolymerized cellulose ether product continuously supplied from the depolymerization step to obtain a washed depolymerized cellulose ether product.

3. The method for continuously producing depolymerized cellulose ether according to claim 1, wherein: The ratio of the supply rate of the humidity-controlled cellulose ether from the humidity-control step to the temperature-raising step to the discharge rate of the depolymerized cellulose ether product discharged from the depolymerization step is in the range of 0.9 to 1.

1.

4. The method for continuously producing depolymerized cellulose ether according to claim 1, wherein: The method comprises a cooling step after the neutralization step, wherein the depolymerized cellulose ether is cooled.

5. The method for continuously producing depolymerized cellulose ether according to claim 1, wherein: The temperature of the humidity-controlled cellulose ether continuously supplied from the humidity-control step to the temperature-raising step is 50°C to 90°C.

6. The method for continuously producing depolymerized cellulose ether according to claim 1, wherein: In the humidity control step, the jacket temperature of the humidity control tank is 20°C to 120°C.

7. The method for continuously producing depolymerized cellulose ether according to any one of claims 1 to 6, wherein The raw material cellulose ether is at least one selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose and hydroxyalkyl alkyl cellulose.

Citation Information

Patent Citations

  • Production of cellulose ether low in degree of polymerization

    JP1996301901A

  • Controlled preparation of low molecular weight cellulose ethers

    JP2020531599A