Anti-aging insulated cable material and preparation method thereof

By adding modified stabilizers and nano-calcium carbonate and other ingredients into insulated cable materials to form a composite, the problem of performance degradation of traditional insulated cable materials under heat, light and chemical corrosion is solved, and the durability and safety of the material are improved. .

CN118725482AInactive Publication Date: 2024-10-01SUMITOMO ELECTRIC OPTICAL FIBER & CABLE SHENZHEN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410854277.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional insulated cable materials are susceptible to heat, light, and chemical corrosion during long-term use, leading to performance degradation and safety hazards. Existing anti-aging technologies have problems with low thermal stability and poor durability.

Method used

Use polyvinyl chloride resin and polypropylene as the matrix, add modified stabilizers, nano-calcium carbonate, alkyd resin, polyvinyl alcohol, silicone flame retardants and antioxidants, and form a composite through processes such as ultrasonic dispersion, ball milling and chemical synthesis. material to improve the thermal stability, mechanical properties and flame retardant properties of the material.

Benefits of technology

Significantly improve the material's heat resistance, light resistance and chemical corrosion resistance, extend the service life of the cable, enhance the stability and safety in harsh environments, and meet strict safety standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917644820000161
    Figure BDA0004917644820000161
Patent Text Reader

Abstract

The invention discloses an anti-aging insulated cable material and a preparation method thereof, and belongs to the technical field of cable materials, the cable material realizes excellent anti-aging performance through a specific formula and process, and the cable material mainly comprises polyvinyl chloride resin, polypropylene, a modified stabilizer and a filler. A series of functional additives including alkyd resin, polyvinyl alcohol, an organic silicon flame retardant, a plasticizer and an antioxidant; the preparation process of the insulated cable material comprises the steps of premixing, melting and mixing, plasticizing treatment, extrusion, cooling and curing, pelletizing and drying treatment. Compared with the prior art, the cable insulating material provided by the invention has the advantages of long service life, high safety and excellent mechanical property, and is suitable for various harsh environmental conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cable materials, and in particular to an anti-aging insulating cable material and a preparation method thereof. Background Art

[0002] With the acceleration of industrialization and urbanization, cables, as essential components for power transmission and communications, are increasingly used in modern society. The performance of insulating cable materials is directly related to the service life, safety, and reliability of the cables. Traditional insulating cable materials, such as polyvinyl chloride (PVC) and polypropylene (PP), while offering excellent insulation and mechanical properties, are susceptible to factors such as heat, light, and chemical corrosion over long-term use, leading to degradation of material performance and, in turn, compromising the safe operation of the cables.

[0003] Especially in outdoor applications, cables must withstand harsh environmental conditions such as UV radiation, temperature fluctuations, and mechanical stress, all of which accelerate cable aging. Aging cables not only degrade in performance but can also pose safety risks such as overheating and insulation cracking, increasing maintenance costs and replacement frequency. Therefore, developing insulating cable materials with excellent aging resistance is crucial for extending cable life and reducing maintenance costs.

[0004] While existing anti-aging technologies, such as adding traditional stabilizers, antioxidants, and UV absorbers, can improve cable aging resistance to a certain extent, they still suffer from issues such as low thermal stability, poor compatibility with the matrix resin, and poor dispersibility. Furthermore, with increasing environmental protection requirements, some traditional additives are restricted or banned due to the presence of hazardous substances.

[0005] Chinese invention patent CN111925604B discloses a cable material and its preparation method. The material comprises the following components, by weight: 30-50 parts polyvinyl chloride resin, 15-25 parts plasticizer, 5-12 parts stabilizer, 0.1-1 part antioxidant, 0.1-1 part lubricant, 10-30 parts inorganic filler, 0.5-2 parts anti-aging agent, 1-2 parts dispersant, and 0.5-1 part anti-leakage agent. The plasticizer comprises at least two different benzene plasticizers. This cable material meets the relevant requirements of Australian standards, including tensile strength, elongation, aging performance, weight loss, and plasticizer exudation. However, this cable material still suffers from insufficient resistance to heat and UV aging, as well as poor durability. Summary of the Invention

[0006] In response to the deficiencies in the prior art, the present invention aims to provide a new type of anti-aging insulating cable material and a preparation method thereof. Through innovative formulas and processes, the material's heat resistance, light resistance, chemical corrosion resistance and other properties are significantly improved, thereby effectively extending the service life of the cable and enhancing its stability and safety in harsh environments.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0008] A method for preparing an anti-aging insulating cable material is as follows:

[0009] Add polyvinyl chloride resin and polypropylene into a mixer and pre-mix them. Heat the pre-mixed polyvinyl chloride resin and polypropylene to a molten state, then add a modified stabilizer and a filler, and keep mixing to ensure uniform dispersion. After the melt mixing is uniform, add alkyd resin, polyvinyl alcohol, silicone flame retardant, plasticizer and antioxidant in sequence, and mix until all components are completely and evenly dispersed. Put the mixture into a twin-screw extruder for plasticization. The plasticized mixture is extruded through the extruder and cooled and solidified in a water tank. The cooled material is pelletized by a pelletizer, and the pellets are dried to obtain an insulating cable material.

[0010] The weight proportions of the various substances are as follows: 50 to 70 parts of polyvinyl chloride resin, 15 to 25 parts of polypropylene, 8 to 12 parts of modified stabilizer, 4 to 6 parts of filler, 10 to 15 parts of alkyd resin, 5 to 10 parts of polyvinyl alcohol, 1 to 3 parts of organosilicon flame retardant, 1 to 3 parts of plasticizer and 2 to 4 parts of antioxidant.

[0011] The filler is at least one of nano calcium carbonate, nano carbon black and silicon dioxide.

[0012] The plasticizer is at least one of glycerol tripalerate, dioctyl terephthalate, and tricresyl phosphate.

[0013] The antioxidant is at least one of p-phenylenediamine, didodecyl alcohol ester, didetradecyl alcohol ester, didedecyl alcohol ester, dilauryl thiodipropionate, and lauryl octadecyl thiodipropionate.

[0014] The heating to a molten state is heating to a molten state at 180-190°C.

[0015] The temperature of the plasticizing treatment is 190-210°C.

[0016] The extrusion temperature is 190-210° C., and the screw speed is 20-50 rpm.

[0017] The temperature of the drying process is 40-60°C.

[0018] The preparation method of the modified stabilizer is as follows, in parts by weight:

[0019] S1. Mix 12 to 18 parts of nano zinc sulfide and 18 to 22 parts of bentonite, add them to 180 to 220 parts of 0.5 to 1 mol / L nitric acid, and perform ultrasonic dispersion. The ultrasonic dispersion frequency is 20 to 60 kHz, the power is 200 to 400 W, and the time is 20 to 40 minutes. After ultrasonic dispersion, wash with water and dry to obtain an acid-treated mixture; add the acid-treated mixture to a ball mill, perform thorough ball milling and mixing, and pass through a 200 to 400 mesh sieve to obtain a mixed powder; add 18 to 22 parts of the mixed powder to 70 to 90 parts of a 4 to 6 wt% aqueous solution of sodium carboxymethyl cellulose, stir and disperse, and add 4 to 6 parts of 1-(4-isothiocyanate) diacetylene triamine and 1 to 3 parts of tri(isopropenyloxy)vinyl silane. After stirring and mixing for 10 to 30 minutes, dry at a temperature of 90 to 100° C. to constant weight to obtain a composite;

[0020] S2. Dissolve 2 to 4 parts of hydroquinone in 18 to 22 parts of anhydrous ethanol, add 0.5 to 1 part of dimethyl sulfate and 1 to 3 parts of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 4 to 6 hours, add to 80 to 120 parts of a pre-mixed mixed solvent of ethyl acetate and n-hexane, the mass ratio of ethyl acetate to n-hexane being 2 to 4:6 to 8; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 8000 to 12000 rpm for 3 to 8 minutes, wash with anhydrous ethanol, and then dry at 40 to 50°C to obtain a modified stabilizer.

[0021] In the method for preparing the insulating cable material of the present invention, each substance has the following functions:

[0022] Polyvinyl chloride resin, as the main polymer matrix, provides basic insulation properties and mechanical strength of the cable.

[0023] Polypropylene may be used to increase the toughness and heat resistance of polyvinyl chloride resins, as well as to improve processing properties.

[0024] Modified stabilizers improve the thermal stability and light stability of materials and prevent aging during processing and use.

[0025] Nano-calcium carbonate as a filler may be used to improve the hardness, heat resistance and dimensional stability of materials.

[0026] Alkyd resins may be used to improve the bonding properties and increase the mechanical strength of the material.

[0027] Polyvinyl alcohol may be used to improve the material's flexibility and chemical resistance.

[0028] Silicone flame retardants provide or enhance the flame retardant properties of materials to meet safety standards.

[0029] Glyceryl tripalerate acts as a plasticizer to improve the flexibility and processing properties of the material.

[0030] Paraphenylenediamine acts as an antioxidant to prevent thermal degradation of the material at high temperatures.

[0031] Sodium carboxymethyl cellulose acts as a stabilizer or dispersant to improve the dispersibility of the components in the modified stabilizer.

[0032] The unique molecular structure and chemical properties of 1-(4-isothiocyanate) diacetylene triamine may provide improved thermal stability, light stability, and flame retardancy for cable insulation materials. These properties help maintain the material's performance during aging and extend its service life.

[0033] The unique molecular structure and chemical properties of tris(isopropenyloxy)vinylsilane may provide improved thermal stability, light stability, and flame retardancy for cable insulation materials. These properties help maintain the material's performance during aging and extend its service life.

[0034] In the preparation of modified stabilizers, hydroquinone may participate as a reactant in forming the desired stabilizer structure.

[0035] Anhydrous ethanol is used as a solvent to dissolve hydroquinone and other reactants.

[0036] Dimethyl sulfate may act as a reactant and participate in the formation of specific functional groups in the modified stabilizer.

[0037] The molecular characteristics of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) give it advantages in heat aging resistance, UV aging resistance and fire retardant properties.

[0038] Ethyl acetate and n-hexane are used as mixed solvents to dissolve and disperse the complex in the modified stabilizer.

[0039] The combination and interaction of these substances make the prepared insulating cable material have good physical properties, aging resistance and flame retardant properties.

[0040] Compared with the existing technology, it has the following beneficial effects:

[0041] 1) The present invention significantly improves the thermal stability of the material by adding a modified stabilizer, particularly a composite comprising nano-zinc sulfide and bentonite, making it more resistant to performance degradation under long-term high temperatures; 1-(4-isothiocyanate) diacetylene triamine and tris(isopropenyloxy) vinyl silane contained in the modified stabilizer improve the aging resistance of the material and extend the service life of the cable. Through the protective effect of the modified stabilizer, the cable is more adaptable to various environmental conditions, including ultraviolet radiation and high temperature environments.

[0042] 2) The addition of nano-calcium carbonate in the present invention may increase the hardness and rigidity of the material while maintaining a certain toughness, thereby enhancing the mechanical properties of the cable; the addition of silicone flame retardant and p-phenylenediamine improves the flame retardant properties of the material, helping to meet strict safety standards and fire protection requirements; glyceryl tripalerate as a plasticizer improves the processing properties of the material, reduces the melt viscosity, and makes the extrusion process smoother.

[0043] 3) The addition of polyvinyl alcohol and alkyd resin of the present invention may improve the electrical insulation performance of the material and ensure the electrical safety of the cable. DETAILED DESCRIPTION

[0044] Main sources of substances:

[0045] Polyvinyl chloride resin: Shenzhen Donghongjia Technology Co., Ltd., brand: TL-700.

[0046] Polypropylene: Suzhou Lingsu Plastic Technology Co., Ltd., item number: RD368CF.

[0047] Nano calcium carbonate: Hebei Kexu Building Materials Co., Ltd., model: KX-01, particle size: 6250 mesh.

[0048] Alkyd resin: Shenzhen Jitian Chemical Co., Ltd., brand: E1301-6D.

[0049] Polyvinyl alcohol: Xuzhou Hebang Chemical Co., Ltd., model: 2488.

[0050] Silicone flame retardant: Dongguan Xingyuan Chemical Co., Ltd., product model: FR-2010.

[0051] Nano zinc sulfide: Qinghe County Yaoxie Metal Materials Co., Ltd., item number: 867322.

[0052] Bentonite: Shandong Yousuo Chemical Technology Co., Ltd., product number: I93102115.

[0053] 1-(4-Isothiocyanate)diacetylenetriamine: CAS: 102650-30-6.

[0054] Tris(isopropenyloxy)vinylsilane: CAS: 17988-31-7.

[0055] 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol): CAS: 197966-97-5.

[0056] The design idea of ​​the present invention is to prepare an insulating cable material with anti-aging properties. Through a specific formula and process flow, the thermal stability, mechanical properties, flame retardancy and weather resistance of the material are improved, thereby extending the service life of the cable and ensuring its reliability under various environmental conditions.

[0057] PVC resin and polypropylene are pre-mixed in a mixer to ensure uniform mixing of the two polymers, laying the foundation for subsequent processing. Heating the pre-mixed polymers to a molten state at 185°C helps improve mixing efficiency and uniformity.

[0058] Modified stabilizer and nano calcium carbonate are added. The modified stabilizer can improve the thermal stability and light stability of the material and appropriately enhance the flame retardant properties. Nano calcium carbonate, as a filler, can enhance the hardness and rigidity of the material.

[0059] The preparation of the modified stabilizer involves multiple steps such as ultrasonic dispersion, ball milling, and chemical synthesis, which help to form a composite with good dispersibility and stability, ultimately improving the overall performance of the cable material.

[0060] Other additives such as alkyd resin, polyvinyl alcohol, silicone flame retardant, glyceryl tripalerate and paraphenylenediamine are added to improve the material's adhesion, flame retardancy, flexibility and chemical corrosion resistance.

[0061] Plasticizing was carried out by a twin-screw extruder at 200°C to ensure that all components were fully integrated and formed a homogeneous mixture.

[0062] The plasticized mixture is extruded through an extruder and cooled and solidified in water to form the basic shape of the cable.

[0063] The cooled material is pelletized by a pelletizer and dried to obtain insulating cable material pellets suitable for processing and extrusion.

[0064] Example 1

[0065] A method for preparing an anti-aging insulating cable material is as follows, in parts by weight:

[0066] 60 parts of polyvinyl chloride resin and 20 parts of polypropylene are added to a mixer for premixing. The premixed polyvinyl chloride resin and polypropylene are heated at 185° C. to a molten state. 10 parts of a modified stabilizer and 5 parts of nano-calcium carbonate are added and kept mixed to ensure uniform dispersion. After the melt mixing is uniform, 12 parts of an alkyd resin, 8 parts of polyvinyl alcohol, 2 parts of a silicone flame retardant, 2 parts of glycerol tripalerate and 3 parts of p-phenylenediamine are added in sequence and mixed until all components are completely and evenly dispersed. The mixture is placed in a twin-screw extruder for plasticizing at 200° C. The plasticized mixture is extruded through the extruder at an extrusion temperature of 200° C. and a screw speed of 40 rpm. The mixture is cooled and solidified in a water tank. The cooled material is pelletized by a pelletizer, and the pellets are dried at 50° C. to obtain an insulating cable material.

[0067] The preparation method of the modified stabilizer is as follows:

[0068] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0069] S2. Dissolve 3 g of hydroquinone in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0070] Example 2

[0071] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0072] The preparation method of the modified stabilizer is as follows:

[0073] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethylcellulose, and 5 g of triethylenetetraaminehexaacetic acid and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0074] S2. Dissolve 3 g of hydroquinone in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0075] Example 3

[0076] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0077] The preparation method of the modified stabilizer is as follows:

[0078] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of diethylenetriamine pentaacetic acid and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0079] S2. Dissolve 3 g of hydroquinone in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0080] Example 4

[0081] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0082] The preparation method of the modified stabilizer is as follows:

[0083] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt% aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of 6,6-divinyl-2,5,7,10-tetraoxa-6-silicon were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0084] S2. Dissolve 3 g of hydroquinone in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0085] Example 5

[0086] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0087] The preparation method of the modified stabilizer is as follows:

[0088] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of vinyltriethoxysilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0089] S2. Dissolve 3 g of hydroquinone in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0090] Example 6

[0091] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0092] The preparation method of the modified stabilizer is as follows:

[0093] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of vinyl tris(2-methoxyethoxy) silane were added while stirring and dispersing, and the mixture was stirred and mixed for 20 minutes, and then dried at 95° C. to constant weight to obtain a composite;

[0094] S2. Dissolve 3 g of hydroquinone in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0095] Example 7

[0096] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0097] The preparation method of the modified stabilizer is as follows:

[0098] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0099] S2. Dissolve 3 g of 2-cyclopentylphenol in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0100] Example 8

[0101] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0102] The preparation method of the modified stabilizer is as follows:

[0103] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0104] S2. Dissolve 3 g of 2-(1-ethylhexyl)phenol in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azepine diyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0105] Example 9

[0106] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0107] The preparation method of the modified stabilizer is as follows:

[0108] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0109] S2. Dissolve 3 g of octylphenol in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treat for 5 hours, and add to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0110] Example 10

[0111] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0112] The preparation method of the modified stabilizer is as follows:

[0113] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0114] S2, 3g of hydroquinone was dissolved in 20g of anhydrous ethanol, 0.8g of dimethyl sulfate and 2g of 4-(isopropylamino)butanol were added to the dissolved solution, and the mixture was treated for 5 hours. The mixture was added to 100g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane was 3:7; the complex obtained in step S1 was added to the mixed solvent and stirred to disperse; the mixture was then centrifuged at 10000rpm for 5 minutes, washed with anhydrous ethanol, and then dried at 45°C to obtain a modified stabilizer.

[0115] Example 11

[0116] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0117] The preparation method of the modified stabilizer is as follows:

[0118] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0119] S2. Dissolve 3 g of hydroquinone in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of dibutanolamine to the dissolved solution, treat for 5 hours, and add it to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0120] Example 12

[0121] The preparation method of an anti-aging insulating cable material is basically the same as that of Example 1, the only difference being the preparation method of the modified stabilizer.

[0122] The preparation method of the modified stabilizer is as follows:

[0123] S1. 15 g of nano zinc sulfide and 20 g of bentonite were mixed and added to 200 g of 0.8 mol / L nitric acid, and ultrasonically dispersed at a frequency of 20 kHz, a power of 300 W, and a time of 30 minutes. After ultrasonic dispersion, the mixture was washed with water and dried to obtain an acid-treated mixture; the acid-treated mixture was added to a ball mill, and fully ball-milled and mixed, and passed through a 300-mesh sieve to obtain a mixed powder; 20 g of the mixed powder was added to 80 g of a 5 wt % aqueous solution of sodium carboxymethyl cellulose, and 5 g of 1-(4-isothiocyanate) diacetylene triamine and 2 g of tri(isopropenyloxy)vinylsilane were added while stirring and dispersing. After stirring and mixing for 20 minutes, the mixture was dried at 95° C. to constant weight to obtain a composite;

[0124] S2. Dissolve 3 g of hydroquinone in 20 g of anhydrous ethanol, add 0.8 g of dimethyl sulfate and 2 g of 2-butylaminoethanol to the dissolved solution, treat for 5 hours, and add it to 100 g of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 3:7; add the complex obtained in step S1 to the mixed solvent, stir and disperse; then centrifuge at 10,000 rpm for 5 minutes, wash with anhydrous ethanol, and then dry at 45°C to obtain a modified stabilizer.

[0125] Comparative Example 1

[0126] A method for preparing an anti-aging insulating cable material is as follows, in parts by weight:

[0127] 60 parts of polyvinyl chloride resin and 20 parts of polypropylene are added to a mixer for premixing. The premixed polyvinyl chloride resin and polypropylene are heated at 185°C to a molten state, and then 10 parts of a mixture of nano zinc sulfide and bentonite and 5 parts of nano calcium carbonate are added, the mass ratio of nano zinc sulfide to bentonite is 3:4, and the mixing is maintained to ensure uniform dispersion. After the melt mixing is uniform, 12 parts of alkyd resin, 8 parts of polyvinyl alcohol, 2 parts of silicone flame retardant, 2 parts of glycerol tripalerate and 3 parts of p-phenylenediamine are added in sequence, and the mixture is mixed until all components are completely and evenly dispersed. The mixture is placed in a twin-screw extruder for plasticization at 200°C. The plasticized mixture is extruded through the extruder at an extrusion temperature of 200°C and a screw speed of 40 rpm, and is cooled and solidified in a water tank. The cooled material is pelletized by a pelletizer, and the pellets are dried at 50°C to obtain an insulating cable material.

[0128] Comparative Example 2

[0129] A method for preparing an anti-aging insulating cable material is as follows, in parts by weight:

[0130] 60 parts of polyvinyl chloride resin and 20 parts of polypropylene are added to a mixer for premixing. The premixed polyvinyl chloride resin and polypropylene are heated at 185° C. to a molten state. 5 parts of nano-calcium carbonate are added and kept mixed to ensure uniform dispersion. After the melt mixing is uniform, 12 parts of alkyd resin, 8 parts of polyvinyl alcohol, 2 parts of silicone flame retardant, 2 parts of glycerol tripalerate and 3 parts of p-phenylenediamine are added in sequence and mixed until all components are completely and evenly dispersed. The mixture is placed in a twin-screw extruder for plasticization at 200° C. The plasticized mixture is extruded through the extruder at an extrusion temperature of 200° C. and a screw speed of 40 rpm. The mixture is cooled and solidified in a water tank. The cooled material is pelletized by a pelletizer, and the pellets are dried at 50° C. to obtain an insulating cable material.

[0131] Test Example 1

[0132] Anti-aging performance test

[0133] The tensile strength and elongation at break of the insulated cable materials prepared in the examples and comparative examples of the present invention were tested according to the method required by GB / T 1040.3-2006;

[0134] The heat aging test is carried out in accordance with the method required by GB / T2951.12-2008, with an aging temperature of 90±2°C and an aging time of 360h;

[0135] Insulated cable materials were placed in a UV aging chamber for accelerated UV aging testing. The test temperature was 80°C, the light source was a 600W high-pressure mercury lamp, and the distance between the sample and the light source was 20 mm. The irradiation time was 720 hours. The tensile strength and elongation at break of the insulating cable materials were measured before and after irradiation. The test results are shown in Table 1.

[0136] Table 1

[0137]

[0138]

[0139] Test Example 2

[0140] Fire retardant performance test

[0141] The insulating cable materials prepared in the examples of the present invention and the comparative examples were tested according to the method required by GB / T2406.2-2009. The test results are shown in Table 2.

[0142] Table 2

[0143] Experimental plan Limiting oxygen index (%) Example 1 39.2 Example 2 38.1 Example 3 37.9 Example 4 38.3 Example 5 38.0 Example 6 37.8 Example 7 38.8 Example 8 38.5 Example 9 38.6 Example 10 38.5 Example 11 38.4 Example 12 38.4 Comparative Example 1 36.2 Comparative Example 2 33.1

[0144] It can be seen from Test Examples 1 and 2 that the insulating cable material obtained in Example 1 of the present invention has good resistance to heat aging and UV aging, and its fire retardant performance is also further improved.

[0145] In Examples 1 to 3, 1-(4-isothiocyanate) diacetylene triamine performs better than triethylenetetraaminehexaacetic acid and diethylenetriaminepentaacetic acid in terms of heat aging resistance, UV aging resistance, and fire retardant properties. 1-(4-isothiocyanate) diacetylene triamine contains an isothiocyanate group (-N=C=S), which may have higher stability than the functional groups of other amine compounds. The isothiocyanate group may be more stable during thermal degradation, helping to maintain the overall performance of the material. The isothiocyanate group may also have good ultraviolet light absorption ability, thereby protecting the material from damage by ultraviolet rays. During thermal aging and light aging, the material will degrade due to the attack of free radicals. The isothiocyanate group may have a strong free radical capture ability, which can neutralize free radicals through chemical reactions and slow down the aging process. The structure of 1-(4-isothiocyanate) diacetylene triamine may promote the formation of chemical crosslinks with the polymer matrix. This cross-linking can enhance the mechanical properties and heat resistance of the material, thereby improving its anti-aging and flame retardancy. Although triethylenetetraaminehexaacetic acid and diethylenetriaminepentaacetic acid also contain amine groups, their molecular structures may be unstable under high temperature or UV conditions, and their free radical capture ability is poor, thus affecting the thermal stability of the material.

[0146] Compared with Examples 1 and 4 to 6, tri(isopropenyloxy)vinylsilane exhibits superior thermal aging resistance, UV aging resistance, and flame retardancy compared to other silane coupling agents (such as 6,6-divinyl-2,5,7,10-tetraoxa-6-silane, vinyltriethoxysilane, and vinyltri(2-methoxyethoxy)silane). Tri(isopropenyloxy)vinylsilane contains multiple isopropenylsiloxy groups, which may increase the thermal stability of the molecule because these groups decompose at high temperatures. The vinyl groups (double bonds) in this molecule may slow the aging process by capturing free radicals. The structure of tri(isopropenyloxy)vinylsilane may enable it to capture free radicals more effectively. The isopropenyloxy groups can participate in cross-linking reactions, forming a three-dimensional network structure, enhancing the mechanical properties and heat resistance of the material, thereby improving its aging resistance. Furthermore, during the combustion process, a flame-retardant silicon oxide layer may be formed, isolating oxygen and heat, thereby improving the flame retardancy of the material. Silicon-oxygen bonds (Si-O) and carbon-silicon bonds (C-Si) generally have higher bond energies, making silane coupling agents more stable at high temperatures.

[0147] Compared with Example 1 and Examples 7 to 9, hydroquinone performs better in terms of heat aging resistance and UV aging resistance than structurally similar compounds such as 2-cyclopentylphenol, 2-(1-ethylhexyl)phenol, and octylphenol. The phenolic hydroxyl group of hydroquinone has high reactivity and can react with other compounds to form stable derivatives. These derivatives may have better anti-aging properties.

[0148] Example 1 uses 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol), and Examples 7 to 9 use 4-(isopropylamino)butanol, dibutanolamine, and 2-butylaminoethanol, respectively, which perform better in terms of heat aging resistance, UV aging resistance, and fire retardant properties. 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) contains a longer alkyl chain and multiple amino groups, which increases the steric hindrance of the molecule, thereby improving thermal stability. The amino group can capture and neutralize free radicals, slowing down the thermal degradation and photodegradation process of the material. 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) may form chemical crosslinks with other components in the material, improving the mechanical properties and heat resistance of the material. The longer alkyl chain may promote van der Waals forces between molecules and enhance intermolecular stacking, thereby improving the thermal stability of the material and increasing flame retardancy. 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) contains amino and hydroxyl groups and may form a stable complex with the reaction product of hydroquinone and dimethyl sulfate, further improving the thermal stability and flame retardant properties of the modified stabilizer.

[0149] Among them, nano zinc sulfide has excellent light stability and thermal stability, and can also form a complex with bentonite, enhancing the shielding properties of the material and protecting the cable from ultraviolet rays and heat.

Claims

1. A method for preparing an anti-aging insulating cable material, It is characterized in that Here’s how: Add polyvinyl chloride resin and polypropylene into a mixer for premixing, heat the premixed polyvinyl chloride resin and polypropylene to a molten state, add a modified stabilizer and a filler, and keep mixing to ensure uniform dispersion, add alkyd resin, polyvinyl alcohol, silicone flame retardant, plasticizer and antioxidant in sequence after the melt mixing is uniform, mix until all components are completely and evenly dispersed, put the mixture into a twin-screw extruder for plasticization, extrude the plasticized mixture through the extruder, cool and solidify in a water tank, pelletize the cooled material through a pelletizer, dry the pellets to obtain an insulating cable material.

2. The method for preparing the anti-aging insulating cable material according to claim 1, It is characterized in that The weight proportions of the various substances are as follows: 50 to 70 parts of polyvinyl chloride resin and 15 to 25 parts of polypropylene, 8 to 12 parts of modified stabilizer, 4 to 6 parts of filler, 10 to 15 parts of alkyd resin, 5 to 10 parts of polyvinyl alcohol, 1 to 3 parts of silicone flame retardant, 1 to 3 parts of plasticizer and 2 to 4 parts of antioxidant.

3. A method for preparing an anti-aging insulating cable material according to claim 1 or 2, It is characterized in that The filler is at least one of nano calcium carbonate, nano carbon black and silicon dioxide.

4. The method for preparing the anti-aging insulating cable material according to claim 1 or 2, It is characterized in that The plasticizer is at least one of glycerol tripalerate, dioctyl terephthalate, and tricresyl phosphate.

5. The method for preparing the anti-aging insulating cable material according to claim 1 or 2, It is characterized in that The antioxidant is at least one of p-phenylenediamine, didodecyl alcohol ester, didetradecyl alcohol ester, didedecyl alcohol ester, dilauryl thiodipropionate, and lauryl octadecyl thiodipropionate.

6. The method for preparing the anti-aging insulating cable material according to claim 1, It is characterized in that The heating to a molten state is heating to a molten state at 180-190°C.

7. The method for preparing the anti-aging insulating cable material according to claim 1, It is characterized in that The temperature of the plasticizing treatment is 190-210°C.

8. The method for preparing the anti-aging insulating cable material according to claim 1, It is characterized in that The extrusion temperature is 190-210°C, and the screw speed is 20-50 rpm; The temperature of the drying process is 40-60°C.

9. The method for preparing the anti-aging insulating cable material according to claim 1 or 2, It is characterized in that The preparation method of the modified stabilizer is as follows, in parts by weight: S1. Mix 12 to 18 parts of nano zinc sulfide and 18 to 22 parts of bentonite, add them to 180 to 220 parts of 0.5 to 1 mol / L nitric acid, and perform ultrasonic dispersion. The ultrasonic dispersion frequency is 20 to 60 kHz, the power is 200 to 400 W, and the time is 20 to 40 minutes. After ultrasonic dispersion, wash and dry with water to obtain an acid-treated mixture; add the acid-treated mixture to a ball mill, perform sufficient ball milling and mixing, and pass through a 200 to 400 mesh sieve to obtain a mixed powder; add 18 to 22 parts of the mixed powder to 70 to 90 parts of a 4 to 6 wt% aqueous solution of sodium carboxymethyl cellulose, add 4 to 6 parts of 1-(4-isothiocyanate) diacetylene triamine and 1 to 3 parts of tri(isopropenyloxy) vinyl silane while stirring and dispersing, stir and mix for 10 to 30 minutes, and then dry at a temperature of 90 to 100° C. to constant weight to obtain a composite; S2, dissolving 2-4 parts of hydroquinone in 18-22 parts of anhydrous ethanol, adding 0.5-1 parts of dimethyl sulfate and 1-3 parts of 4,4'-((2-aminoethyl)azadiyl)bis(1-butanol) to the dissolved solution, treating for 4-6 hours, adding to 80-120 parts of a pre-mixed mixed solvent of ethyl acetate and n-hexane, wherein the mass ratio of ethyl acetate to n-hexane is 2-4:6-8; adding the complex obtained in step S1 to the mixed solvent, stirring and dispersing; then centrifuging at 8000-12000 rpm for 3-8 minutes, washing with anhydrous ethanol, and then drying at 40-50°C to obtain a modified stabilizer. 10.An anti-aging insulating cable material, It is characterized in that The preparation method is as described in any one of claims 1 to 9.