Rubber material as well as preparation method and application thereof
The rubber material is prepared by combining materials such as EPDM rubber and vinyl silicone, which solves the durability problem of vehicle exhaust pipes hanging under high temperature conditions, achieves higher heat resistance and fatigue resistance, and is suitable for vehicles The exhaust pipe is hung to extend the service life.
Patent Information
- Application Number
- CN202410899205.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
AI Technical Summary
Existing vehicle exhaust pipe hanging products have poor durability under high-temperature working conditions and are difficult to meet the needs for improving vehicle safety, comfort and operability.
The rubber material is prepared through a specific refining process using a combination of polymer modifications of EPDM rubber and alkenyl silica gel, olefin-based silane coupling agent, filler, plasticizer, zinc oxide and vulcanizing agent to improve its durability. High temperature and fatigue resistance.
It significantly improves the durability and fatigue resistance of rubber materials at high temperatures, and is suitable for vehicle exhaust pipe hanging, extending its service life and improving stability in high temperature environments.
Smart Images

Figure CN118725466A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of rubber materials, and in particular to a rubber material. The present invention also relates to a preparation method of the rubber material and application of the rubber material. Background Art
[0002] Rubber is a highly elastic polymer material with reversible deformation. It is elastic at room temperature and can produce large deformation under a small external force, and can return to its original shape after the external force is removed. Rubber is a completely amorphous polymer with a low glass transition temperature (Tg) and a large molecular weight of more than hundreds of thousands.
[0003] Rubber products have many application scenarios in vehicle manufacturing, such as vehicle sealing products, vehicle shock-absorbing rubber products, vehicle hoses, tires, etc. Among them, vehicle shock-absorbing rubber products play an important role in vehicles, especially when encountering potholes on the road, rubber springs can effectively absorb the impact and ensure the smooth driving of the vehicle. In addition, shock-absorbing rubber can also withstand the pressure borne by key vehicle components and extend their service life.
[0004] In recent years, in order to improve the safety, comfort and operability of vehicles, the variety and quantity of shock-absorbing rubber products for vehicles have continued to increase, such as suspension modules used in vehicle exhaust systems. The exhaust system is one of the important assemblies on modern vehicles, and plays a very important role in purifying exhaust emissions and absorbing engine exhaust excitation noise. Suspension, as a load-bearing and vibration-isolating component of the exhaust system, plays the role of suspending the exhaust system and effectively preventing the vehicle body from being excited by the exhaust system.
[0005] The basic performance requirements of the suspension are: reasonable dynamic and static stiffness, able to support the exhaust system while isolating it from vibration excitation; sufficient strength and service life in high temperature environments to ensure its reliability. The rubber material commonly used in existing vehicle exhaust pipe suspension products still has poor durability under high temperature working conditions. Summary of the invention
[0006] In view of this, the present invention provides a rubber material to improve the durability of the rubber under high temperature conditions.
[0007] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0008] A rubber material, wherein the raw materials for preparing the rubber material include the following components in parts by weight:
[0009] 50-70 parts of the polymer modified product of EPDM rubber and olefinic silica gel, 30-50 parts of the polymer modified product of EPDM rubber and olefinic silane coupling agent, 50-80 parts of filler, 45-55 parts of plasticizer, 4-6 parts of zinc oxide, and 4-6 parts of vulcanizer.
[0010] Furthermore, the weight ratio of EPDM rubber to alkenyl silica gel in the raw materials for preparing the polymer modified product of EPDM rubber and alkenyl silica gel is (80-90): (20-10).
[0011] Furthermore, the alkenyl silica gel includes at least one of methyl vinyl silica gel and methyl phenyl vinyl silica gel.
[0012] Furthermore, the weight ratio of ethylene propylene diene monomer rubber and olefin-based silane coupling agent in the raw materials for preparing the polymerized modified product of ethylene propylene diene monomer rubber and olefin-based silane coupling agent is (95-99.5): (0.5-5).
[0013] Furthermore, the olefin-based silane coupling agent includes at least one of vinyltriethoxysilane and vinyltrimethoxysilane.
[0014] Furthermore, the vulcanizing agent includes a peroxide vulcanizing agent or a sulfur vulcanizing agent.
[0015] The present invention further provides a method for preparing the above-mentioned rubber material, which comprises the following steps:
[0016] Mixing a polymer modified product of EPDM rubber and olefinic silica gel, a polymer modified product of EPDM rubber and olefinic silane coupling agent, a plasticizer and zinc oxide, and refining the mixture;
[0017] Add filler to the mixture and continue refining. When the temperature rises to 105-115℃, exhaust gas;
[0018] Continue to seal and refine, and when the temperature rises to 135-145°C, discharge the rubber to obtain the mixed rubber;
[0019] The rubber compound is mixed with a vulcanizing agent and refined to obtain the rubber material.
[0020] Furthermore, the method for preparing the polymerized modified product of EPDM rubber and olefinic silica gel comprises the following steps:
[0021] The temperature of the internal mixer is raised to 55-65°C, and EPDM rubber, the first initiator and vinyl silica gel are added to mix and then refined;
[0022] When the temperature rises to 105-110℃, exhaust;
[0023] The sealed refining is continued, the stirring speed is adjusted to 60 r / min, and the refining temperature is controlled to be maintained at 110-160° C. After the refining is completed, the polymer modified product of the EPDM rubber and the vinyl silica gel is obtained.
[0024] Furthermore, the preparation method of the polymer modified product of EPDM rubber and olefin-based silane coupling agent comprises the following steps:
[0025] The temperature of the internal mixer is raised to 55-65°C, and EPDM rubber, the second initiator and the olefin-based silane coupling agent are added and mixed for refining;
[0026] When the temperature rises to 105-110℃, exhaust;
[0027] The sealed refining is continued, the stirring speed is adjusted to 60 r / min, and the refining temperature is controlled to be maintained at 110-160° C. After the refining is completed, the polymer modified product of the EPDM rubber and the olefin-based silane coupling agent is obtained.
[0028] The present invention also proposes an application of the rubber material in preparing a vehicle exhaust pipe hanger.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] The rubber material prepared by the present invention has the advantages of high temperature resistance and fatigue resistance by mixing the polymer modified product of EPDM rubber and olefinic silica gel, and the polymer modified product of EPDM rubber and olefinic silane coupling agent, and adding filler, plasticizer, zinc oxide and vulcanizer. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0032] Figure 1 It is a schematic diagram of the dehydrogenation reaction route of EPDM rubber induced by free radicals in the preparation process of the polymer modified product of EPDM rubber and alkenyl silica gel according to the present invention;
[0033] Figure 2 It is a schematic diagram of the graft polymerization reaction route of EPDM rubber and alkenyl silica gel with free radicals in the process of preparing the polymer modified product of EPDM rubber and alkenyl silica gel of the present invention;
[0034] Figure 3 The present invention is a schematic diagram of a graft polymerization reaction route of ethylene propylene diene monomer rubber and olefin-based silane coupling agent in the process of preparing the polymer modified product of ethylene propylene diene monomer rubber and olefin-based silane coupling agent. DETAILED DESCRIPTION
[0035] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0036] The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are purchased from conventional biochemical reagent stores unless otherwise specified. In addition, except for special instructions in this example, the terms and processes involved in this example are understood according to the general knowledge and conventional methods in the prior art.
[0037] The present invention will be described in detail below with reference to embodiments.
[0038] The present embodiment relates to a rubber material. The raw materials for preparing the rubber material include the following components by weight: 50-70 parts of a polymer modified product of EPDM rubber and olefinic silica gel, 30-50 parts of a polymer modified product of EPDM rubber and olefinic silane coupling agent, 50-80 parts of a filler, 45-55 parts of a plasticizer, 4-6 parts of zinc oxide, and 4-6 parts of a vulcanizer.
[0039] In this embodiment, the rubber material prepared by mixing the polymer modified product of EPDM rubber and olefinic silica gel, and the polymer modified product of EPDM rubber and olefinic silane coupling agent, and adding fillers, plasticizers, zinc oxide and vulcanizers has the advantages of high temperature resistance and fatigue resistance.
[0040] Ethylene propylene diene monomer (EPDM) is a terpolymer of ethylene, propylene and non-conjugated dienes. Ethylene and propylene are the main comonomers, forming long-chain polymers through copolymerization, and non-conjugated dienes are used to introduce saturation and cross-linking properties. Its structural characteristics allow only one highly active double bond to participate in the copolymerization, while the other less active double bond remains on the copolymer molecular chain. The main chain of EPDM is composed of chemically stable saturated hydrocarbons, and only contains unsaturated double bonds in the side chains.
[0041] Due to the molecular structure of EPDM, EPDM can work for a long time in high temperature environment and can withstand temperatures up to 150℃ or above. It has excellent weather resistance, ozone resistance, heat resistance, acid and alkali resistance and other aging resistance. It can be used for a long time, or temporarily or intermittently between 120℃, 150℃ and 200℃. It can also maintain its softness in cold environment, which makes EPDM can be used in various extreme climate conditions. EPDM has good resistance to most chemicals and can work in corrosive media such as acids, alkalis and solvents. Especially under the long-term action of concentrated acid, the performance can still remain stable. It has good elasticity and softness, and can quickly restore its original shape after deformation. EPDM can withstand frequent use and mechanical stress, and has good wear and tear resistance. It also has excellent water vapor resistance. In superheated steam at 230℃, the appearance is basically unchanged after nearly 100 hours.
[0042] The polymerization monomers of the EPDM rubber of the present invention are preferably ENB and VNB types, and more preferably VNB type, which has higher reaction activity and the modified product has better heat resistance and durability.
[0043] The molecular structure of alkenyl silica gel is mainly composed of silicon-oxygen bonds (Si-O) to form its basic skeleton, and side chains such as methyl and vinyl are attached to the silicon atom. The basic skeleton of alkenyl silica gel is a long chain structure formed by alternating silicon atoms and oxygen atoms, that is, a repeating unit of...Si-O-Si-O... This structure gives silica gel excellent high temperature resistance and chemical stability. On the silicon atom, there are usually two different side chains: methyl and vinyl. The introduction of these side chains not only affects the physical and chemical properties of silica gel, but also provides it with specific functionality. Methyl, as a saturated hydrocarbon group, can enhance the hydrophobicity and oil resistance of silica gel; while vinyl gives silica gel a certain reactivity, which can form a three-dimensional network structure through cross-linking reaction, thereby improving the strength and stability of silica gel.
[0044] As a polymer material, vinyl silicone can be processed by various methods such as thermal cross-linking and UV curing, showing excellent processing flexibility. Vinyl silicone can maintain structural stability for a long time under high temperature environment, and will not produce reactions such as oxidative degradation. It has good resistance to most chemicals and can work in corrosive media such as acids, alkalis, and solvents.
[0045] The polymerized modified product of ethylene propylene diene rubber and ethylene propylene diene rubber is formed by polymerization of double bonds, and has very good high temperature resistance. The polymerized monomer of ethylene propylene diene rubber is preferably VNB type ethylene propylene diene rubber. Compared with ENB type ethylene propylene diene rubber, VNB type has higher activity and can form more cross-linked bonds, thus having higher heat resistance. The preferred weight ratio of ethylene propylene diene rubber and ethylene propylene diene silicone in the raw materials for preparing the polymerized modified product of ethylene propylene diene rubber and ethylene propylene diene silicone of the present invention is (80-90): (20-10). The ethylene propylene diene silicone preferably adopts at least one of methyl vinyl silicone and methyl phenyl vinyl silicone.
[0046] Olefin silane coupling agents are mainly composed of silanoxy and olefin groups. The silanoxy groups are easily hydrolyzed during the coupling process to generate silanol groups, which then form chemical bonds with the surface of inorganic substances. The olefin groups are highly active and can react chemically with organic materials. Due to the presence of silanoxy and olefin groups, olefin silane coupling agents have high reactivity and can react chemically with inorganic and organic substances at the same time to form stable chemical bonds.
[0047] The olefin-based silane coupling agent and ethylene propylene diene monomer rubber are polymerized through double bonds to form a polymer modified product of ethylene propylene diene monomer rubber and olefin-based silane coupling agent. During the mixing process, the hydrolyzable group undergoes a hydrolysis reaction with white carbon black to form a chemical bond between the polymer and white carbon black, so that the rubber material has very good fatigue durability. The preferred weight ratio of ethylene propylene diene monomer rubber and olefin-based silane coupling agent in the raw materials for preparing the polymer modified product of ethylene propylene diene monomer rubber and olefin-based silane coupling agent of the present invention is (95-99.5): (0.5-5). The olefin-based silane coupling agent includes at least one of vinyl triethoxysilane and vinyl trimethoxysilane.
[0048] Fillers can significantly improve the impact resistance, tensile strength, tear resistance and other strengths of vulcanized rubber, as well as the wear resistance and other properties. Carbon compounds, silicon-containing compounds, metal oxides, carbonates, sulfates and the like can be used. The filler of the present invention preferably includes at least one of carbon black and white carbon black, and more preferably uses carbon black-white carbon black dual-phase fillers, which can effectively improve the shock absorption and durability of rubber. It is more preferred to use general furnace carbon black and precipitated white carbon black, and carbon black is selected from grades such as N550, N660, and N774, with a dosage of 35-45 parts, and white carbon black is selected from grades with a nitrogen adsorption specific surface area of 100-230m 2 / g, 150-180m is preferred to balance the operating performance of the compound rubber and the fatigue durability of the product. 2 / g, the amount of white carbon black is 15-25 parts.
[0049] Plasticizer can reduce the force between rubber molecules, thereby reducing the glass transition temperature of rubber, making rubber plastic and fluid, facilitating molding operations such as calendering and extrusion, and can also improve certain physical and mechanical properties of vulcanized rubber, such as reducing hardness and tensile stress, giving higher elasticity and lower heat generation, and improving cold resistance. The plasticizer of the present invention can be selected from cycloalkane oil and paraffin oil, such as paraffin oil, and stearic acid can also be added, wherein the amount of paraffin oil is 45-55 parts, and the amount of stearic acid is 0.5-1.5 parts.
[0050] Zinc oxide can promote the vulcanization reaction, improve the vulcanization efficiency, shorten the vulcanization time, and thus improve production efficiency. Zinc oxide is also an active agent that can react chemically with rubber molecules to increase the crosslinking density of rubber, significantly improving the mechanical properties and vulcanization stability of rubber. Zinc oxide has the characteristics of improving high temperature resistance and anti-aging. When the amount used increases to a certain extent, it can make the products produced have high ductility and be more stable during storage.
[0051] The vulcanizing agent of the present invention preferably comprises a peroxide vulcanizing agent or a sulfur vulcanizing agent. The peroxide vulcanizing agent can be 1,4-di-tert-butyl peroxydiisopropylbenzene, tert-butyl peroxybenzoate, diisopropylbenzene peroxide, dibenzoyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxy-3-acetylene. In order to balance the vulcanization efficiency and the operational safety, the peroxide vulcanizing agent preferably adopts a material with a half-life temperature of 150° C. to 180° C. for 1 min, such as diisopropylbenzene peroxide.
[0052] When peroxide vulcanizing agent is used, in order to increase the crosslinking density of rubber, 2.5-3.5 parts of bridging aid TAIC can be added to the raw material for preparing the rubber material of the present invention. TAIC contains a multifunctional unsaturated compound to help peroxide improve its bridging degree and bridging speed.
[0053] The present invention further proposes a method for preparing the above-mentioned rubber material, which specifically comprises the following steps:
[0054] In the internal mixer, heat to 80°C, mix the polymerized modified product of EPDM rubber and olefinic silica gel, the polymerized modified product of EPDM rubber and olefinic silane coupling agent, plasticizer and zinc oxide, and refine for 60 seconds. Add filler to the mixture in the internal mixer and continue refining. When the temperature rises to 105-115°C, lift the top bolt to exhaust. Continue to seal and refine. When the temperature rises to 135-145°C, lift the top bolt, open the discharge door, press down the top bolt to discharge the rubber, close the discharge door, obtain the mixed rubber, and park for ≥8h for standby. Take another internal mixer, heat to 80°C, put in the mixed rubber and vulcanizer, mix for 120s, lift the top bolt to exhaust, continue mixing for 120s, lift the top bolt, open the discharge door to discharge the rubber, and obtain the rubber material.
[0055] The preparation method of the polymer modified product of EPDM rubber and olefinic silica gel specifically comprises the following steps:
[0056] The temperature of the internal mixer is raised to 55-65℃, and EPDM rubber, the first initiator and olefinic silica gel are added to mix and refine; when the temperature rises to 105-110℃, the top plug is raised to exhaust. The sealed refining is continued, the stirring speed is adjusted to 60r / min, the refining temperature is controlled to be maintained at 110-160℃, and the stirring is carried out for 15-30min. After the refining is completed, the polymer modified product of EPDM rubber and olefinic silica gel is obtained. The amount of the first initiator is 1%-6% of the weight of the EPDM rubber. The refining stirring temperature and time are determined according to the 1min half-life temperature of the first initiator. When benzoyl peroxide with a 1min half-life temperature of 130°C is selected, the mixing temperature is controlled at 110°C-130°C and stirred for 15min-20min. When 1,1-di-tert-butylperoxy-3,3,5-trimethoxycyclohexane with a 1min half-life temperature of 148°C is selected, the mixing temperature is controlled at 130°C-150°C and stirred for 15min-20min. When 2,2-bis(tert-butylperoxide)butane with a 1min half-life temperature of 161°C is selected, the mixing temperature is controlled at 140°C-160°C and stirred for 15min-30min.
[0057] Taking VNB EPDM rubber and peroxide initiator as an example, the preparation route of the polymer modified product of EPDM rubber and vinyl silica gel is as follows: Figure 1 and Figure 2 As shown. First, the peroxide initiator is decomposed into free radicals by heat: ROOR→2RO·, where R represents a variety of hydrocarbon groups; then the free radicals initiate the dehydrogenation reaction of EPDM rubber, as shown Figure 1 ; Graft polymerization of EPDM rubber and olefinic silica gel with free radicals, such as Figure 2 shown.
[0058] The preparation method of the polymer modified product of EPDM rubber and olefin-based silane coupling agent comprises the following steps:
[0059] The temperature of the internal mixer is raised to 55-65°C, and EPDM rubber, a second initiator and an olefin-based silane coupling agent are added and mixed for refining; when the temperature rises to 105-110°C, exhaust is performed; the sealing refining is continued, the stirring speed is adjusted to 60r / min, and the refining temperature is controlled to be maintained at 110-160°C. After the refining is completed, a polymer modified product of EPDM rubber and an olefin-based silane coupling agent is obtained. The second initiator can be selected from 2,4-dichlorobenzamide peroxide, benzoyl peroxide, 1,1-di-tert-butylperoxy-3,3,5-trimethoxycyclohexane, p-chlorobenzoyl peroxide, 2,2-bis(tert-butylperoxide)butane, 1,2-tert-butylperoxide cyclohexane, tert-butyl peroxide 2-ethylate, and tert-butyl peroxide isobutyrate, and the amount used is 1%-6% of the weight of the EPDM rubber.
[0060] Taking VNB EPDM rubber as an example, the preparation route of the polymer modified product of EPDM rubber with free radicals and olefin-based silane coupling agent is as follows: Figure 3 shown.
[0061] The rubber material of the present invention can be used to prepare vehicle exhaust pipe hangers. The vehicle exhaust pipe hangers prepared by using the rubber material can have good durability under high temperature working conditions.
[0062] The specific implementation scheme of the present invention is described in detail below.
[0063] In order to facilitate the comparison of the material proportions of various embodiments of the present invention and the comparative examples, the present invention lists the raw materials used in various embodiments in the form of a table as follows:
[0064] Example 1
[0065] The preparation method of the rubber material of this embodiment comprises the following steps:
[0066] Preparation of polymer modified products of EPDM rubber and olefinic silica gel:
[0067] The temperature of the internal mixer was raised to 55°C, and VNB type EPDM rubber, initiator and methylphenyl vinyl silica gel were added for mixing and refining; when the temperature rose to 105°C, the top plug was raised for exhaust. The sealed refining was continued, the stirring speed was adjusted to 60r / min, the refining temperature was controlled to be maintained at 125°C to 130°C, and the stirring was performed for 20 minutes. After the refining was completed, the polymer modified product of EPDM rubber and vinyl silica gel was obtained. The initiator was benzoyl peroxide with a 1min half-life temperature of 130°C.
[0068] The dosage of the above raw materials is shown in Table 1 below:
[0069] Table 1 Polymer 1-1
[0070]
[0071] Preparation of polymer modified products of EPDM rubber and olefin-based silane coupling agent:
[0072] The temperature of the internal mixer was raised to 55°C, and VNB type EPDM rubber, initiator and vinyl triethoxysilane were added for mixing and refining; when the temperature rose to 105°C, the gas was exhausted; the sealed refining was continued, the stirring speed was adjusted to 60r / min, and the refining temperature was controlled to be maintained at 125°C-130°C for mixing for 20min. After the refining was completed, the polymer modified product of EPDM rubber and olefin-based silane coupling agent was obtained. The initiator was selected as benzoyl peroxide with a half-life of 1min at 130°C.
[0073] The dosage of the above raw materials is shown in Table 2 below:
[0074] Table 2 Polymer 2-1
[0075]
[0076] Preparation of rubber material:
[0077] In an internal mixer, heat to 80°C, mix 50 parts of a polymer modified product of EPDM rubber and olefinic silica gel, 50 parts of a polymer modified product of EPDM rubber and olefinic silane coupling agent, a plasticizer (including 50 parts of paraffin oil and 1 part of stearic acid) and 5 parts of zinc oxide, and perform refining for 60 seconds; add filler (40 parts of carbon black and 20 parts of white carbon black) to the mixture in the internal mixer, continue refining, and when the temperature rises to 105°C, raise the top bolt to exhaust. Continue to seal and refine. When the temperature rises to 135°C, lift the upper bolt, open the discharge door, press down the upper bolt to discharge the glue, close the discharge door, obtain the mixed rubber, and park it for ≥8h for standby use. Take another internal mixer, heat it to 80°C, put the mixed rubber and 5 parts of diisopropylbenzene peroxide (vulcanizing agent) and 3 parts of bridging agent TAIC into it, mix it, mix it for 120s, lift the upper bolt to exhaust, continue mixing for 120s, lift the upper bolt, open the discharge door to discharge the glue, and obtain the rubber material.
[0078] Example 2
[0079] The preparation method of the rubber material of this embodiment comprises the following steps:
[0080] Preparation of polymer modified products of EPDM rubber and olefinic silica gel:
[0081] The temperature of the internal mixer was raised to 55°C, and VNB type EPDM rubber, initiator and methylphenyl vinyl silica gel were added for mixing and refining; when the temperature rose to 105°C, the top plug was raised for exhaust. The sealed refining was continued, the stirring speed was adjusted to 60r / min, the refining temperature was controlled to be maintained at 125°C to 130°C, and the stirring was performed for 20 minutes. After the refining was completed, the polymer modified product of EPDM rubber and vinyl silica gel was obtained. The initiator was benzoyl peroxide with a 1min half-life temperature of 130°C.
[0082] The dosage of the above raw materials is shown in Table 3 below:
[0083] Table 3 Polymer 1-2
[0084]
[0085] Preparation of polymer modified products of EPDM rubber and olefin-based silane coupling agents:
[0086] The temperature of the internal mixer was raised to 55°C, and VNB type EPDM rubber, initiator and vinyl triethoxysilane were added for mixing and refining; when the temperature rose to 105°C, the gas was exhausted; the sealed refining was continued, the stirring speed was adjusted to 60r / min, and the refining temperature was controlled to be maintained at 125°C-130°C for mixing for 20min. After the refining was completed, the polymer modified product of EPDM rubber and olefin-based silane coupling agent was obtained. The initiator was selected as benzoyl peroxide with a half-life of 1min at 130°C.
[0087] The dosage of the above raw materials is shown in Table 4 below:
[0088] Table 4 Polymer 2-2
[0089]
[0090] Preparation of rubber material:
[0091] In an internal mixer, heat to 80°C, mix 55 parts of a polymer modified product of EPDM rubber and olefinic silica gel, 45 parts of a polymer modified product of EPDM rubber and olefinic silane coupling agent, a plasticizer (including 45 parts of paraffin oil and 1 part of stearic acid) and 5 parts of zinc oxide, and perform refining for 60 seconds; add filler (40 parts of carbon black and 20 parts of white carbon black) to the mixture in the internal mixer, continue refining, and when the temperature rises to 115°C, raise the top plug to exhaust; Continue to seal and refine. When the temperature rises to 145°C, lift the upper plug, open the discharge door, press down the upper plug to discharge the glue, close the discharge door, obtain the mixed rubber, and park it for ≥8h for standby use. Take another internal mixer, heat it to 80°C, put the mixed rubber and 5 parts of tert-butyl perbenzoate (vulcanizing agent) and 3 parts of bridging aid TAIC into it, mix it, mix it for 120s, lift the upper plug to exhaust, continue mixing for 120s, lift the upper plug, open the discharge door to discharge the glue, and obtain the rubber material.
[0092] Example 3
[0093] The preparation method of the rubber material of this embodiment comprises the following steps:
[0094] Preparation of polymer modified products of EPDM rubber and olefinic silica gel:
[0095] The temperature of the internal mixer was raised to 80°C, and VNB EPDM rubber, initiator and methyl vinyl silica gel were added for mixing and refining; when the temperature rose to 105°C, the top plug was raised for exhaust. The sealed refining was continued, the stirring speed was adjusted to 60r / min, the refining temperature was controlled to be maintained at 130°C-150°C, and the stirring was continued for 30 minutes. After the refining was completed, the polymer modified product of EPDM rubber and vinyl silica gel was obtained. Among them, 1,1-di-tert-butylperoxy-3,3,5-trimethoxycyclohexane was selected as the initiator.
[0096] The dosage of the above raw materials is shown in Table 5 below:
[0097] Table 5 Polymers 1-3
[0098]
[0099] Preparation of polymer modified products of EPDM rubber and olefin-based silane coupling agents:
[0100] The temperature of the internal mixer is raised to 55°C, and VNB type EPDM rubber, initiator and vinyl triethoxysilane are added for mixing and refining; when the temperature rises to 105°C, exhaust gas is discharged; the sealed refining is continued, the stirring speed is adjusted to 60r / min, and the refining temperature is controlled to be maintained at 140°C-160°C for mixing for 20 minutes. After the refining is completed, a polymer modified product of EPDM rubber and olefin-based silane coupling agent is obtained. Among them, tert-butyl peroxyisobutyrate is selected as the initiator.
[0101] The dosage of the above raw materials is shown in Table 6 below:
[0102] Table 6 Polymer 2-3
[0103]
[0104] Preparation of rubber material:
[0105] In an internal mixer, heat to 80°C, mix 60 parts of a polymer modified product of EPDM rubber and olefinic silica gel, 40 parts of a polymer modified product of EPDM rubber and olefinic silane coupling agent, a plasticizer (including 50 parts of paraffin oil and 1 part of stearic acid) and 5 parts of zinc oxide, and refine for 60 seconds; add filler (40 parts of carbon black and 20 parts of white carbon black) to the mixture in the internal mixer, continue to refine, and when the temperature rises to 105°C, raise the top bolt to exhaust. Continue sealed refining. When the temperature rises to 135°C, lift the upper bolt, open the discharge door, press down the upper bolt to discharge the glue, close the discharge door, obtain the mixed rubber, and park it for ≥8h for standby use. Take another internal mixer, heat it to 80°C, put the mixed rubber and 5 parts of dibenzoyl peroxide (vulcanizing agent) and 3 parts of bridging aid TAIC into it, mix it, mix it for 120s, lift the upper bolt to exhaust, continue mixing for 120s, lift the upper bolt, open the discharge door to discharge the glue, and obtain the rubber material.
[0106] Example 4
[0107] The preparation method of the rubber material of this embodiment comprises the following steps:
[0108] Preparation of polymer modified products of EPDM rubber and olefinic silica gel:
[0109] The temperature of the internal mixer was raised to 80℃, and VNB type EPDM rubber, initiator and methyl vinyl silica gel were added for mixing and refining; when the temperature rose to 105℃, the top plug was raised for exhaust. The sealed refining was continued, the stirring speed was adjusted to 60r / min, the refining temperature was controlled to be maintained at 155℃-160℃, and the stirring was performed for 30min. After the refining was completed, the polymer modified product of EPDM rubber and vinyl silica gel was obtained. The initiator was 2,2-bis(tert-butyl peroxide)butane with a 1min half-life temperature of 160℃.
[0110] The dosage of the above raw materials is shown in Table 7 below:
[0111] Table 7 Polymers 1-4
[0112]
[0113] Preparation of polymer modified products of EPDM rubber and olefin-based silane coupling agents:
[0114] The temperature of the internal mixer was raised to 55°C, and VNB EPDM rubber, initiator and methylphenyl vinyl silica gel were added for mixing and refining; when the temperature rose to 105°C, the top plug was raised for exhaust. The sealed refining was continued, the stirring speed was adjusted to 60r / min, the refining temperature was controlled to be maintained at 125°C to 130°C, and the stirring was continued for 20 minutes. After the refining was completed, the polymer modified product of EPDM rubber and vinyl silica gel was obtained. The initiator was 2,4-dichlorobenzamide peroxide.
[0115] The dosage of the above raw materials is shown in Table 8 below:
[0116] Table 8 Polymers 2-4
[0117]
[0118] Preparation of rubber material:
[0119] In an internal mixer, heat to 80°C, mix 70 parts of a polymer modified product of EPDM rubber and olefinic silica gel, 30 parts of a polymer modified product of EPDM rubber and olefinic silane coupling agent, a plasticizer (including 50 parts of paraffin oil and 1 part of stearic acid) and 5 parts of zinc oxide, and perform refining for 60 seconds; add filler (40 parts of carbon black and 20 parts of white carbon black) to the mixture in the internal mixer, continue refining, and when the temperature rises to 105°C, raise the top plug to vent; continue sealing and refining, when When the temperature rises to 135°C, lift the upper bolt, open the discharge door, press down the upper bolt to discharge the glue, close the discharge door, obtain the mixed rubber, and park it for ≥8h for standby; take another internal mixer, heat it to 80°C, put the mixed rubber and 5 parts of 2,5-dimethyl-2,5-di-tert-butylperoxy-3-acetylene (vulcanizing agent) and 3 parts of bridging agent TAIC into it, mix it, mix it for 120s, lift the upper bolt to exhaust, continue mixing for 120s, lift the upper bolt, open the discharge door to discharge the glue, and obtain the rubber material.
[0120] Example 5
[0121] The preparation method of the rubber material of this embodiment comprises the following steps:
[0122] Preparation of polymer modified products of EPDM rubber and olefinic silica gel:
[0123] The temperature of the internal mixer was raised to 80℃, and ENB type EPDM rubber, initiator and methyl vinyl silica gel were added for mixing and refining; when the temperature rose to 105℃, the top plug was raised for exhaust. The sealed refining was continued, the stirring speed was adjusted to 60r / min, the refining temperature was controlled to be maintained at 155℃-160℃, and the stirring was performed for 30min. After the refining was completed, the polymer modified product of EPDM rubber and vinyl silica gel was obtained. The initiator was 2,2-bis(tert-butyl peroxide)butane with a 1min half-life temperature of 160℃.
[0124] The dosage of the above raw materials is shown in Table 9 below:
[0125] Table 9
[0126]
[0127] Preparation of polymer modified products of EPDM rubber and olefin-based silane coupling agents:
[0128] The temperature of the internal mixer was raised to 80℃, and VNB type EPDM rubber, initiator and methyl vinyl silica gel were added for mixing and refining; when the temperature rose to 105℃, the top plug was raised for exhaust. The sealed refining was continued, the stirring speed was adjusted to 60r / min, the refining temperature was controlled to be maintained at 155℃-160℃, and the stirring was continued for 30min. After the refining was completed, the polymer modified product of EPDM rubber and vinyl silica gel was obtained. Among them, tert-butyl peroxyisobutyrate was selected as the initiator.
[0129] The dosage of the above raw materials is shown in Table 10 below:
[0130] Table 10
[0131]
[0132]
[0133] Preparation of rubber material:
[0134] In an internal mixer, heat to 80°C, mix 50 parts of a polymer modified product of EPDM rubber and olefinic silica gel, 50 parts of a polymer modified product of EPDM rubber and olefinic silane coupling agent, a plasticizer (including 50 parts of paraffin oil and 1 part of stearic acid) and 5 parts of zinc oxide, and perform refining for 60 seconds; add filler (40 parts of carbon black and 20 parts of white carbon black) to the mixture in the internal mixer, continue refining, and when the temperature rises to 105°C, raise the top plug to exhaust; continue to close the mixer. Seal refining, when the temperature rises to 135℃, lift the upper bolt, open the discharge door, press down the upper bolt to discharge the glue, close the discharge door, obtain the mixed rubber, and park it for ≥8h for standby; take another internal mixer, heat it to 80℃, put the mixed rubber and 5 parts of 1,4-di-tert-butylperoxydiisopropylbenzene (vulcanizing agent) and 3 parts of bridging auxiliary agent TAIC into it, mix it, mix it for 120s, lift the upper bolt to exhaust, continue mixing for 120s, lift the upper bolt, open the discharge door to discharge the glue, and obtain the rubber material.
[0135] In order to facilitate comparison of the material proportions of various embodiments of the present invention, the raw materials used in preparing the rubber materials of various embodiments of the present invention are listed in the form of a table as shown in Table 11 below.
[0136] Table 11
[0137]
[0138]
[0139] Comparative Example 1
[0140] The preparation method of the rubber material of this comparative example comprises the following steps:
[0141] In an internal mixer, heat to 80°C, mix 90 parts of VNB EPDM rubber, 10 parts of methyl vinyl silicone, 2 parts of vinyl trimethoxy silane, a plasticizer (including 50 parts of paraffin oil and 1 part of stearic acid) and 5 parts of zinc oxide, and refine for 60 seconds; add filler (40 parts of carbon black and 20 parts of white carbon black) to the mixture in the internal mixer, continue to refine, and when the temperature rises to 105°C, raise the top plug to vent; continue to seal and refine, when When the temperature rises to 135°C, lift the upper bolt, open the discharge door, press down the upper bolt to discharge the glue, close the discharge door, obtain the mixed rubber, and park it for ≥8h for standby; take another internal mixer, heat it to 80°C, put the mixed rubber and 5 parts of 1,4-di-tert-butylperoxydiisopropylbenzene (vulcanizing agent) and 3 parts of bridging agent TAIC into it, mix it, mix it for 120s, lift the upper bolt to exhaust, continue mixing for 120s, lift the upper bolt, open the discharge door to discharge the glue, and obtain the rubber material.
[0142] Comparative Example 2
[0143] The preparation method of the rubber material of this comparative example comprises the following steps:
[0144] In an internal mixer, heat to 80°C, mix 50 parts of the polymerized modified product of EPDM rubber and alkenyl silica gel prepared in Example 1, 50 parts of VNB type EPDM rubber, 2 parts of vinyl trimethoxysilane, a plasticizer (including 50 parts of paraffin oil and 1 part of stearic acid) and 5 parts of zinc oxide, and refine for 60 seconds; add filler (40 parts of carbon black and 20 parts of white carbon black) to the mixture in the internal mixer, continue to refine, and when the temperature rises to 105°C, raise the top plug to exhaust. ; Continue sealed refining, when the temperature rises to 135°C, lift the upper bolt, open the discharge door, press down the upper bolt to discharge the glue, close the discharge door, obtain the mixed rubber, and park it for ≥8h for standby; take another internal mixer, heat it to 80°C, put the mixed rubber and 5 parts of 1,4-di-tert-butylperoxydiisopropylbenzene (vulcanizing agent) and 3 parts of bridging agent TAIC into it, mix it, mix it for 120s, lift the upper bolt to exhaust, continue mixing for 120s, lift the upper bolt, open the discharge door to discharge the glue, and obtain the rubber material.
[0145] Comparative Example 3
[0146] The preparation method of the rubber material of this comparative example comprises the following steps:
[0147] In an internal mixer, heated to 80° C., 40 parts of EPDM rubber, 10 parts of methyl vinyl silica gel, 50 parts of the polymerized modified product of EPDM rubber and olefin-based silane coupling agent prepared in Example 1, a plasticizer (including 50 parts of paraffin oil and 1 part of stearic acid) and 5 parts of zinc oxide were mixed and refined for 60 seconds; fillers (40 parts of carbon black and 20 parts of white carbon black) were added to the mixture in the internal mixer, and the refining was continued. When the temperature rose to 105° C., the top plug was raised to exhaust; Continue to seal and refine. When the temperature rises to 135°C, lift the upper bolt, open the discharge door, press down the upper bolt to discharge the glue, close the discharge door, obtain the mixed rubber, and park it for ≥8h for standby use. Take another internal mixer, heat it to 80°C, put the mixed rubber and 5 parts of 1,4-di-tert-butylperoxydiisopropylbenzene (vulcanizing agent) and 3 parts of bridging agent TAIC into it, mix it, mix it for 120s, lift the upper bolt to exhaust, continue mixing for 120s, lift the upper bolt, open the discharge door to discharge the glue, and obtain the rubber material.
[0148] Comparative Example 4
[0149] This comparative example is the EPDM rubber modified material of Preparation Example 2-1 disclosed in Patent No. CN111793286A.
[0150] The rubber materials of the above-mentioned embodiments and comparative examples were subjected to performance tests, and the test data are shown in Table 12 below.
[0151] Table 12
[0152]
[0153] Note: The durability index is based on 100.
[0154] The above test data show that:
[0155] Comprehensively comparing technical indicators such as tensile strength and elongation at break, each embodiment is superior to each comparative example, and the rubber material of the present invention has better heat resistance and fatigue resistance.
[0156] Compared with comparative example 1, the two polymer modified substances improve the temperature resistance of the rubber material by 23°C and the durability index by 38 values.
[0157] Comparison between Example 1 and Example 5 shows that the thermal stability of the polymer after graft modification of the VNB type EPDM rubber used in Example 1 is higher than that of the ENB type EPDM rubber used in Example 5.
[0158] Comparing Example 3 with Example 4, Example 3 in which the amount of the polymerized modified product of EPDM rubber and olefin-based silane coupling agent used is higher has higher fatigue durability.
[0159] Comparing Example 2 and Example 3, as the amount of the polymerized modified product of EPDM rubber and olefinic silicone increases, the heat resistance is improved, but the durability is reduced.
[0160] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0161] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A rubber material, characterized in that: The raw materials for preparing the rubber material include the following components by weight: 50-70 parts of the polymer modified product of EPDM rubber and olefinic silica gel, 30-50 parts of the polymer modified product of EPDM rubber and olefinic silane coupling agent, 50-80 parts of filler, 45-55 parts of plasticizer, 4-6 parts of zinc oxide, and 4-6 parts of vulcanizer.
2. The rubber material according to claim 1, characterized in that: The weight ratio of EPDM rubber to alkenyl silica gel in the raw materials for preparing the polymer modified product of EPDM rubber and alkenyl silica gel is (80-90): (20-10).
3. The rubber material according to claim 2, characterized in that: The alkenyl silica gel includes at least one of methyl vinyl silica gel and methyl phenyl vinyl silica gel.
4. The rubber material according to claim 1, characterized in that: The weight ratio of ethylene propylene diene monomer rubber and olefin-based silane coupling agent in the raw materials for preparing the polymer modified product of ethylene propylene diene monomer rubber and olefin-based silane coupling agent is (95-99.5): (0.5-5).
5. The rubber material according to any one of claims 4, characterized in that: The olefin-based silane coupling agent includes at least one of vinyltriethoxysilane and vinyltrimethoxysilane.
6. The rubber material according to any one of claims 1 to 5, characterized in that: The vulcanizing agent includes a peroxide vulcanizing agent or a sulfur vulcanizing agent.
7. A method for preparing a rubber material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: Mixing a polymer modified product of EPDM rubber and olefinic silica gel, a polymer modified product of EPDM rubber and olefinic silane coupling agent, a plasticizer and zinc oxide, and refining the mixture; Add filler to the mixture and continue refining. When the temperature rises to 105-115℃, exhaust gas; Continue to seal and refine, and when the temperature rises to 135-145°C, discharge the rubber to obtain the mixed rubber; The rubber compound is mixed with a vulcanizing agent and refined to obtain the rubber material.
8. The method for preparing the rubber material according to claim 7, characterized in that: The preparation method of the polymer modified product of EPDM rubber and olefinic silica gel comprises the following steps: The temperature of the internal mixer is raised to 55-65°C, and EPDM rubber, the first initiator and vinyl silica gel are added to mix and then refined; When the temperature rises to 105-110℃, exhaust; The sealed refining is continued, the stirring speed is adjusted to 60 r / min, and the refining temperature is controlled to be maintained at 110-160° C. After the refining is completed, the polymer modified product of the EPDM rubber and the vinyl silica gel is obtained.
9. The method for preparing a rubber material according to claim 7 or 8, characterized in that: The method for preparing the polymerized modified product of EPDM rubber and olefin-based silane coupling agent comprises the following steps: The temperature of the internal mixer is raised to 55-65°C, and EPDM rubber, the second initiator and the olefin-based silane coupling agent are added and mixed for refining; When the temperature rises to 105-110℃, exhaust; The sealed refining is continued, the stirring speed is adjusted to 60 r / min, and the refining temperature is controlled to be maintained at 110-160° C. After the refining is completed, the polymer modified product of the EPDM rubber and the olefin-based silane coupling agent is obtained.
10. Use of the rubber material according to any one of claims 1 to 6 in preparing a vehicle exhaust pipe hanger.