Leaky coaxial cable capable of reducing smoke density and manufacturing method thereof
By using specific materials and processes in coaxial cables, the mechanical strength and flame retardant properties are enhanced, the performance degradation problem of cables in extreme environments is solved, and environmental pollution is reduced, achieving higher safety and environmental protection.
Patent Information
- Application Number
- CN202411078299.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-01
AI Technical Summary
The performance of existing coaxial cables degrades in extreme environments and lacks high mechanical durability, environmental adaptability, safety and environmental protection. In particular, aging is accelerated under high temperature and UV conditions, and traditional cable combustion produces a large amount of smoke and toxic gases, which increases Fire hazard and environmental pollution.
Using thermoplastic polymers, flame retardants, antimony trioxide, nanoscale titanium oxide, nanoscale silica, modified epoxy resin and multi-functional additives, through high-speed mixing, twin-screw extrusion and curing processes, the cable's performance is enhanced. mechanical strength, thermal stability and flame retardant properties, and use bio-based polymers and low-smoke halogen-free materials to reduce environmental impact.
Significantly improves the mechanical strength and durability of the cable, enhances resistance to high temperatures and UV, reduces the generation of fire smoke and toxic gases, reduces environmental pollution, and complies with environmental protection and safety standards.
Smart Images

Figure CN118725441A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cable equipment, in particular to a leaky coaxial cable capable of reducing smoke density and a manufacturing method thereof. Background Art
[0002] Coaxial cable is a cable used to transmit high-frequency signals. Due to its unique structural design, it has good anti-interference performance. Its basic structure includes inner conductor, insulation layer, outer conductor and outer sheath. The inner conductor is located in the center of the cable and is usually made of copper or silver-plated copper. It is used to transmit electrical signals. Wrapped around the inner conductor is the insulation layer, which is usually made of polyethylene or polytetrafluoroethylene to isolate the inner conductor and the outer conductor. The outer conductor is located outside the insulation layer and is usually composed of a woven copper mesh or aluminum foil to shield electromagnetic interference. Due to the coaxial structure of the coaxial cable, it has low loss, high bandwidth and good anti-interference ability when transmitting signals. It is widely used in television signal transmission, Internet access, telephone networks and other fields that require high-frequency signal transmission.
[0003] However, the existing coaxial cable materials are ordinary polyethylene or polyvinyl chloride. Although they have certain mechanical strength and can withstand physical stress such as stretching, bending and wear, they may still degrade in performance under extreme environments such as high mechanical loads or wear conditions, which limits their use in certain industrial applications. Secondly, the environmental tolerance of existing cables, especially the demand for thermal stability and UV resistance, becomes increasingly important as the complexity of the application environment increases. In high temperature environments or when exposed to sunlight for a long time, cable materials may age faster, resulting in performance degradation, which is particularly significant in outdoor or high temperature applications. In addition, the safety of cables, especially in terms of fire resistance, is an important consideration in the existing technology. In the event of a fire, cables need to have good flame retardant properties to reduce the spread of fire. However, many traditional cables may produce a lot of smoke and toxic gases when burning, which not only increases the risk of fire, but also poses a threat to escape and rescue operations. Finally, with the increasing awareness of environmental protection, the challenges facing existing cable technology also include how to reduce the environmental impact during production and use. The production of traditional cables usually involves the use of a large amount of chemicals, which may cause long-term pollution to the environment after the cable life cycle ends. Therefore, while ensuring high performance, existing cable technology also needs to address its shortcomings in durability, environmental adaptability, safety and environmental protection. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention provides a leaky coaxial cable with reduced smoke density and a manufacturing method thereof, which solves the problem of poor wear resistance of the equipment.
[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: a leaky coaxial cable for reducing smoke density, comprising the following component materials: 70 to 80 parts of a thermoplastic polymer, 5 to 10 parts of a flame retardant, 1 to 3 parts of antimony trioxide, 1 to 3 parts of nano-scale titanium oxide, 1 to 3 parts of nano-scale silicon dioxide, 2 to 5 parts of a modified epoxy resin, and 0.5 to 2 parts of a multifunctional additive.
[0006] Preferably, the thermoplastic polymer includes polyethylene, polypropylene and polyvinyl chloride, and the addition ratio of polyethylene, polypropylene and polyvinyl chloride is 5:2:3.
[0007] Preferably, the flame retardant includes aluminum hydroxide and magnesium hydroxide, and the addition ratio of the aluminum hydroxide and magnesium hydroxide is 1:1.5. The modified epoxy resin includes basic epoxy resin and nano-siloxane, and the addition ratio of the epoxy resin and nano-siloxane is 9:5.
[0008] Preferably, the multifunctional additives include antioxidants, ultraviolet absorbers, and antistatic agents, and the addition ratio of the antioxidants, ultraviolet absorbers, and antistatic agents is 5:3:2; the antistatic agents include benzophenones, benzotriazoles, and organic nickel compounds, and the addition ratio of the benzophenones, benzotriazoles, and organic nickel compounds is 7:7:6.
[0009] Preferably, the antioxidant includes benzotriazoles and phosphates, and the addition ratio of the benzotriazoles and phosphates is 3:2; the ultraviolet absorber includes benzophenones and benzotriazoles, and the addition ratio of the benzophenones and benzotriazoles is 1:1.
[0010] A method for manufacturing a leaky coaxial cable with reduced smoke density comprises the following steps: S1. Material preparation: prepare thermoplastic polymer, flame retardant, antimony trioxide, nano-sized titanium oxide, nano-sized silicon dioxide, modified epoxy resin, and multifunctional additives; S2. Material mixing: premix the thermoplastic polymer, flame retardant, antimony trioxide, nano-sized titanium oxide, nano-sized silicon dioxide, modified epoxy resin and multifunctional additive in a high-speed mixer in a specified proportion to ensure uniform distribution; S3, secondary mixing: antioxidant, ultraviolet absorber, antistatic agent and specific benzophenone, benzotriazole and organic nickel compound are accurately metered into a high-speed mixer according to a specified ratio, and all additives are further mixed and dispersed to form a uniform mixture A; S4, curing and molding: melt-extrude the mixture A through a twin-screw extruder to obtain a cable conductor, then put the cable conductor into a curing furnace for heating and curing, and then put the cured cable conductor into a cooling device for cooling and fixing the shape; S5. Post-processing: Use a polishing machine to polish and grind the cooled cable conductor, and then use a coating machine to coat the polished cable conductor with an antistatic agent.
[0011] Preferably, in the step S2, the speed of the high-speed mixer is 524 rpm to 986 rpm, and the temperature of the high-speed mixer is 27° C. to 40° C.
[0012] Preferably, in step S3, the speed of the high-speed mixer is 1120 rpm to 1000 rpm, and the temperature of the high-speed mixer is 32° C. to 49° C.
[0013] Preferably, in the step S2, the temperature of the twin-screw extruder is set to 164°C to 215°C, the speed of the twin-screw extruder is set to 55rpm to 147rpm, the temperature of the curing furnace is set to 184°C to 249°C, and the curing time of the curing furnace is 2h to 3h.
[0014] Preferably, in the step S5, the rotation speed of the polishing machine is set to 200 rpm to 500 rpm, and the coating speed of the coating machine is set to 14 m / min to 20 m / min.
[0015] The present invention provides a leaky coaxial cable with reduced smoke density and a manufacturing method thereof. The cable has the following beneficial effects: 1. The present invention significantly enhances the mechanical strength and durability of the cable by adding modified epoxy resin and nano-scale filler to the cable material. This improvement makes the cable stronger and able to withstand greater physical pressure and wear, thereby extending its service life, and is particularly suitable for high wear and high stress environments.
[0016] 2. The environmental adaptability of the cable is significantly improved by introducing specific UV resistors and heat stabilizer additives. These additives enable the cable to withstand more severe environmental conditions, such as strong sunlight exposure and high temperature, while maintaining its performance unaffected.
[0017] 3. The flame retardant properties of the cable of the present invention are enhanced by adding flame retardants such as aluminum hydroxide and magnesium hydroxide. These materials can release moisture at high temperatures to inhibit the spread of flames. In addition, the amount of smoke and toxic gases generated by the cable when it burns is also greatly reduced, providing higher safety protection in the event of a fire, and is suitable for use in closed or crowded environments.
[0018] 4. The bio-based polymers and low-smoke halogen-free materials used in the cable manufacturing of the present invention reduce the impact on the environment and support the goal of sustainable development. These materials release fewer harmful substances during production and waste treatment and are easier to recycle and handle, which is in line with global environmental trends and regulatory requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0020] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Example 1: Basic Leaky Coaxial Cable to Reduce Smoke Density Overview of steps: S1. Material preparation: 70 parts of polyethylene, 8 parts of flame retardant, 1 part of antimony trioxide, 1 part of nano-sized titanium oxide, 1 part of nano-sized silicon dioxide, 2 parts of modified epoxy resin, and 0.5 parts of multifunctional additive; S2, mixing: Mix all materials in a high-speed mixer at 524 rpm and 30° C. for 20 minutes; S3, extrusion: extrusion by a twin-screw extruder at 190°C and 100 rpm; S4, curing: curing in a curing oven at 200°C for 2 hours; S5, post-processing: polishing machine speed 300rpm, coating speed 17m / min.
[0022] Summary: This basic cable is suitable for general environments and can achieve consistent quality and performance through standard proportions and mild handling conditions.
[0023] Example 2: High heat-resistant leaky coaxial cable Overview of steps: S1. Material adjustment: Use 75 parts of polypropylene, add 3 parts of nano-grade titanium oxide, and mix the remaining materials according to the basic ratio; S2, mixing: the mixer was set to 986 rpm and the temperature was maintained at 40°C; S3, extrusion: the extrusion temperature is increased to 215°C and the speed is adjusted to 55 rpm; S4, curing: the curing temperature is increased to 249°C and the curing time is extended to 3 hours; S5, post-processing: polishing machine speed 500rpm to increase surface smoothness.
[0024] Summary: Suitable for high temperature environments, enhanced titanium oxide provides better UV protection and thermal stability.
[0025] Embodiment 3: Leaky coaxial cable with enhanced mechanical strength Overview of steps: S1. Material adjustment: 80 parts of polyvinyl chloride, increase nano-silicon dioxide to 3 parts; S2, mixing: mixing speed 1120 rpm, temperature 49 ° C; S3, extrusion: extrusion temperature 190 ° C, rotation speed 147 rpm; S4, curing: curing temperature 240 ° C, curing time 3 hours; S5, post-treatment: coating speed increased to 20m / min.
[0026] Summary: This cable has higher abrasion resistance and tear resistance, suitable for environments with harsh physical conditions.
[0027] Example 4: Environmentally friendly leaky coaxial cable Overview of steps: S1. Material selection: Use bio-based polymers as the main material; S2. Processing conditions: reduce mixing and extrusion temperatures to reduce energy consumption; S3. Post-processing: Use environmentally friendly materials for surface treatment.
[0028] Summary: The production of this cable is more environmentally friendly and reduces the impact on the environment.
[0029] Example 5: Ultra-high durability leaky coaxial cable Overview of steps: S1. Material strengthening: the dosage of all additives reaches the upper limit; S2, mixing: the speed and temperature of the high-speed mixer are set to the highest value; S3, extrusion and curing: use the most stringent temperature and time control; S4, Post-treatment: Add additional protective coating to ensure long-term durability.
[0030] Summary: Suitable for long-term exposure to harsh environments, with extremely high physical and chemical stability.
[0031] Summary: These five examples show how to adapt to various application requirements by adjusting material ratios, processing conditions and using different materials. Each cable has unique performance characteristics to ensure optimal performance in its specific application environment. Through these diverse implementation schemes, it can be clearly seen that the cable technology is very flexible and adaptable to meet the changing needs of the market.
[0032] 1. Mechanical strength test Testing process: A. Use a universal material testing machine; B. Fix the cable sample in the fixture of the testing machine to ensure that the sample is straight and without distortion; C. Slowly increase the tensile force until the sample breaks; D. Record the maximum tensile force and elongation at break.
[0033] Data table: Example Maximum pulling force (N) Elongation (%) Basic 350 15 High heat resistance type 300 12 Enhanced mechanical strength 400 18 Environmentally friendly 320 14 Ultra-high durability 450 20 Summary: Mechanical strength test results show that ultra-high durability cables have the highest tensile force and elongation, and are suitable for use in environments that need to withstand greater mechanical stress. Enhanced mechanical strength types also perform well and are suitable for applications with higher physical requirements. Basic and environmentally friendly cables have moderate mechanical properties and are suitable for general applications. Although high heat-resistant cables have excellent heat resistance, they are slightly inferior in mechanical strength and are recommended for use in environments with higher temperatures but lower mechanical loads.
[0034] 2. Thermal stability test Testing process: A. Cut the cable sample into specified length and put it into the oven; B. Set the oven to run for a certain period of time at different temperatures (from 100°C to the maximum operating temperature); C. Take out samples regularly, check physical changes and weigh them to calculate mass loss.
[0035] Data table: Example Test temperature (°C) weightlessness(%) Basic 200 0.5 High heat resistance type 250 0.2 Enhanced mechanical strength 220 0.7 Environmentally friendly 210 0.3 Ultra-high durability 250 0.1 Summary: High heat resistant and ultra-high durability cables performed best in thermal stability tests, especially the ultra-high durability type, which had almost no quality loss and was very suitable for high temperature environments. Basic and environmentally friendly cables performed moderately and were suitable for general environmental conditions. Although the enhanced mechanical strength type had slightly poor thermal stability, it still maintained acceptable performance and was suitable for environments where the temperature was not overly extreme.
[0036] 3.UV resistance test Testing process: A. Place the sample in a UV light box to simulate long-term sunlight exposure; B. Check the color and physical state changes of the samples at regular intervals.
[0037] Data table: Example UV exposure time (hours) Change level Basic 500 slight High heat resistance type 500 No change Enhanced mechanical strength 500 slight Environmentally friendly 500 obvious Ultra-high durability 500 No change Summary: High heat resistant and ultra-high durability cables show excellent UV resistance with almost no visible changes, which are very suitable for applications exposed to sunlight for a long time. Basic and enhanced mechanical strength types perform well and are suitable for general outdoor applications. Environmentally friendly cables perform slightly worse in this test and may require additional protection measures to prevent UV-induced aging.
[0038] 4. Wear resistance test Testing process: A. Use a wear tester to wear the sample for a specified period of time; B. Weigh the samples before and after abrasion to calculate the mass loss.
[0039] Data table: Example Wear cycle Abrasion resistance (% weight loss) Basic 1000 0.2 High heat resistance type 1000 0.5 Enhanced mechanical strength 1000 0.1 Environmentally friendly 1000 0.3 Ultra-high durability 1000 0.05 Summary: The enhanced mechanical strength cable performed best in the abrasion resistance test, and the minimal mass loss shows that it is suitable for high-wear environments. The ultra-high durability type also showed good abrasion resistance and is suitable for long-term use. The basic type and high heat-resistant type cables provide average abrasion resistance, while the environmentally friendly type cable is slightly lacking in abrasion resistance.
[0040] 5. Flame retardant performance test Testing process: A. Hang the cable sample vertically on the test frame; B. Use a standard flame to ignite the bottom of the sample and extinguish it after a certain period of time; C. Observe the burning conditions and self-extinguishing time of the sample.
[0041] Data Analysis: Example Burning time (seconds) Burning length (cm) Self-extinguishing time (seconds) Basic 30 15 5 High heat resistance type 30 10 3 Enhanced mechanical strength 30 8 2 Environmentally friendly 30 12 4 Ultra-high durability 30 5 1 Summary: Ultra-high durability cables showed the best performance in the flame retardant performance test, with the shortest burning length and the fastest self-extinguishing time, which is very suitable for environments that require high fire protection standards. Enhanced mechanical strength and high heat resistance cables also showed good flame retardant performance and are suitable for environments where there may be fire risks. Although the flame retardant performance of basic and environmentally friendly cables is lower, it is still within the safety standard range.
[0042] Summary: The cables in these five examples demonstrate that through scientific material selection and manufacturing processes, the performance and safety of cables can be significantly improved to meet the needs of different environments and applications. Through comprehensive testing and evaluation, the characteristics and applicable scenarios of each cable are clearly defined, providing valuable data and insights for the development and optimization of future products.
[0043] Comparative experiment 1: Mechanical properties test Existing technical solutions: Traditional coaxial cables usually use ordinary PVC or PE materials as insulation layers and sheaths.
[0044] The solution of the present invention: modified epoxy resin and nano-scale additives (titanium oxide, silicon dioxide) are used to enhance the mechanical properties of the cable.
[0045] Testing process: 1. Use a universal material testing machine to perform tensile and compression tests; 2. Record the breaking strength, elongation and compression strength.
[0046] Data Records: Parameters / cable type Breaking strength (N) Elongation (%) Prior art 300 10 The present invention 400 18 Summary: In mechanical performance tests, the leaky coaxial cable of the present invention exhibits significantly better breaking strength and elongation than the prior art. By adding modified epoxy resin and nano-scale additives, the mechanical toughness and durability of the cable are enhanced. This allows the cable to have higher reliability and longer service life in applications that require high mechanical stress, such as industrial or extreme environments.
[0047] Comparative experiment 2: Environmental tolerance test Prior art solution: Ordinary cables are not subjected to special UV protection or heat resistance treatment.
[0048] The solution of the present invention: UV resist (benzophenone and benzotriazole) and heat stabilizer (nano oxide) are incorporated into the cable.
[0049] Testing process: 1. Heat and UV expose the cable in a simulated environment; 2. Determine the changes in physical and chemical properties of materials at different temperatures and after UV exposure.
[0050] Data Records: Parameters / cable type Thermal stability (% weight loss) UV resistance (color change level) Prior art 0.7 obvious The present invention 0.1 slight Summary: The leaky coaxial cable of the present invention also performs well in thermal stability and UV resistance. The addition of nano-oxides effectively improves the thermal stability of the material, while the use of UV resistors slows down the aging effect of ultraviolet rays on the material. These characteristics make the cable particularly suitable for outdoor or high temperature environments and can maintain performance for a longer period of time without degradation.
[0051] Comparative experiment three: environmental performance test Existing technical solution: conventional polymers are used without adding any special environmentally friendly materials.
[0052] The solution of the present invention: Use bio-based polymers and low-smoke halogen-free materials to reduce environmental impact.
[0053] Testing process: 1. Evaluate the recyclability of cable materials and the hazardous substances released during incineration; 2. Test the biodegradation rate of cable materials.
[0054] Data Records: Parameters / cable type Recyclability (%) Hazardous substance release (ppm) Prior art 70 50 The present invention 90 10 Summary: Compared with traditional cables, the present invention has made significant progress in environmental performance. The use of bio-based polymers and low-smoke halogen-free materials not only improves the recyclability of cables, but also significantly reduces the release of harmful substances during production and disposal. These improvements support the goals of green building and sustainable development and contribute to environmental protection.
[0055] Summary: These three comparative experiments fully demonstrate the obvious advantages of the cables of the present invention over the existing technologies in terms of mechanical properties, environmental tolerance and environmental friendliness. Through scientific material selection and innovative manufacturing processes, the present invention not only provides high-performance cable solutions, but also shows a deep consideration of environmental impacts. The high durability, excellent environmental adaptability and low environmental impact of these cables make them the first choice in a variety of application fields, especially for high-end markets that require high durability and environmental friendliness. In the long run, the promotion and application of this technology will help promote the entire cable industry to develop in a higher standard and greener direction.
[0056] The leaky coaxial cable of the present invention performs well in providing high performance and environmentally friendly solutions, not only meeting industrial standards and safety requirements, but also promoting the application of material innovation and environmental protection technology in the cable manufacturing industry. These characteristics and advantages make the present invention have an important competitive position in the future cable market.
[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A leaky coaxial cable for reducing smoke density, characterized in that: The composition comprises the following components: 70 to 80 parts of thermoplastic polymer, 5 to 10 parts of flame retardant, 1 to 3 parts of antimony trioxide, 1 to 3 parts of nano-sized titanium oxide, 1 to 3 parts of nano-sized silicon dioxide, 2 to 5 parts of modified epoxy resin and 0.5 to 2 parts of multifunctional additive.
2. A leaky coaxial cable for reducing smoke density according to claim 1, characterized in that: The thermoplastic polymer includes polyethylene, polypropylene and polyvinyl chloride, and the addition ratio of polyethylene, polypropylene and polyvinyl chloride is 5:2:
3.
3. A leaky coaxial cable for reducing smoke density according to claim 1, characterized in that: The flame retardant includes aluminum hydroxide and magnesium hydroxide, and the addition ratio of the aluminum hydroxide and magnesium hydroxide is 1:1.
5. The modified epoxy resin includes basic epoxy resin and nano-siloxane, and the addition ratio of the epoxy resin and nano-siloxane is 9:
5.
4. A leaky coaxial cable for reducing smoke density according to claim 1, characterized in that: The multifunctional additives include antioxidants, ultraviolet absorbers, and antistatic agents, and the addition ratio of the antioxidants, ultraviolet absorbers, and antistatic agents is 5:3:
2. The antistatic agents include benzophenones, benzotriazoles, and organic nickel compounds, and the addition ratio of the benzophenones, benzotriazoles, and organic nickel compounds is 7:7:
6.
5. A leaky coaxial cable for reducing smoke density according to claim 4, characterized in that: The antioxidants include benzotriazoles and phosphates, and the addition ratio of the benzotriazoles and phosphates is 3:
2. The ultraviolet absorbers include benzophenones and benzotriazoles, and the addition ratio of the benzophenones and benzotriazoles is 1:
1.
6. A method for manufacturing a leaky coaxial cable with reduced smoke density, used for manufacturing a leaky coaxial cable with reduced smoke density as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Material preparation: prepare thermoplastic polymer, flame retardant, antimony trioxide, nano-sized titanium oxide, nano-sized silicon dioxide, modified epoxy resin, and multifunctional additives; S2. Material mixing: premix the thermoplastic polymer, flame retardant, antimony trioxide, nano-sized titanium oxide, nano-sized silicon dioxide, modified epoxy resin and multifunctional additive in a high-speed mixer in a specified proportion to ensure uniform distribution; S3, secondary mixing: antioxidant, ultraviolet absorber, antistatic agent and specific benzophenone, benzotriazole and organic nickel compound are accurately metered into a high-speed mixer according to a specified ratio, and all additives are further mixed and dispersed to form a uniform mixture A; S4, curing and molding: melt-extrude the mixture A through a twin-screw extruder to obtain a cable conductor, then put the cable conductor into a curing furnace for heating and curing, and then put the cured cable conductor into a cooling device for cooling and fixing the shape; S5. Post-processing: Use a polishing machine to polish and grind the cooled cable conductor, and then use a coating machine to coat the polished cable conductor with an antistatic agent.
7. The method for manufacturing a leaky coaxial cable with reduced smoke density according to claim 6, characterized in that: In the step S2, the rotation speed of the high-speed mixer is 524 rpm to 986 rpm, and the temperature of the high-speed mixer is 27° C. to 40° C.
8. The method for manufacturing a leaky coaxial cable with reduced smoke density according to claim 6, characterized in that: In the step S3, the speed of the high-speed mixer is 1120 rpm to 1000 rpm, and the temperature of the high-speed mixer is 32° C. to 49° C.
9. The method for manufacturing a leaky coaxial cable with reduced smoke density according to claim 6, characterized in that: In the step S2, the temperature of the twin-screw extruder is set to 164° C. to 215° C., the speed of the twin-screw extruder is set to 55 rpm to 147 rpm, the temperature of the curing furnace is set to 184° C. to 249° C., and the curing time of the curing furnace is 2 h to 3 h.
10. The method for manufacturing a leaky coaxial cable with reduced smoke density according to claim 6, characterized in that: In the step S5, the polishing machine rotation speed is set to 200 rpm to 500 rpm, and the coating speed of the coating machine is set to 14 m / min to 20 m / min.