Corrosion-resistant magnetic material used as door stopper

By using anti-corrosion additives and magnetic material surface coating treatment in door suction materials, the problem of poor corrosion resistance of existing door suction materials is solved, corrosion resistance and strength are significantly improved, and service life is extended.

CN118725480AInactive Publication Date: 2024-10-01WUXI AFORST PRECISION MASCH MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410819833.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The corrosion resistance of existing door latch materials is poor, resulting in a short service life.

Method used

A corrosion-resistant magnetic material is used, and through newly prepared anti-corrosion additives and magnetic material surface coating treatment, combined with PVC, CPE and other additives, a door latch material with improved corrosion resistance is prepared. The anti-corrosion additive is mixed with polyaniline, polypyrrole copolymer and montmorillonite, and compounded with zinc oxide nanoparticles. The magnetic material seals pores and cracks through the ZnAl coating to improve corrosion resistance.

Benefits of technology

Significantly improves the corrosion resistance and strength of the door suction material and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004908795830000111
    Figure BDA0004908795830000111
  • Figure BDA0004908795830000121
    Figure BDA0004908795830000121
Patent Text Reader

Abstract

The invention discloses a corrosion-resistant magnetic material used as a door stopper. The corrosion-resistant magnetic material is prepared from the following raw materials in parts by weight: 70.5 to 85.8 parts of PVC (Polyvinyl Chloride), 12.6 to 20.4 parts of CPE (Chlorinated Polyethylene), 24.5 to 32.8 parts of plasticizer, 26.8 to 34.5 parts of magnetic material, 5.3 to 7.5 parts of stabilizer, 1.2 to 1.8 parts of dispersant and 10.2 to 14.2 parts of corrosion-resistant additive. Wherein a newly-prepared corrosion-resistant auxiliary agent is used for resisting corrosion, and the auxiliary agent is a plurality of composite materials formed by copolymerizing polyaniline and polypyrrole, mixing the copolymerized polyaniline and polypyrrole with montmorillonite and compounding the mixture with zinc oxide nanoparticles. The component of the magnetic material is Nd2Fe14B, in order to improve the corrosion resistance of the magnetic material, surface protection treatment is carried out, the surface of the magnetic material is coated with a layer of ZnA coating, the ZnA coating seals most of pores and cracks of Nd2Fe14B, and the special structure of the ZnA coating is beneficial to shielding and preventing corrosion of an external corrosion medium to a magnet. And secondly, in a complex corrosive environment, zinc and aluminum in the coating can be used as sacrificial anodes for preferential corrosion, so that corrosion to the magnet is delayed, and the effect of protecting the magnet ring is further achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of house decoration supplies and relates to a corrosion-resistant magnetic material used as a door stopper. Background Art

[0002] Door catches, also known as door stops, are basic accessories for household wooden doors. They are used to fix the open door against the wall. The commonly used door catches are split structures, with one part installed at the door corner and the other installed on the wall or the ground. Since the current door catches are made of permanent magnets, they have poor corrosion resistance and a short service life. Summary of the invention

[0003] The object of the present invention is to provide a corrosion-resistant magnetic material used as a door stopper to solve the problem of poor corrosion resistance mentioned in the background technology.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A corrosion-resistant magnetic material used as a door stopper, comprising the following raw materials in parts by weight:

[0006] PVC 70.5-85.8 parts, CPE 12.6-20.4 parts, plasticizer 24.5-32.8 parts, magnetic material 26.8-34.5 parts, stabilizer 5.3-7.5 parts, dispersant 1.2-1.8 parts, anti-corrosion additive 10.2-14.2 parts;

[0007] The corrosion-resistant magnetic material used as a door stopper is prepared by the following steps:

[0008] Step A1, weighing and mixing the raw materials according to their weight, kneading and oiling at high speed for 20-25 minutes, then unloading the materials and stirring them in a cold mixing pot for 15-25 minutes, and putting the materials into a twin-screw extruder for granulation to obtain a prefabricated material;

[0009] Step A2, magnetizing the prefabricated material obtained in step A1 to make the magnetic material arranged in a directional manner, thereby obtaining a corrosion-resistant magnetic material used as a door stopper.

[0010] Furthermore, the plasticizer is one of phthalate, dioctanoic acid, adipic acid ester polyester, citrate or epoxy.

[0011] Furthermore, the stabilizer is one of a Ca / Zn composite stabilizer, pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (1010), tris(2,4-di-tert-butylphenyl)phosphite (168), and distearyl thiodipropionate (DSTDP).

[0012] Furthermore, the dispersant is one of silicates, alkali metal phosphates, triethylhexyl phosphate or sodium dodecyl sulfate.

[0013] Furthermore, the magnetization in step A2 is voltage magnetization or magnetic field magnetization.

[0014] The magnetic material is prepared by the following steps:

[0015] Step S1, Nd(NO3)3·6H2O, Fe(NO3)3·9H2O and H3BO3 are mixed, put into deionized water, and continuously stirred with a magnetic stirrer until the raw materials are completely dissolved, 0.1 mol / L NaOH solution is added to adjust the pH to 9, and the prepared raw material solution is poured into a stainless steel reactor for hydrothermal reaction at 180°C for 6h, then washed with deionized water and anhydrous ethanol for 2-3 times, and vacuum dried to obtain powder a;

[0016] Step S2, placing the powder a prepared in step S1 in a magnetic boat, and then placing it in a tube furnace, heating it to 810-850° C. in air and keeping it warm for 2 hours to obtain powder b;

[0017] Step S3, mixing powder b with CaH2, placing in a tube furnace, heating to 900°C for 2-3h in a 5% H2 / Ar mixed gas protection, to obtain a precursor;

[0018] Step S4, silane, anhydrous ethanol and pure water are mixed, and slowly stirred at room temperature to prepare a uniform silane hydrolyzate, zinc and aluminum powders are added thereto, and ethylene glycol is added during stirring to prepare a uniform Zn-Al coating liquid, and a ZnAl coating is prepared on the surface of the precursor prepared in step S3 by an air spraying process, and the coating is dried after spraying to obtain a magnetic material.

[0019] Furthermore, in step S1, the usage ratio of Nd(NO3)3·6H2O, Fe(NO3)3·9H2O, H3BO3 and deionized water is 0.30-0.35 g: 0.53-0.64 g: 0.01-0.015 g: 25-35 mL.

[0020] Furthermore, in step S3, the mass ratio of powder b and CaH2 is 1:1.25-1.3.

[0021] Furthermore, in step S4, the mass ratio of silane, anhydrous ethanol, pure water, zinc and aluminum powder is 1:1:2.5-2.8:3:1.

[0022] The anti-corrosion additive is prepared by the following steps:

[0023] Step C1, adding sulfosalicylic acid to deionized water, stirring to fully dissolve it, then adding aniline and pyrrole, electromagnetically stirring for 1.5-2.5 hours in an ice-water bath to form a uniform emulsion, adding ammonium persulfate to deionized water to prepare a solution, slowly adding it dropwise to the above emulsion, controlling the reaction temperature at 0-4°C, reacting for 6 hours, maintaining the pH of the reaction solution at 3.9-4.0, filtering and drying to obtain a copolymer;

[0024] Step C2, adding the copolymer prepared in step C1 into a three-necked flask, adding hydrochloric acid to adjust the pH to 1-2 to obtain an emulsion, dispersing the montmorillonite in deionized water, ultrasonically dispersing for 1.5-2 hours to obtain a suspension, mixing the emulsion and the suspension, stirring for 3-4 hours, then adding ammonium persulfate, stirring and reacting at 30-32° C. for 10-11 hours, and demulsifying with ethanol, filtering, washing, drying, and grinding to obtain an intermediate product a;

[0025] Step C3, mixing hydrated zinc acetate and deionized water, heating to 65-68°C, adding 1 mol / L sodium hydroxide solution to adjust the pH to 13, adding potassium citrate, reacting for 4-5 hours, filtering, washing the precipitate with distilled water until it is neutral, and drying to obtain an intermediate product b;

[0026] Step C4, add intermediate product a and 1.0 mol / L hydrochloric acid solution to a three-necked flask, place it in an ice bath and stir for 40-60 minutes, add intermediate product b and ammonium persulfate, stir for 10-15 hours, filter, wash the precipitate with anhydrous ethanol and distilled water 2-3 times, and dry to obtain an anti-corrosion additive.

[0027] Furthermore, in step C1, the molar ratio of sulfosalicylic acid, deionized water, aniline, pyrrole, ammonium persulfate, and deionized water is 1:6.5-7:1:1:1:3-3.5.

[0028] Furthermore, the molar ratio of the copolymer, montmorillonite, deionized water and ammonium persulfate in step C2 is 1:0.06:3-4:2.6-2.8.

[0029] Furthermore, in step C3, the dosage ratio of hydrated zinc acetate, deionized water and potassium citrate is 0.12-0.14 mol:110-130 mL:13-15 mg.

[0030] Furthermore, in step C4, the usage ratio of the intermediate product a, the hydrochloric acid solution, the intermediate product b, and the ammonium persulfate is 0.3-0.5 g: 50-60 mL: 20-35 mg: 55-60 mg.

[0031] Beneficial effects of the present invention:

[0032] The invention discloses a corrosion-resistant magnetic material used as a door stopper, and the corrosion-resistant effect is a newly prepared anti-corrosion auxiliary agent, which is a plurality of composite materials prepared by copolymerizing polyaniline and polypyrrole and mixing with montmorillonite, and then compounding with zinc oxide nanoparticles. Some high molecular conductive polymers such as polyaniline and polypyrrole have efficient inhibition, because the presence of π electrons, quaternary nitrogen atoms and macromolecules protects metals from corrosion, and polyaniline has the advantages of low price, stable properties and unique anti-corrosion mechanism, and polypyrrole has the advantages of easy synthesis, excellent electrical conductivity and low monomer toxicity, and is also highly concerned in the application of anti-corrosion field, and secondly, it is compounded with montmorillonite, and montmorillonite sheets have an obstructive effect on water molecules and oxygen molecules, thereby enhancing its anti-solution permeability, and enhancing the anti-corrosion performance of the polymer itself.

[0033] The composition of the magnetic material is Nd2Fe 14 B. The source of magnetism is the vector of the atomic magnetic moment and the interaction with neighboring atoms. 14 In B magnets, there are mainly three types of exchange interactions between Nd-Nd, Nd-Fe and Fe-Fe atomic pairs, among which the exchange interaction between Nd-Nd atomic pairs is the weakest, and that between Fe-Fe is the strongest. 14 The magnetic moments of Nd and Fe in B are arranged in parallel, which is ferromagnetic coupling. It is the magnet with the highest Ms among rare earth-based magnets. The magnetic material is loose and porous inside and on the surface, and has a multi-phase structure, resulting in poor corrosion resistance. In order to improve the corrosion resistance of the magnetic material itself, surface protection treatment is carried out. The surface coating is used to isolate the corrosive medium in the working environment from eroding the magnet. A layer of ZnAl coating is applied on the surface of the magnet. The ZnAl coating seals the Nd2Fe 14 The ZnAl coating can fill most of the pores and cracks of the magnet, and the special structure of the ZnAl coating helps to shield and prevent the corrosion of the magnet by external corrosive media. Secondly, in a complex corrosive environment, the zinc and aluminum in the coating can act as sacrificial anodes for preferential corrosion to delay the corrosion of the magnet, thereby protecting the magnetic ring. Finally, the corrosion products formed by metals such as Zn and Al during the corrosion process further fill the pores and cracks, which hinders the movement of the corrosive medium and further improves the corrosion resistance of the magnet. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] The magnetic material is prepared by the following steps:

[0037] Step S1, 0.30g Nd(NO3)3·6H2O, 0.53g Fe(NO3)3·9H2O and 0.01g H3BO3 were mixed, put into 25mL deionized water, and stirred continuously with a magnetic stirrer until the raw materials were completely dissolved, 0.1mol / L NaOH solution was added to adjust the pH to 9, and the prepared raw material solution was poured into a stainless steel reactor for hydrothermal reaction at 180°C for 6h, then washed twice with deionized water and anhydrous ethanol, and vacuum dried to obtain powder a;

[0038] Step S2, placing the powder a prepared in step S1 in a magnetic boat, and then placing it in a tube furnace, heating it to 810° C. in air and keeping it at this temperature for 2 hours to obtain powder b;

[0039] Step S3, mixing powder b with CaH2, placing in a tube furnace, heating to 900°C for 2 hours in a 5% H2 / Ar mixed gas protection, to obtain a precursor, wherein the mass ratio of powder b to CaH2 is 1:1.25;

[0040] Step S4, mixing silane, anhydrous ethanol and pure water, slowly stirring at room temperature to prepare a uniform silane hydrolyzate, adding zinc and aluminum powders thereto, adding ethylene glycol during stirring to prepare a uniform Zn-Al coating liquid, and using an air spraying process to prepare a ZnAl coating on the surface of the precursor prepared in step S3, and drying after spraying to obtain a magnetic material, wherein the mass ratio of silane, anhydrous ethanol, pure water, zinc and aluminum powders is 1:1:2.5:3:1.

[0041] Example 2

[0042] The magnetic material is prepared by the following steps:

[0043] Step S1, 0.32g Nd(NO3)3·6H2O, 0.58g Fe(NO3)3·9H2O and 0.012g H3BO3 were mixed and placed in 30mL deionized water, and stirred continuously with a magnetic stirrer until the raw materials were completely dissolved, 0.1mol / L NaOH solution was added to adjust the pH to 9, and the prepared raw material solution was poured into a stainless steel reactor for hydrothermal reaction at 180°C for 6h, and then washed twice with deionized water and anhydrous ethanol, and vacuum dried to obtain powder a;

[0044] Step S2, placing the powder a prepared in step S1 in a magnetic boat, and then placing it in a tube furnace, heating it to 840° C. in air and keeping it at this temperature for 2 hours to obtain powder b;

[0045] Step S3, mixing powder b with CaH2, placing in a tube furnace, heating to 900°C for 2 hours in a 5% H2 / Ar mixed gas protection, to obtain a precursor, wherein the mass ratio of powder b to CaH2 is 1:1.27;

[0046] Step S4, silane, anhydrous ethanol, and pure water are mixed, and slowly stirred at room temperature to prepare a uniform silane hydrolyzate, zinc and aluminum powders are added thereto, and ethylene glycol is added during stirring to prepare a uniform Zn-Al coating liquid, and a ZnAl coating is prepared on the surface of the precursor prepared in step S3 by air spraying, and the coating is dried after spraying to obtain a magnetic material, wherein the mass ratio of silane, anhydrous ethanol, pure water, zinc, and aluminum powder is 1:1:2.7:3:1

[0047] Example 3

[0048] The magnetic material is prepared by the following steps:

[0049] Step S1, 0.35g Nd(NO3)3·6H2O, 0.64g Fe(NO3)3·9H2O and 0.015g H3BO3 were mixed and placed in 35mL deionized water, and stirred continuously with a magnetic stirrer until the raw materials were completely dissolved, 0.1mol / L NaOH solution was added to adjust the pH to 9, and the prepared raw material solution was poured into a stainless steel reactor for hydrothermal reaction at 180°C for 6h, and then washed with deionized water and anhydrous ethanol for 3 times, and vacuum dried to obtain powder a;

[0050] Step S2, placing the powder a prepared in step S1 in a magnetic boat, and then placing it in a tube furnace, heating it to 850° C. in air and keeping it at this temperature for 2 hours to obtain powder b;

[0051] Step S3, mixing powder b with CaH2, placing in a tube furnace, heating to 900°C for 3 hours in a 5% H2 / Ar mixed gas protection, to obtain a precursor, wherein the mass ratio of powder b to CaH2 is 1:1.3;

[0052] Step S4, mixing silane, anhydrous ethanol and pure water, slowly stirring at room temperature to prepare a uniform silane hydrolyzate, adding zinc and aluminum powders thereto, adding ethylene glycol during stirring to prepare a uniform Zn-Al coating liquid, and using an air spraying process to prepare a ZnAl coating on the surface of the precursor prepared in step S3, and drying after spraying to obtain a magnetic material, wherein the mass ratio of silane, anhydrous ethanol, pure water, zinc and aluminum powders is 1:1:2.8:3:1.

[0053] Example 4

[0054] The anti-corrosion additive is prepared by the following steps:

[0055] Step C1, adding sulfosalicylic acid to deionized water, stirring to fully dissolve it, then adding aniline and pyrrole, electromagnetically stirring for 1.5 hours under ice-water bath conditions to form a uniform emulsion, adding ammonium persulfate to deionized water to prepare a solution, slowly adding it dropwise to the above emulsion, controlling the reaction temperature at 0°C, reacting for 6 hours, maintaining the pH of the reaction solution at 3.9, filtering and drying to obtain a copolymer, wherein the molar ratio of sulfosalicylic acid, deionized water, aniline, pyrrole, ammonium persulfate, and deionized water is 1:6.5:1:1:1:3;

[0056] Step C2, adding the copolymer prepared in step C1 into a three-necked flask, adding hydrochloric acid to adjust the pH to 1 to obtain an emulsion, dispersing montmorillonite in deionized water, ultrasonically dispersing for 1.5 hours to obtain a suspension, mixing the emulsion and the suspension, stirring for 3-4 hours, then adding ammonium persulfate, stirring and reacting at 30-32° C. for 10 hours, demulsifying with ethanol, filtering, washing, drying, and grinding to obtain an intermediate product a, wherein the molar ratio of the copolymer, montmorillonite, deionized water, and ammonium persulfate is 1:0.06:3:2.6;

[0057] Step C3, mixing hydrated zinc acetate and deionized water, heating to 65°C, adding 1 mol / L sodium hydroxide solution to adjust the pH to 13, adding potassium citrate, reacting for 4 hours, filtering, washing the precipitate with distilled water until neutral, and drying to obtain an intermediate product b, wherein the amount ratio of hydrated zinc acetate, deionized water, and potassium citrate is 0.12 mol:110 mL:13 mg;

[0058] Step C4, add intermediate product a and 1.0 mol / L hydrochloric acid solution to a three-necked flask, place it in an ice bath and stir for 40 minutes, add intermediate product b and ammonium persulfate, stir for 10 hours, filter, wash the precipitate with anhydrous ethanol and distilled water 2-3 times, and dry to obtain an anti-corrosion additive, wherein the amount ratio of intermediate product a, hydrochloric acid solution, intermediate product b, and ammonium persulfate is 0.3g:50mL:20mg:55mg.

[0059] Example 5

[0060] The anti-corrosion additive is prepared by the following steps:

[0061] Step C1, adding sulfosalicylic acid to deionized water, stirring to fully dissolve it, then adding aniline and pyrrole, electromagnetically stirring for 2 hours under ice-water bath conditions to form a uniform emulsion, adding ammonium persulfate to deionized water to prepare a solution, slowly adding it dropwise to the above emulsion, controlling the reaction temperature at 2°C, reacting for 6 hours, maintaining the pH of the reaction solution at 3.9, filtering and drying to obtain a copolymer, wherein the molar ratio of sulfosalicylic acid, deionized water, aniline, pyrrole, ammonium persulfate, and deionized water is 1:6.7:1:1:1:3.2;

[0062] Step C2, adding the copolymer prepared in step C1 into a three-necked flask, adding hydrochloric acid to adjust the pH to 1 to obtain an emulsion, dispersing montmorillonite in deionized water, ultrasonically dispersing for 2 hours to obtain a suspension, mixing the emulsion and the suspension, stirring for 3 hours, then adding ammonium persulfate, stirring and reacting at 31° C. for 10 hours, demulsifying with ethanol, filtering, washing, drying, and grinding to obtain an intermediate product a, wherein the molar ratio of the copolymer, montmorillonite, deionized water, and ammonium persulfate is 1:0.06:3:2.7;

[0063] Step C3, mixing hydrated zinc acetate and deionized water, heating to 67°C, adding 1 mol / L sodium hydroxide solution to adjust the pH to 13, adding potassium citrate, reacting for 4 hours, filtering, washing the precipitate with distilled water until neutral, and drying to obtain an intermediate product b, wherein the amount ratio of hydrated zinc acetate, deionized water, and potassium citrate is 0.13 mol:120 mL:14 mg;

[0064] Step C4, add intermediate product a and 1.0 mol / L hydrochloric acid solution to a three-necked flask, place it in an ice bath and stir for 50 minutes, add intermediate product b and ammonium persulfate thereto, stir for 12 hours, filter, wash the precipitate twice with anhydrous ethanol and distilled water, and dry to obtain an anti-corrosion additive, wherein the amount ratio of intermediate product a, hydrochloric acid solution, intermediate product b, and ammonium persulfate is 0.4g:55mL:27mg:57mg.

[0065] Example 6

[0066] The anti-corrosion additive is prepared by the following steps:

[0067] Step C1, adding sulfosalicylic acid to deionized water, stirring to fully dissolve it, then adding aniline and pyrrole, electromagnetically stirring for 2.5 hours under ice-water bath conditions to form a uniform emulsion, adding ammonium persulfate to deionized water to prepare a solution, slowly adding it dropwise to the above emulsion, controlling the reaction temperature at 4°C, reacting for 6 hours, maintaining the pH of the reaction solution at 4.0, filtering and drying to obtain a copolymer, wherein the molar ratio of sulfosalicylic acid, deionized water, aniline, pyrrole, ammonium persulfate, and deionized water is 1:7:1:1:1:3.5;

[0068] Step C2, adding the copolymer prepared in step C1 into a three-necked flask, adding hydrochloric acid to adjust the pH to 2 to obtain an emulsion, dispersing montmorillonite in deionized water, ultrasonically dispersing for 2 hours to obtain a suspension, mixing the emulsion and the suspension, stirring for 4 hours, then adding ammonium persulfate, stirring and reacting at 32° C. for 11 hours, demulsifying with ethanol, filtering, washing, drying, and grinding to obtain an intermediate product a, wherein the molar ratio of the copolymer, montmorillonite, deionized water, and ammonium persulfate is 1:0.06:4:2.8;

[0069] Step C3, mixing hydrated zinc acetate and deionized water, heating to 68°C, adding 1 mol / L sodium hydroxide solution to adjust the pH to 13, adding potassium citrate, reacting for 5 hours, filtering, washing the precipitate with distilled water until neutral, and drying to obtain an intermediate product b, wherein the amount ratio of hydrated zinc acetate, deionized water, and potassium citrate is 0.14 mol:130 mL:15 mg;

[0070] Step C4, add intermediate product a and 1.0 mol / L hydrochloric acid solution to a three-necked flask, place it in an ice bath and stir for 60 minutes, add intermediate product b and ammonium persulfate thereto, stir for 15 hours, filter, wash the precipitate with anhydrous ethanol and distilled water for 3 times, and dry to obtain an anti-corrosion additive, wherein the amount ratio of intermediate product a, hydrochloric acid solution, intermediate product b, and ammonium persulfate is 0.5g:60mL:35mg:60mg.

[0071] Example 7

[0072] A corrosion-resistant magnetic material used as a door stopper, comprising the following raw materials in parts by weight:

[0073] 70.5 parts of PVC, 12.6 parts of CPE, 24.5 parts of phthalate, 26.8 parts of the magnetic material prepared in Example 1, 5.35 parts of Ca / Zn composite stabilizer, 1.2 parts of silicates, and 10.2 parts of the anti-corrosion additive prepared in Example 4;

[0074] The corrosion-resistant magnetic material used as a door stopper is prepared by the following steps:

[0075] Step A1, weigh and mix the raw materials according to their weight, knead and oil-fill for 20 minutes at high speed, then unload the materials and stir them in a cold mixing pot for 15 minutes, and put the materials into a twin-screw extruder for granulation to obtain a prefabricated material;

[0076] Step A2, applying voltage to the prefabricated material obtained in step A1 to make the magnetic material arranged in a directional manner, thereby obtaining a corrosion-resistant magnetic material used as a door stopper.

[0077] Example 8

[0078] A corrosion-resistant magnetic material used as a door stopper, comprising the following raw materials in parts by weight:

[0079] 80 parts of PVC, 15.5 parts of CPE, 27.2 parts of dioctanoic acid, 29.1 parts of the magnetic material prepared in Example 2, 6 parts of tris(2,4-di-tert-butylphenyl)phosphite (168), 1.5 parts of alkali metal phosphates, and 12.7 parts of the anti-corrosion additive prepared in Example 5;

[0080] The corrosion-resistant magnetic material used as a door stopper is prepared by the following steps:

[0081] Step A1, weigh and mix the raw materials according to their weight, knead and oil-fill for 22 minutes at high speed, then unload the materials and stir them in a cold mixing pot for 20 minutes, and put the materials into a twin-screw extruder for granulation to obtain a prefabricated material;

[0082] Step A2, applying voltage to the prefabricated material obtained in step A1 to make the magnetic material arranged in a directional manner, thereby obtaining a corrosion-resistant magnetic material used as a door stopper.

[0083] Example 9

[0084] A corrosion-resistant magnetic material used as a door stopper, comprising the following raw materials in parts by weight:

[0085] 85.8 parts of PVC, 20.4 parts of CPE, 32.8 parts of adipic acid ester polyester, 34.5 parts of the magnetic material prepared in Example 3, 7.5 parts of distearyl thiodipropionate (DSTDP), 1.8 parts of sodium lauryl sulfate, and 14.2 parts of the anti-corrosion additive prepared in Example 6;

[0086] The corrosion-resistant magnetic material used as a door stopper is prepared by the following steps:

[0087] Step A1, weigh and mix the raw materials according to their weight, knead and oil-fill for 25 minutes at high speed, then unload the materials and stir them in a cold mixing pot for 5 minutes, and put the materials into a twin-screw extruder for granulation to obtain a prefabricated material;

[0088] Step A2, magnetizing the prefabricated material obtained in step A1 in a magnetic field so that the magnetic material is arranged in a directional manner, thereby obtaining a corrosion-resistant magnetic material used as a door stopper.

[0089] Comparative Example 1

[0090] Door catch magnetic materials produced by Zhejiang Qiaci Magnetic Industry Co., Ltd.

[0091] Comparative Example 2

[0092] The preparation method of the door attractant magnetic material of Comparative Example 2 refers to that of Example 7, except that no anti-corrosion additive is added.

[0093] Comparative Example 3

[0094] The preparation method of the door stopper magnetic material of Comparative Example 3 refers to Example 8, except that the magnetic material is not subjected to the coating process of the Zn-Al coating liquid.

[0095] The door stopper magnetic materials obtained in Examples 7-9 and Comparative Examples 1-3 were subjected to the following performance tests: tensile strength (ASTMD412), elongation at break (ASTMD412), corrosion resistance (a neutral salt spray test was performed on the door stopper using a salt spray corrosion test box to study the corrosion resistance of the coating. According to national standards, a continuous spray test method was used. The experimental temperature of this experiment was 35°C ± 1°C, the salt water concentration was 5%, the pH value of the salt water was 6.7-7.2, and the spray volume was 1.0-2.0 / 80cm 2 h, the sample surface is placed in the salt spray chamber at an inclination angle of 20°±5. When visible corrosion products appear, the time ends, and the corresponding time is the neutral salt spray resistance time of the product for measurement). The test results are shown in Table 1:

[0096] Table 1

[0097]

[0098]

[0099] It can be seen from Table 1 that compared with Comparative Examples 1-3, the door attractant magnetic materials prepared in Examples 7-9 have better strength and corrosion resistance.

[0100] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0101] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A corrosion-resistant magnetic material used as a door stopper, It is characterized in that The raw materials include the following parts by weight: 70.5-85.8 parts of PVC, 12.6-20.4 parts of CPE, 24.5-32.8 parts of plasticizer, 26.8-34.5 parts of magnetic material, 5.3-7.5 parts of stabilizer, 1.2-1.8 parts of dispersant, and 10.2-14.2 parts of anti-corrosion additive; The corrosion-resistant magnetic material used as a door stopper is prepared by the following steps: Step A1, weighing and mixing the raw materials according to their weight, kneading and oiling at high speed for 20-25 minutes, then unloading the materials and stirring them in a cold mixing pot for 15-25 minutes, and putting the materials into a twin-screw extruder for granulation to obtain a prefabricated material; Step A2, magnetizing the prefabricated material obtained in step A1 to make the magnetic material arranged in a directional manner, thereby obtaining a corrosion-resistant magnetic material used as a door stopper.

2. A corrosion-resistant magnetic material used as a door stopper according to claim 1, Features: The plasticizer is one of phthalate, dioctanoic acid, adipic acid ester polyester, citrate or epoxy.

3. The corrosion-resistant magnetic material used as a door stopper according to claim 1, Features: The stabilizer is one of Ca / Zn composite stabilizer, pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (1010), tris(2,4-di-tert-butylphenyl)phosphite (168), and distearyl thiodipropionate (DSTDP), and the dispersant is one of silicates, alkali metal phosphates, triethylhexyl phosphoric acid or sodium dodecyl sulfate.

4. The corrosion-resistant magnetic material used as a door stopper according to claim 1, Features: The magnetization in step A2 is voltage magnetization or magnetic field magnetization.

5. The corrosion-resistant magnetic material used as a door stopper according to claim 1, Features: The magnetic material is prepared by the following steps: Step S1: Nd(NO 3 ) 3 6H 2 O,Fe(NO 3 ) 3 9H 2 O and H 3 BO 3 Mix, put into deionized water, stir until the raw materials are completely dissolved, add 0.1 mol / L NaOH solution to adjust the pH to 9, pour the prepared raw material solution into the reactor for reaction, wash and dry to obtain powder a; Step S2, placing the powder a prepared in step S1 in a magnetic boat, and then placing it in a tube furnace, and heating it in air to obtain powder b; Step S3, mixing powder b with CaH 2 Mix and place in a tube furnace in 5% H 2 / Ar mixed gas protection, heating to obtain a precursor; Step S4, mixing silane, anhydrous ethanol and pure water, slowly stirring at room temperature to prepare a uniform silane hydrolyzate, adding zinc and aluminum powders thereto, adding ethylene glycol while stirring to prepare a uniform Zn-Al coating liquid, and using an air spraying process to prepare a ZnAl coating on the surface of the precursor prepared in step S3, and drying after spraying to obtain a magnetic material.

6. The corrosion-resistant magnetic material used as a door stopper according to claim 1, Features: The anti-corrosion additive is prepared by the following steps: Step C1, adding sulfosalicylic acid to deionized water, stirring, then adding aniline and pyrrole, stirring and mixing in an ice-water bath to form a uniform emulsion, adding ammonium persulfate to deionized water to prepare a solution, slowly dropping it into the above emulsion, maintaining the pH at 3.9-4.0, reacting at 0-4°C, filtering and drying to obtain a copolymer; Step C2, adding the copolymer prepared in step C1 into a three-necked flask, adding hydrochloric acid to adjust the pH to 1-2 to obtain an emulsion, dispersing the montmorillonite in deionized water, ultrasonically dispersing for 1.5-2h to obtain a suspension, mixing the emulsion and the suspension, stirring, and then adding ammonium persulfate, stirring for reaction, demulsifying with ethanol, filtering, washing, drying, and grinding to obtain an intermediate product a; Step C3, mixing hydrated zinc acetate and deionized water, heating to 65-68°C, adding sodium hydroxide solution to adjust the pH to 13, adding potassium citrate, reacting for 4-5h, filtering, washing and drying the precipitate to obtain the intermediate product b; Step C4, add intermediate product a and 1.0 mol / L hydrochloric acid solution to a three-necked flask and place in an ice bath. Stir for 40-60 min, add intermediate product b and ammonium persulfate, stir for 10-15 h, filter, The precipitate is washed and dried to obtain an anti-corrosion additive.