Preparation method of fluorine-containing rubber for automobile rubber pipe
By using a combination of composite fillers prepared from mica and silicon tetrachloride with silicone rubber and fluorine rubber, the problem of insufficient mechanical strength and heat resistance of fluorine-containing rubber in automotive hoses is solved, significantly improving the performance of the hose and suitable for The high temperature and pressure environment of modern automotive hoses.
Patent Information
- Application Number
- CN202410972715.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
AI Technical Summary
The mechanical strength and heat resistance of fluorine-containing rubber in automobile hoses are not ideal, and it is difficult to meet the requirements of modern automobile hoses for fuel resistance, high temperature resistance and low refrigerant permeability.
A combination of composite fillers including mica and silicon tetrachloride, silicone rubber and fluorine rubber is used to prepare fluorine-containing rubber through an open refining process. Mica and silicon-based materials are used to jointly prepare porous silica materials to improve the mechanical properties and durability of the hose. Thermal performance.
Significantly improves the mechanical properties and heat resistance of fluorine-containing rubber for automotive hoses, making it more suitable for use in high-temperature and high-pressure environments and extending the service life of the hose.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical materials, and in particular to a fluorine-containing rubber for automobile hoses and a preparation method thereof. Background Art
[0002] The rapid development of my country's automobile industry has brought good development opportunities to automobile hose products. With the development of automobiles towards high speed, functionality and comfort, as well as the use of electrical equipment or components such as electronic fuel injection devices and turbochargers to ensure complete fuel combustion, the market potential of automobile hose products continues to increase. In addition, in order to protect the environment, the original refrigerant R12 for automobile air conditioners has been gradually replaced by R134a. The narrowing of automobile engine compartments and the increase in temperature have put forward higher requirements for automobile hoses. Fuel resistance, high temperature resistance, low refrigerant permeability, and long service life have become the mainstream of the development of automobile hoses.
[0003] From the perspective of the rubber layer structure of the hose, in order to achieve the above effects, those skilled in the art are increasingly using multi-layer materials to prepare automotive hoses. For example, a layer of resin and a layer of rubber, or a layer of resin and two layers of rubber, or two layers of different rubber materials, etc. This multi-layer structure has been verified and used in fuel hoses, air conditioning hoses, and turbocharger hoses.
[0004] At present, automobile hoses are usually made of materials such as fluorine-containing rubber, butyl rubber, silicone rubber, epichlorohydrin rubber, hydrogenated nitrile rubber, chlorosulfonated polyethylene rubber, acrylate rubber, EPDM rubber, etc. Taking fuel hoses as an example, with the use of unleaded gasoline and electronic fuel injection devices in automobiles, the mainstream development trend of fuel hoses is to use fluorine-containing rubber, polyamide rubber, epichlorohydrin rubber or acrylate rubber or their composite structure in the inner rubber layer; epichlorohydrin rubber, acrylate rubber or chlorosulfonated polyethylene rubber is generally used to replace chloroprene rubber in the outer rubber layer. In addition, a reinforcement layer is provided between the inner rubber layer and the outer rubber layer, and the reinforcement layer is woven or wound with glass fiber, polyester fiber or nylon fiber.
[0005] Among the above materials, fluorine-containing rubber is a synthetic polymer elastomer containing fluorine atoms on the carbon atoms of the main chain or side chain. Due to the introduction of fluorine atoms, it can give rubber excellent heat resistance, oxidation resistance, oil resistance, corrosion resistance and atmospheric aging resistance. Therefore, fluorine-containing rubber has been widely used in aerospace, aviation, automobile, petroleum and household appliances, and is particularly suitable for automotive hose products such as fuel hoses.
[0006] Although fluororubber, as a synthetic rubber with excellent oil resistance and penetration resistance, is very suitable as an inner layer material that is in direct contact with oil, the mechanical strength and heat resistance of fluororubber are not ideal, which has always been a technical problem that technicians in this field have been committed to solving. Summary of the invention
[0007] One of the problems solved by the present invention is how to provide a fluorine-containing rubber for automobile hoses with better mechanical strength and heat resistance.
[0008] In order to solve at least one of the above problems, the present invention provides a method for preparing fluorine-containing rubber for automobile hoses, the preparation method comprising:
[0009] S100, preparing a composite filler using raw materials including mica and silicon tetrachloride;
[0010] S200, using raw materials including silicone rubber and the composite filler to prepare a first mixture through open refining;
[0011] S300, using raw materials including fluororubber and auxiliary additives to prepare a second mixture through open refining;
[0012] S400, mixing the first mixture and the second mixture to prepare the fluorine-containing rubber.
[0013] In any of the above technical solutions, S200 specifically includes: feeding the silicone oil, the composite filler, the styrene-butadiene rubber and the silicone rubber into an open mixing mill, and after the materials are completely consumed, thinning and sheeting to prepare the first mixture.
[0014] In any of the above technical solutions, the mass ratio of silicone oil:composite filler:styrene-butadiene rubber:silicone rubber=(2-4):(10-25):(20-25):(50-80).
[0015] In any of the above technical solutions, the auxiliary additives include: a compatibilizer, an acid absorber, a vulcanizing agent and a cross-linking agent.
[0016] In any of the above technical solutions, S300 specifically includes:
[0017] The compatibilizer, the vulcanizer, the crosslinking agent and the fluororubber are fed into an open mill, mixed and kneaded uniformly, and then the acid absorber is added, and mixed and kneaded uniformly again to prepare a second mixture.
[0018] In any of the above technical solutions, the mass ratio of compatibilizer: acid absorber: vulcanizing agent: cross-linking agent: fluororubber is (2-4): (2-4): (1-2): (1-2): (60-80).
[0019] In any of the above technical solutions, the compatibilizer includes at least one of the following or a combination thereof: fluororubber grafted vinyl tri-tert-butyl peroxysilane, fluororubber grafted vinyl triethoxysilane, fluororubber grafted γ-methacryloxypropyl trimethoxysilane; and / or the acid absorber includes at least one of the following or a combination thereof: magnesium oxide, calcium oxide; and / or the vulcanizing agent includes at least one of the following or a combination thereof: benzoyl peroxide, diisopropyl peroxide, 2,4-dichlorobenzoyl peroxide; and / or the cross-linking agent includes at least one of the following or a combination thereof: triallyl isocyanurate, triallyl cyanurate.
[0020] In any of the above technical solutions, S100 specifically includes:
[0021] S110, dispersing the mica in a mixture of water and ethanol by ultrasonic at a mass ratio of mica: water: ethanol = (5-10): (25-35): 100 to obtain a mica suspension;
[0022] S120, adding silicon tetrachloride to the mica suspension at a mass ratio of silicon tetrachloride: mica = (2.5-3): 1 and according to the amount of mica added in S110, while stirring simultaneously, adjusting the pH value to 3-5 after the addition is completed and continuing to stir for 1 hour to 1.5 hours to obtain a silica sol containing mica;
[0023] S130. After aging the silica sol in ethanol for 18 to 24 hours, take it out and put it into a vacuum reactor filled with ethanol, and keep it warm and pressurized for 2 hours to 2.5 hours at a temperature of 245°C to 265°C and a pressure of 6.5MPa to 7.5MPa. After the treatment, cool and release the pressure, separate, wash with water, and dry to obtain the composite filler.
[0024] In any of the above technical solutions, S100 specifically further includes:
[0025] S140. According to the mass ratio of urea: kh560 silane coupling agent: composite filler = (2-3): (3-4): 100, the urea, the kh560 silane coupling agent and the composite filler obtained in S140 are fed into a planetary ball mill, and dry-milled for 1 hour to 1.5 hours using zirconium oxide balls as the medium to obtain the modified composite filler.
[0026] The present invention also provides a fluorine-containing rubber for automobile hoses, and the fluorine-containing rubber for automobile hoses is obtained by using the preparation method described in any of the above technical solutions.
[0027] Beneficial Effects
[0028] The present invention provides a method for preparing fluorine-containing rubber for automobile hoses. The method first uses raw materials including silicone rubber and composite fillers to prepare a first mixture through open refining, then uses raw materials including fluorine rubber and auxiliary additives to prepare a second mixture through open refining, and finally mixes the first mixture and the second mixture to prepare fluorine-containing rubber. Among them, the composite filler of the present invention is prepared by using raw materials including mica and silicon tetrachloride. The addition of the composite filler prepared by mica and silicon-based materials makes the fluorine-containing rubber for automobile hoses of the present invention have good mechanical properties and good heat resistance. In addition, the present invention uses silicon tetrachloride as a raw material, and prepares silicon dioxide sol by a sol method by dropping silicon tetrachloride into a water and ethanol suspension containing mica. Then, a porous silica material containing mica is prepared as a composite filler through supercritical reaction. The filler with a porous structure can further improve the heat resistance of the fluorine-containing rubber for automobile hoses. DETAILED DESCRIPTION
[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the specific embodiments of the present invention.
[0030] Unless otherwise specified, the reagents and raw materials used in the present invention can be purchased through commercial channels. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.
[0031] The embodiment of the present invention provides a method for preparing fluorine-containing rubber for automobile hoses, the preparation method comprising:
[0032] S100, preparing a composite filler using raw materials including mica and silicon tetrachloride;
[0033] S200, using raw materials including silicone rubber and the composite filler to prepare a first mixture through open refining;
[0034] S300, using raw materials including fluororubber and auxiliary additives to prepare a second mixture through open refining;
[0035] S400, mixing the first mixture and the second mixture to prepare the fluorine-containing rubber.
[0036] Preferably, the temperature for milling the raw materials including the silicone rubber and the composite filler is 70-90° C. and the time is 5-10 min.
[0037] Preferably, the temperature for refining the raw materials including fluororubber and auxiliary additives is 80-100° C. and the time is 5-10 min.
[0038] Preferably, the first mixture and the second mixture are kneaded at a temperature of 165-175° C. and a time of 15-20 min.
[0039] Specifically, the present invention prepares a composite material of silicone rubber and fluororubber. Fluororubber refers to a synthetic polymer elastomer containing fluorine atoms on the carbon atoms of the main chain or side chain. The introduction of fluorine atoms gives the rubber excellent oil resistance and corrosion resistance. Fluororubber has a high degree of chemical stability and is currently the best medium resistance among all elastomers. Silicone rubber refers to a rubber whose main chain is composed of alternating silicon and oxygen atoms, and the silicon atom is usually connected to two organic groups. This special molecular structure gives silicone rubber unique properties. First of all, silicone rubber itself has good heat resistance, and its cold resistance is also excellent. The cold resistance can be further improved after the introduction of phenyl.
[0040] In some embodiments of the present invention, S200 specifically includes: feeding the silicone oil, the composite filler, the styrene-butadiene rubber and the silicone rubber into an open mixing mill, and after the materials are completely consumed, thinning and sheeting to prepare the first mixture.
[0041] Preferably, the silicone oil used in the present invention is hydroxy silicone oil. The present invention replaces traditional diphenylsilanediol with silicone oil as a structure control agent in silicone rubber processing, thereby improving the processing performance of silicone rubber and making it easier to process into a desired shape and size. In addition, silicone oil also has a certain heat resistance, which can improve the heat resistance of silicone rubber to a certain extent, so that it can still remain stable under high temperature environment. In addition, the present invention uses styrene-butadiene rubber as a modifier and blends it with silicone rubber to improve the tear strength or oil resistance of rubber products.
[0042] In some embodiments of the present invention, the mass ratio of silicone oil:composite filler:styrene-butadiene rubber:silicone rubber=(2-4):(10-25):(20-25):(50-80).
[0043] Preferably, in terms of mass ratio, silicone oil:composite filler:styrene-butadiene rubber:silicone rubber=2:15:23:60.
[0044] In some embodiments of the present invention, the auxiliary additives include: a compatibilizer, an acid absorber, a vulcanizing agent and a crosslinking agent. The compatibilizer helps to improve the fluidity of the rubber, making it easier to flow and process, and good fluidity helps to reduce the difficulty of processing and improve production efficiency. In the vulcanization process of fluororubber, an acid substance, hydrogen fluoride, is generated, which has a significant corrosive effect on the mold. The role of the acid absorber is to absorb hydrogen fluoride to prevent it from causing pollution and damage to the mold. In addition, the acid absorber can not only neutralize hydrogen fluoride, but also promote the vulcanization reaction and increase the vulcanization crosslinking density. This makes the vulcanized fluororubber have better thermal stability and mechanical properties. The vulcanizing agent is a key component in the vulcanization process of fluororubber. It can induce and promote the crosslinking reaction between rubber molecular chains, so that the fluororubber is transformed from a linear structure to a three-dimensional network structure. This transformation significantly improves the physical and mechanical properties of the fluororubber, such as strength, hardness, wear resistance, solvent resistance, etc., thereby giving the fluororubber excellent performance. The cross-linking agent forms chemical bonds between linear fluororubber molecules, connecting these molecules to form a network structure, which significantly improves the hardness and tensile strength of fluororubber. This network structure can effectively disperse stress and prevent the material from breaking when subjected to stress.
[0045] In some embodiments of the present invention, S300 specifically includes: feeding the compatibilizer, the vulcanizer, the crosslinking agent and the fluororubber into an open mill, adding the acid absorber after mixing them evenly, and mixing them evenly again to prepare a second mixture.
[0046] In some embodiments of the present invention, the mass ratio of compatibilizer: acid absorber: vulcanizing agent: cross-linking agent: fluororubber is (2-4): (2-4): (1-2): (1-2): (60-80).
[0047] Preferably, in some embodiments of the present invention, the mass ratio of compatibilizer: acid absorber: vulcanizing agent: cross-linking agent: fluororubber is 2:2:1.5:1.5:80.
[0048] In some embodiments of the present invention, the compatibilizer includes at least one of the following or a combination thereof: fluororubber grafted vinyl tri-tert-butyl peroxysilane, fluororubber grafted vinyl triethoxysilane, and fluororubber grafted γ-methacryloxypropyl trimethoxysilane.
[0049] In some embodiments of the present invention, the acid scavenger includes at least one of the following or a combination thereof: magnesium oxide, calcium oxide.
[0050] In some embodiments of the present invention, the vulcanizing agent includes at least one of the following or a combination thereof: benzoyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide.
[0051] In some embodiments of the present invention, the cross-linking agent includes at least one of the following or a combination thereof: triallyl isocyanurate, triallyl cyanurate.
[0052] In some implementations of the present invention, S100 specifically includes:
[0053] S110, dispersing the mica in a mixture of water and ethanol by ultrasonic at a mass ratio of mica: water: ethanol = (5-10): (25-35): 100 to obtain a mica suspension;
[0054] S120, adding silicon tetrachloride to the mica suspension at a mass ratio of silicon tetrachloride: mica = (2.5-3): 1 and according to the amount of mica added in S110, while stirring simultaneously, adjusting the pH value to 3-5 after the addition is completed and continuing to stir for 1 hour to 1.5 hours to obtain a silica sol containing mica;
[0055] S130. After aging the silica sol in ethanol for 18 to 24 hours, take it out and put it into a vacuum reactor filled with ethanol, and keep it warm and pressurized for 2 hours to 2.5 hours at a temperature of 245°C to 265°C and a pressure of 6.5MPa to 7.5MPa. After the treatment, cool and release the pressure, separate, wash with water, and dry to obtain the composite filler.
[0056] Preferably, in some implementation modes of the present invention, S100 specifically includes:
[0057] S110, dispersing the mica in a mixture of water and ethanol by ultrasonication at a mass ratio of mica: water: ethanol = 5:30:100 to obtain a mica suspension;
[0058] S120, adding silicon tetrachloride to the mica suspension at a mass ratio of silicon tetrachloride: mica = 2.8:1 and according to the amount of mica added in S110, while stirring simultaneously, adjusting the pH value to 4 after the addition is completed and continuing to stir for 1.5 hours to obtain a silica sol containing mica;
[0059] S130, after aging the silica sol in ethanol for 20 hours, take it out and put it into a vacuum reactor filled with ethanol, and keep it warm and pressurized for 2 hours at a temperature of 250° C. and a pressure of 6.7 MPa. After the treatment, cool and release the pressure, separate, wash with water, and dry to obtain the composite filler.
[0060] The reason why the present invention adopts the above steps S110 to S130 to prepare the composite filler is that the present invention is committed to obtaining a composite filler with good mechanical properties and good heat resistance and heat insulation properties, so as to improve the heat resistance and heat insulation properties of fluororubber by adding special composite fillers, making it more suitable for the manufacture of automotive hose products.
[0061] Specifically, because mica has a large diameter-to-thickness ratio, it can form an effective reinforcement network in the rubber, disperse and bear external stress. Therefore, adding mica as a filler to fluororubber can significantly improve the physical and mechanical properties of fluororubber such as tensile strength and tear strength, and the mica itself has good heat insulation and flame retardant effects. However, the disadvantage of mica is that its hexagonal flaky crystal shape makes it difficult to peel off mica, and it is easier to agglomerate than other inorganic non-metallic oxides. The agglomeration and uneven dispersion of fillers in rubber will affect the uniformity of rubber products, as well as the properties of mechanical strength, chemical stability, aging resistance and other aspects. To this end, the present invention provides a filler composited with mica and silicon oxide. Moreover, compared with the method of mechanically mixing mica and silicon oxide directly, the present invention adds powdered mica to a mixture of water and ethanol to prepare a mica suspension, and mixes silicon tetrachloride with the mica suspension, thereby preparing a silica sol in which mica particles are uniformly dispersed, and then the silica sol is aged, and the silica sol is heated and pressurized in ethanol in a supercritical state, in order to obtain a composite filler. This composite filler includes mica and silica, and the mica and silica are uniformly mixed with each other. By mixing nano-scale silica with mica to prepare composite filler particles, the attraction between the mica lamellae structure can be reduced, and its agglomeration is hindered. Therefore, the dispersion performance of the composite filler prepared by the present invention in rubber is better than the dispersion performance of mica particles in rubber. Moreover, the ethanol in a supercritical state can extract the organic matter in the silica sol, so that the surface of the silica particles forms a three-dimensional porous structure without collapse, and this structure helps to improve the heat-resistant and heat-insulating performance of the composite filler.
[0062] In some implementations of the present invention, S100 specifically further includes:
[0063] S140. According to the mass ratio of urea: kh560 silane coupling agent: composite filler = (2-3): (3-4): 100, the urea, the kh560 silane coupling agent and the composite filler obtained in S140 are fed into a planetary ball mill, and dry-milled for 1 hour to 1.5 hours using zirconium oxide balls as the medium to obtain the modified composite filler.
[0064] Preferably, in some implementation modes of the present invention, S100 specifically further includes:
[0065] S140. According to the mass ratio of urea: kh560 silane coupling agent: composite filler = 2.5:4:100, the urea, the kh560 silane coupling agent and the composite filler obtained in S140 are fed into a planetary ball mill, and dry-milled for 1 hour using zirconium oxide balls as the medium to obtain the modified composite filler.
[0066] Mixing urea and KH560 silane coupling agent with the composite filler and dry grinding can help further improve the dispersion performance of the composite filler in rubber.
[0067] Example 1
[0068] This embodiment provides a method for preparing fluorine-containing rubber for automobile hoses, which comprises the following steps:
[0069] S1. According to the mass ratio of mica: water: ethanol = 5:30:100, mica is ultrasonically dispersed in a mixture of water and ethanol to obtain a mica suspension;
[0070] S2, according to the mass ratio of silicon tetrachloride: mica = 2.8:1, according to the amount of mica added in S1, silicon tetrachloride is added to the mica suspension and stirred simultaneously, after the addition is completed, the pH value is adjusted to 4 and stirring is continued for 1.5 hours to obtain a silica sol containing mica;
[0071] S3, soaking the silica sol in ethanol and aging it for 20 hours, taking it out and sending it into a vacuum reactor filled with ethanol, keeping it warm and pressurized for 2 hours at a temperature of 250° C. and a pressure of 6.7 MPa, cooling and releasing the pressure after the treatment, separating, washing with water, and drying to obtain a composite filler;
[0072] S4, according to the mass ratio of urea: kh560 silane coupling agent: composite filler = 2.5:4:100, the composite filler obtained by urea, kh560 silane coupling agent and S140 was sent to a planetary ball mill, and dry-milled for 1 hour using zirconium oxide balls as the medium to obtain a modified composite filler;
[0073] S5. According to the mass ratio of silicone oil: composite filler: styrene-butadiene rubber: silicone rubber = 2:15:23:60, silicone oil, composite filler, styrene-butadiene rubber and silicone rubber are fed into an open mill. After the materials are completely eaten, thin-pass and sheeting are performed to prepare a first mixture. The open milling temperature is 80° C. and the time is 10 min.
[0074] S6. According to the mass ratio of fluororubber-grafted vinyl triethoxysilane compatibilizer: calcium oxide acid absorber: benzoyl peroxide vulcanizer: triallyl isocyanurate crosslinker: fluororubber = 2:2:1.5:1.5:80, the compatibilizer, vulcanizer, crosslinker and fluororubber are fed into an open mill, the acid absorber is added after mixing evenly, and the mixture is mixed evenly again to prepare a second mixture; the temperature of the open mill is 90° C. and the time is 10 min;
[0075] S7, mixing the first mixture and the second mixture to prepare a fluorine-containing rubber; the mixing temperature is 170° C. and the time is 15 minutes.
[0076] The physical and chemical properties of the fluorine-containing rubber obtained in Example 1 were tested according to GB / T 528-1998, GB / T 529-1999, GB / T 531-1998, and GB / T 3512-2001, and some of the test results are shown as follows: the hot air aging condition is 200°C×72; the tensile strength before the hot air aging test is 9.1 MPa, and the elongation at break is 423%; the tensile strength after the hot air aging test is 8.7 MPa, and the elongation at break is 401%.
[0077] Example 2
[0078] This embodiment provides a method for preparing fluorine-containing rubber for automobile hoses, which comprises the following steps:
[0079] S1. According to the mass ratio of mica: water: ethanol = 5:30:100, mica is ultrasonically dispersed in a mixture of water and ethanol to obtain a mica suspension;
[0080] S2, according to the mass ratio of silicon tetrachloride: mica = 2.8:1, according to the amount of mica added in S1, silicon tetrachloride is added to the mica suspension and stirred simultaneously, after the addition is completed, the pH value is adjusted to 4 and stirring is continued for 1.5 hours to obtain a silica sol containing mica;
[0081] S3, soaking the silica sol in ethanol and aging it for 20 hours, taking it out and sending it into a vacuum reactor filled with ethanol, keeping it warm and pressurized for 2 hours at a temperature of 250° C. and a pressure of 6.7 MPa, cooling and releasing the pressure after the treatment, separating, washing with water, and drying to obtain a composite filler;
[0082] S4. According to the mass ratio of silicone oil: composite filler: styrene-butadiene rubber: silicone rubber = 2:15:23:60, silicone oil, composite filler, styrene-butadiene rubber and silicone rubber are fed into an open mill. After the materials are completely fed, thin-pass and sheeting are performed to prepare a first mixture. The open milling temperature is 80° C. and the time is 10 min.
[0083] S5. According to the mass ratio of fluororubber-grafted vinyl triethoxysilane compatibilizer: calcium oxide acid absorber: benzoyl peroxide vulcanizer: triallyl isocyanurate crosslinker: fluororubber = 2:2:1.5:1.5:80, the compatibilizer, vulcanizer, crosslinker and fluororubber are fed into an open mill, the acid absorber is added after mixing evenly, and the mixture is mixed evenly again to prepare a second mixture; the temperature of the open mill is 90° C. and the time is 10 min;
[0084] S6. Mix the first mixture and the second mixture to prepare a fluorine-containing rubber; the mixing temperature is 170° C. and the mixing time is 15 minutes.
[0085] According to the same standard, the physical and chemical properties of the fluorine-containing rubber obtained in Example 2 were tested, and some of the test results are shown as follows: the hot air aging conditions are 200°C×72; the tensile strength before the hot air aging experiment is 8.8MPa, and the elongation at break is 412%; the tensile strength after the hot air aging experiment is 8.3MPa, and the elongation at break is 389%.
[0086] Example 3
[0087] This embodiment provides a method for preparing fluorine-containing rubber for automobile hoses, which comprises the following steps:
[0088] S1. According to the mass ratio of silicone oil: mica: silicon dioxide: styrene-butadiene rubber: silicone rubber = 2:6:9:23:60, silicone oil, mica, silicon dioxide, styrene-butadiene rubber and silicone rubber are fed into an open mill. After the materials are completely eaten, thin-pass and sheet-form to prepare a first mixture; the opening temperature is 80° C. and the time is 10 min;
[0089] S5. According to the mass ratio of fluororubber-grafted vinyl triethoxysilane compatibilizer: calcium oxide acid absorber: benzoyl peroxide vulcanizer: triallyl isocyanurate crosslinker: fluororubber = 2:2:1.5:1.5:80, the compatibilizer, vulcanizer, crosslinker and fluororubber are fed into an open mill, the acid absorber is added after mixing evenly, and the mixture is mixed evenly again to prepare a second mixture; the temperature of the open mill is 90° C. and the time is 10 min;
[0090] S6. Mix the first mixture and the second mixture to prepare a fluorine-containing rubber; the mixing temperature is 170° C. and the mixing time is 15 minutes.
[0091] According to the same standard, the physical and chemical properties of the fluorine-containing rubber obtained in Example 3 were tested, and some of the test results are shown as follows: the hot air aging conditions are 200°C×72; the tensile strength before the hot air aging experiment is 8.1 MPa, and the elongation at break is 401%; the tensile strength after the hot air aging experiment is 7.9 MPa, and the elongation at break is 372%.
Claims
1. A method for preparing fluorine-containing rubber for automobile hoses, characterized in that: The preparation method comprises: S100, preparing a composite filler using raw materials including mica and silicon tetrachloride; S200, using raw materials including silicone rubber and the composite filler to prepare a first mixture through open refining; S300, using raw materials including fluororubber and auxiliary additives to prepare a second mixture through open refining; S400, mixing the first mixture and the second mixture to prepare the fluorine-containing rubber.
2. The preparation method according to claim 1, characterized in that: S200 specifically includes: The silicone oil, the composite filler, the styrene-butadiene rubber and the silicone rubber are fed into an open mixing mill, and after the materials are completely consumed, thin-passed and sheeted to prepare the first mixture.
3. The preparation method according to claim 2, characterized in that: Calculated by mass ratio, silicone oil: composite filler: styrene-butadiene rubber: silicone rubber = (2-4): (10-25): (20-25): (50-80).
4. The preparation method according to claim 1, characterized in that: The auxiliary additives include: a compatibilizer, an acid absorber, a vulcanizing agent and a cross-linking agent.
5. The preparation method according to claim 4, characterized in that: S300 specifically includes: The compatibilizer, the vulcanizer, the crosslinking agent and the fluororubber are fed into an open mill, mixed and kneaded uniformly, and then the acid absorber is added, and mixed and kneaded uniformly again to prepare a second mixture.
6. The preparation method according to claim 5, characterized in that: In terms of mass ratio, compatibilizer: acid absorber: vulcanizing agent: cross-linking agent: fluororubber = (2-4): (2-4): (1-2): (1-2): (60-80).
7. The preparation method according to claim 5, characterized in that: The compatibilizer comprises at least one of the following or a combination thereof: fluororubber grafted vinyl tri-tert-butyl peroxysilane, fluororubber grafted vinyl triethoxysilane, fluororubber grafted γ-methacryloxypropyl trimethoxysilane; and / or The acid absorbent comprises at least one of the following or a combination thereof: magnesium oxide, calcium oxide; and / or The vulcanizing agent comprises at least one of the following or a combination thereof: benzoyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide; and / or The cross-linking agent includes at least one of the following or a combination thereof: triallyl isocyanurate, triallyl cyanurate.
8. The preparation method according to any one of claims 1 to 7, characterized in that S100 specifically includes: S110, dispersing the mica in a mixture of water and ethanol by ultrasonic at a mass ratio of mica: water: ethanol = (5-10): (25-35): 100 to obtain a mica suspension; S120, adding silicon tetrachloride to the mica suspension at a mass ratio of silicon tetrachloride: mica = (2.5-3): 1 and according to the amount of mica added in S110, while stirring simultaneously, adjusting the pH value to 3-5 after the addition is completed and continuing to stir for 1 hour to 1.5 hours to obtain a silica sol containing mica; S130. After aging the silica sol in ethanol for 18 to 24 hours, take it out and put it into a vacuum reactor filled with ethanol, and keep it warm and pressurized for 2 hours to 2.5 hours at a temperature of 245°C to 265°C and a pressure of 6.5MPa to 7.5MPa. After the treatment, cool and release the pressure, separate, wash with water, and dry to obtain the composite filler.
9. The preparation method according to claim 8, characterized in that: S100 also includes: S140. According to the mass ratio of urea: kh560 silane coupling agent: composite filler = (2-3): (3-4): 100, the urea, the kh560 silane coupling agent and the composite filler obtained in S140 are fed into a planetary ball mill, and dry-milled for 1 hour to 1.5 hours using zirconium oxide balls as the medium to obtain the modified composite filler.
10. A fluorine-containing rubber for automobile hose, characterized in that: The fluorine-containing rubber for automobile hose is obtained by the preparation method according to any one of claims 1 to 9.