Preparation method of nylon carbon nanotube composite material and nylon carbon nanotube composite material with enhanced mechanical property
By introducing amino groups to the surface of multi-walled carbon nanotubes and vacuum drying, airgel powder is formed, which solves the problem of interfacial bonding force and dispersion between multi-walled carbon nanotubes and nylon 66 materials, and significantly improves the mechanics of the composite material. performance.
Patent Information
- Application Number
- CN202410947497.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
AI Technical Summary
Existing technology is difficult to effectively improve the interface bonding force and dispersion between multi-walled carbon nanotubes and nylon 66 materials, resulting in insufficient mechanical properties of composite materials.
Amino groups are introduced on the surface of hydroxylated multi-walled carbon nanotubes, and then airflow pulverized after vacuum drying to form airgel powder, which is evenly dispersed in combination with non-thickening surfactants to improve the bonding strength between carbon nanotubes and nylon 66 resin. Dispersion during blending and extrusion.
Significantly improves the mechanical properties of multi-walled carbon nanotubes and nylon 66 composite materials, with the tensile strength increased by 10%-30% and the bending strength increased by 9%-22%. Especially after adding glass fiber, the mechanical properties of the composite materials are further enhanced. .
Smart Images

Figure CN118725561A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nylon materials and carbon nanotube materials, and in particular relates to a preparation method of a nylon carbon nanotube composite material and a nylon carbon nanotube composite material with enhanced mechanical properties. Background Art
[0002] Nylon 66, whose scientific name is polyhexamethylene adipamide, is a widely used thermoplastic engineering resin. It is industrially polycondensed from adipic acid and hexamethylenediamine. Due to the presence of amide bonds, it has high mechanical strength and hardness. In the field of engineering plastics, it can replace metal as machine housings, bearings, impeller blades, etc. In addition, nylon 66 is reinforced by adding glass fibers. The glass fibers include short glass fibers and long glass fibers. The length of the short glass fibers is in the range of 0.01mm-3mm, and the length of the long glass fibers is in the range of 3mm-50mm. For example, the tensile strength of unreinforced nylon 66 is 60MPa-80MPa, and the flexural strength is 120MPa-140MPa. After being reinforced with short glass fibers accounting for 30% of the mass of nylon 66, the tensile strength is in the range of 170MPa-190MPa, and the flexural strength is 250MPa-270MPa.
[0003] Multi-walled carbon nanotubes (MWCNTs) are a type of carbon nanotubes. Figure 1 As shown in the figure, multi-walled carbon nanotubes can be regarded as curled up multi-layer single-walled carbon nanotubes, in which the carbon-carbon bonds are similar to a sp 2 Hybrid structure, so that it has excellent mechanical properties and electrical properties. With the maturity of fluidized bed CVD preparation of multi-walled carbon nanotubes in recent years, industrial mass production has made the cost of multi-walled carbon nanotubes continue to decrease. Therefore, this one-dimensional special nanomaterial is no longer limited to laboratory applications, and has become a hot product in the field of new materials. In recent years, it has been mainly used in lithium batteries, polymers and other fields. However, due to the strong van der Waals force between tubes, multi-walled carbon nanotubes are mostly presented in the form of array agglomeration. In the actual use process, it is necessary to disperse the multi-walled carbon nanotubes as much as possible into a single state, so as to maximize the characteristics of carbon nanomaterials. Especially in the process of blending and modification with polymer resins, the performance of the final product often depends on the dispersion state of carbon nanotubes. At present, there are physical dispersion methods and chemical dispersion methods for carbon nanotubes. The physical dispersion methods mainly include ball milling, sand milling, ultrasound, fluid shearing, etc., and the chemical dispersion methods mainly include adding surfactants, strong acid oxidation, electrochemical oxidation, etc. In addition, the surface of carbon nanotubes presents a π-π conjugated structure similar to that of graphite layers, which makes the van der Waals force between the tubes very large, easy to agglomerate, and the interfacial interaction with polar polymer resins such as nylon 66 is not strong. Therefore, it is necessary to modify the surface of multi-walled carbon nanotubes and add polar groups to improve the interface properties between carbon nanotubes and resins, thereby improving the mechanical properties of the products. Summary of the invention
[0004] The invention provides a method for preparing a nylon carbon nanotube composite material, which can not only improve the interface bonding force between the carbon nanotube and the nylon material, but also improve the dispersibility of the multi-walled carbon nanotube, which is beneficial to the high mechanical properties of the composite material.
[0005] The technical solution of the present invention is: a method for preparing a nylon carbon nanotube composite material, comprising the following steps:
[0006] (1) Surface modification of multi-walled carbon nanotubes
[0007] A silanization solution is used, wherein the silanization solution is a solution obtained by dissolving KH550 in an alcohol solvent, and the chemical structural formula of KH550 is:
[0008]
[0009] placing hydroxylated multi-walled carbon nanotubes (MWCNT-OH) in the silanization solution, condensing hydroxyl groups in the hydroxylated multi-walled carbon nanotubes with hydroxyl groups in the silanization solution, and introducing amino groups (-NH2) into the surface of the hydroxylated multi-walled carbon nanotubes;
[0010] (2) Multi-walled carbon nanotube dispersion
[0011] The multi-walled carbon nanotubes obtained in step (1) are dissolved in a solvent to prepare a suspension, and then a non-thickening surfactant is added to uniformly disperse the suspension to obtain a multi-walled carbon nanotube slurry;
[0012] (3) Preparation of multi-walled carbon nanotube aerogel
[0013] The multi-walled carbon nanotube slurry obtained in step (2) is filtered and vacuum dried to obtain carbon powder, which is then air flow crushed to obtain multi-walled carbon nanotube aerogel powder;
[0014] (4) Blending extrusion
[0015] The multi-walled carbon nanotube aerogel powder obtained in step (3) is blended and extruded with PA66 resin to obtain a nylon carbon nanotube composite material (PA66 / MWCNT), wherein the mass of the PA66 resin in the mixture is 100 parts, and the mass of the multi-walled carbon nanotube aerogel powder is 0.1 part to 1.0 part.
[0016] In the step (1), the hydroxylated multi-walled carbon nanotubes refer to multi-walled carbon nanotubes with hydroxyl groups. The hydroxylated multi-walled carbon nanotubes can be homemade or commercially available, and the preparation method is not limited.
[0017] In step (1), the alcohol solvent is not limited and includes one or more of methanol, ethanol, isopropanol, etc.
[0018] In the step (1), preferably, in terms of weight percentage, KH550 accounts for 10-20 parts and the alcohol solvent accounts for 85-95 parts in the silanization solution.
[0019] In the step (1), preferably, the silanization solution includes an acid, preferably the acid accounts for 0.5 parts to 5 parts by weight; the acid is not limited, and includes one or more of HCl (hydrochloric acid), HAc (acetic acid), H2SO4 (sulfuric acid), etc.
[0020] In the step (1), preferably, the silanization solution includes deionized water, preferably the deionized water accounts for 1 part to 10 parts by weight.
[0021] In the step (1), preferably, the temperature of the silanization solution is 15° C.-25° C., and further preferably, the hydroxylated multi-walled carbon nanotubes are placed in the silanization solution for 30 min-120 min.
[0022] In the step (1), preferably, after amino groups are introduced into the surface of the hydroxylated multi-walled carbon nanotubes, the tubes are taken out and washed with deionized water.
[0023] In the step (2), preferably, the solvent includes water or low-boiling alcohols, and the low-boiling alcohols include but are not limited to one or more of acetone, ether, methanol, ethanol, isopropanol, etc.
[0024] In the step (2), preferably, the carbon nanotubes are dissolved in a solvent to prepare a suspension with a mass percentage concentration of 0.1%-1%. More preferably, the carbon nanotubes are dissolved in a solvent to prepare a suspension with a mass percentage concentration of 0.3%-1%.
[0025] In the step (2), the non-thickening surfactant is not limited, and includes one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, dodecyltrimethylammonium bromide, didodecyldimethylammonium bromide, dioctadecyldimethylammonium bromide, hexadecyltrimethylammonium bromide, sodium lignin sulfonate, alkali lignin, sodium dodecyl sulfate, etc.
[0026] In the step (2), preferably, the mass of the non-thickening surfactant accounts for 10%-50% of the mass of the multi-walled carbon nanotubes.
[0027] In the step (2), preferably, the dispersion method is homogeneous dispersion. Further preferably, the pressure during the homogeneous dispersion is 5000psi-30000psi, and the number of cycles is 2-4 times.
[0028] In the step (3), preferably, the vacuum drying temperature is 80°C-150°C.
[0029] In the step (3), preferably, the vacuum drying time is 30 min-120 min.
[0030] In the step (3), preferably, the powder is crushed in a jet mill.
[0031] In the step (4), preferably, the weight of the multi-walled carbon nanotube aerogel powder in the blend is 0.1 part to 0.5 part, and more preferably 0.2 part to 0.4 part.
[0032] In the step (4), the blend preferably further comprises a dehydrating agent, and the weight of the dehydrating agent is preferably 0.5 to 2 parts. The dehydrating agent is not limited, and includes one or more of DDC (dicyclohexylcarbodiimide), DIC (N,N'-diisopropylcarbodiimide), EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride), etc.
[0033] In the step (4), preferably, a twin-screw extruder is used for blending and extrusion, and the rotation speed of the twin-screw extruder is preferably 150 rpm-220 rpm.
[0034] In the step (4), preferably, the temperature of the co-extrusion from the feed port to the discharge port is controlled in the range of 200°C-300°C.
[0035] In the step (4), preferably, multiple temperature control zones are set from the feed port to the die head for the co-extrusion, for example, six temperature control zones are set, which are 225°C, 235°C, 250°C, 260°C, 255°C, and 250°C, respectively.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The present invention uses KH550 to modify MWCNT-OH. KH550 is hydrolyzed in an alcohol solvent to form R-Si-OH, where R represents an alkyl group connected to Si (NH2-CH2-CH2-CH2-). The hydroxyl group condenses with the hydroxyl group in MWCNT-OH, thereby introducing the -NH2 group into the MWCNT surface, which can improve the interfacial bonding force between carbon nanotubes and nylon 66.
[0038] (2) The present invention disperses multi-walled carbon nanotubes in a solvent to obtain a multi-walled carbon nanotube slurry, and adopts vacuum drying and air flow pulverization to prepare a powder; vacuum drying is because multi-walled carbon nanotubes will form microscopic aggregates again when dried under general non-vacuum conditions. If the multi-walled carbon nanotubes are blended and extruded in the state of microscopic aggregates, the shearing effect of the extruder is insufficient to destroy the aggregated state of the multi-walled carbon nanotubes. In the vacuum drying process, the surface tension of the solvent is close to that of the gas state, so a microscopic network structure is formed, such as Figure 5As shown, the original dispersibility can be maintained during the blending process with the resin, thereby avoiding re-agglomeration during the drying process and greatly improving the dispersion during the powder making process; the purpose of air flow milling is to break up the macroscopic multi-walled carbon nanotube agglomerates formed after drying into an aerogel powder state that is easy to blend and disperse;
[0039] (3) The PA66 / MWCNT composite material obtained by the present invention can enhance the mechanical properties of the composite material after being blended with glass fibers, wherein the glass fibers include short glass fibers and long glass fibers, preferably short glass fibers, and the mass of the short glass fibers preferably accounts for 20-40% of the mass of the nylon carbon nanotube composite material, and more preferably 30%;
[0040] When the mass of the short glass fibers accounts for 30% of the mass of the nylon carbon nanotube composite material, as a comparison, the PA66 and the short glass fibers are blended to obtain PA66 with enhanced mechanical properties, and the mass of the short glass fibers accounts for 30% of the mass of the PA66; compared with the PA66 with enhanced mechanical properties, the mechanical properties of the PA66 / MWCNT composite material with enhanced mechanical properties are greatly improved. When the mass of the short glass fibers accounts for 30% of the mass of the PA66, and the mass of the multi-walled carbon nanotube aerogel powder in the blend is 0.1-0.5 parts, that is, when the mass of the multi-walled carbon nanotube aerogel powder accounts for 0.1%-0.5% of the mass of PA66, the tensile strength is increased by 10%-30%, and the flexural strength is increased by 9%-22%, especially when the mass of the carbon nanotube aerogel powder is controlled to account for 0.2%-0.4% of the mass of PA66, the tensile strength is increased by 20%-30%, and the flexural strength is increased by 14%-22%. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is a schematic diagram of the structure of a multi-walled carbon nanotube.
[0042] Figure 2 This is a dispersion diagram of multi-walled carbon nanotubes in the blend of Comparative Example 1.
[0043] Figure 3 This is a processing flow chart in Example 1.
[0044] Figure 4 This is a dispersion diagram of multi-walled carbon nanotubes in aerogel state after drying under non-vacuum conditions in Comparative Example 3.
[0045] Figure 5 This is a dispersion diagram of multi-walled carbon nanotubes in an aerogel state after vacuum drying in Example 1. DETAILED DESCRIPTION
[0046] The present invention is further described in detail below in conjunction with embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention, and some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.
[0047] The PA66 in the following comparative examples 1-3 and examples 1-5 has the same source and the same performance.
[0048] Comparative Example 1:
[0049] The PA66 / MWCNT composite material was obtained by blending and extruding commercially available MWCNT and PA66 in a twin-screw extruder.
[0050] The components and mass ratios of the blend are: 0.3 parts of MWCNT, 100 parts of PA66 resin, and 1 part of DDC dehydrating agent.
[0051] Multi-walled carbon nanotubes in the blend Figure 2 Shown as agglomerate.
[0052] The process parameters of the twin-screw extruder during extrusion operation are: the rotation speed is 180 rpm, and the temperature control of the six zones from the feed port to the die head are 225°C, 235°C, 250°C, 260°C, 255°C, and 250°C respectively.
[0053] Comparative Example 2:
[0054] (1) Carbon nanotube dispersion
[0055] Commercially available MWCNT-OH (hydroxylated multi-walled carbon nanotubes) were used as raw materials, which were prepared into a 0.5wt% suspension with water, and then a non-thickening surfactant, sodium dodecyl sulfate, which accounted for 30% of the mass of the hydroxylated multi-walled carbon nanotubes, was added; the prepared carbon nanotube suspension was added to a homogenizer for homogenization at a homogenization pressure of 8000psi and a cycle number of 3 times to obtain a multi-walled carbon nanotube slurry.
[0056] (2) Preparation of multi-walled carbon nanotube aerogel
[0057] The multi-walled carbon nanotube slurry prepared in step (1) was filtered, and then vacuum dried at 110° C. for 60 min. Finally, the obtained carbon powder was crushed in a jet mill to obtain an easily processable MWCNT aerogel powder.
[0058] (3) Blending extrusion
[0059] The MWCNT aerogel powder obtained in step (2) is mixed and extruded with PA66 in a twin-screw extruder to obtain a PA66 / MWCNT composite material;
[0060] The materials and mass ratios of the components of the blend are: 0.3 parts of MWCNT aerogel powder, 100 parts of PA66 resin, and 1 part of DDC dehydrating agent;
[0061] The twin-screw extruder in Comparative Example 1 was used, and the extrusion process parameters were controlled to be the same as those in the extrusion operation of Comparative Example 1.
[0062] Comparative Example 3:
[0063] (1) Surface modification of carbon nanotubes
[0064] The raw material MWCNT-OH in Comparative Example 2 was used, immersed in a silanization solution at 25° C. for 60 min, and then washed with deionized water;
[0065] The components and mass fractions of the silanization solution are as follows:
[0066] 15 parts of KH550 reagent, 85 parts of ethanol solvent, 2 parts of sulfuric acid reagent, and 4 parts of DI (deionized water).
[0067] The method for preparing the silanization solution is not limited, and the solution may be prepared by adding KH550 reagent, sulfuric acid reagent and DI into an ethanol solvent respectively and mixing and stirring the mixture evenly.
[0068] (2) Carbon nanotube dispersion
[0069] The modified multi-walled carbon nanotubes obtained in step (1) are dissolved in water to prepare a suspension of multi-walled carbon nanotubes accounting for 0.5wt%, and then a non-thickening surfactant sodium dodecyl sulfate is added, the mass of which is 30% of the mass of the multi-walled carbon nanotubes. The prepared carbon nanotube suspension is added to a homogenizer for homogenization at a homogenization pressure of 8000psi and a cycle number of 3 times to finally obtain a multi-walled carbon nanotube slurry.
[0070] (3) Preparation of carbon nanotube aerogel
[0071] The multi-walled carbon nanotube slurry prepared in step (2) was filtered and then dried at 110° C. under non-vacuum conditions for 60 min. The morphology of the multi-walled carbon nanotubes was as follows: Figure 4 As shown, it is shown that the carbon nanotubes re-agglomerate during the drying process, and finally the obtained carbon powder is crushed in a jet mill to obtain MWCNT powder that is easy to process.
[0072] (4) Blending extrusion
[0073] The MWCNT powder obtained in step (3) is mixed and extruded with PA66 in a twin-screw extruder to obtain a PA66 / MWCNT composite material;
[0074] The materials and mass ratios of the components in the blend are: 0.3 parts of MWCNT aerogel powder, 100 parts of PA66 resin, and 1 part of DDC dehydrating agent;
[0075] The twin-screw extruder in Comparative Example 1 was used, and the extrusion process parameters were controlled to be the same as those in the extrusion operation of Comparative Example 1.
[0076] Embodiment 1:
[0077] In this embodiment, the processing flow is as follows: Figure 3 As shown, the details are as follows.
[0078] (1) The same as step (1) in Comparative Example 3;
[0079] (2) The same as step (2) in Comparative Example 3;
[0080] (3) The multi-walled carbon nanotube slurry prepared in step (2) was filtered and then vacuum dried at 110° C. for 60 min. The morphology of the multi-walled carbon nanotubes was as follows: Figure 5 As shown, it is shown that during the drying process, the carbon nanotubes present a microscopic network structure without agglomeration. Finally, the obtained carbon powder is crushed in a jet mill to obtain MWCNT powder that is easy to process;
[0081] (4) blending the MWCNT powder obtained in step (3) with PA66 in a twin-screw extruder to obtain a PA66 / MWCNT composite material;
[0082] The materials and proportions of the components of the blend are: 0.1 parts of MWCNT aerogel powder, 100 parts of PA66 resin, and 1 part of DDC dehydrating agent;
[0083] The twin-screw extruder in Comparative Example 1 was used, and the extrusion process parameters were controlled to be the same as those in the extrusion operation of Comparative Example 1.
[0084] Embodiment 2:
[0085] (1) The same as step (1) in Example 1;
[0086] (2) The same as step (2) in Example 1;
[0087] (3) The same as step (3) in Example 1;
[0088] (4) blending the MWCNT powder obtained in step (3) with PA66 in a twin-screw extruder to obtain a PA66 / MWCNT composite material;
[0089] The materials and proportions of the components of the blend are: 0.2 parts of MWCNT aerogel powder, 100 parts of PA66 resin, and 1 part of DDC dehydrating agent;
[0090] The twin-screw extruder in Comparative Example 1 was used, and the extrusion process parameters were controlled to be the same as those in the extrusion operation of Comparative Example 1.
[0091] Embodiment 3:
[0092] (1) The same as step (1) in Example 1;
[0093] (2) The same as step (2) in Example 1;
[0094] (3) The same as step (3) in Example 1;
[0095] (4) blending the MWCNT powder obtained in step (3) with PA66 in a twin-screw extruder to obtain a PA66 / MWCNT composite material;
[0096] The materials and proportions of the components of the blend are: 0.3 parts of MWCNT aerogel powder, 100 parts of PA66 resin, and 1 part of DDC dehydrating agent;
[0097] The twin-screw extruder in Comparative Example 1 was used, and the extrusion process parameters were controlled to be the same as those in the extrusion operation of Comparative Example 1.
[0098] Embodiment 4:
[0099] (1) The same as step (1) in Example 1;
[0100] (2) The same as step (2) in Example 1;
[0101] (3) The same as step (3) in Example 1;
[0102] (4) blending the MWCNT powder obtained in step (3) with PA66 in a twin-screw extruder to obtain a PA66 / MWCNT composite material;
[0103] The materials and proportions of the components of the blend are: 0.4 parts of MWCNT aerogel powder, 100 parts of PA66 resin, and 1 part of DDC dehydrating agent;
[0104] The twin-screw extruder in Comparative Example 1 was used, and the extrusion process parameters were controlled to be the same as those in the extrusion operation of Comparative Example 1.
[0105] Embodiment 5:
[0106] (1) The same as step (1) in Example 1;
[0107] (2) The same as step (2) in Example 1;
[0108] (3) The same as step (3) in Example 1;
[0109] (4) blending the MWCNT powder obtained in step (3) with PA66 in a twin-screw extruder to obtain a PA66 / MWCNT composite material;
[0110] The materials and proportions of the components of the blend are: 0.5 parts of MWCNT aerogel powder, 100 parts of PA66 resin, and 1 part of DDC dehydrating agent;
[0111] The twin-screw extruder in Comparative Example 1 was used, and the extrusion process parameters were controlled to be the same as those in the extrusion operation of Comparative Example 1.
[0112] The PA66 / MWCNT composite materials obtained in the above comparative examples 1-3 and examples 1-5 were respectively blended and modified with short glass fibers (i.e., short glass fibers) having a length of 0.8 mm to 1.2 mm, as follows:
[0113] The components and their mass ratios are: 70 parts of PA66 / MWCNT, 30 parts of short glass fiber, 3 parts of compatibilizer POE-g-MAH, and 2 parts of lubricant polyethylene wax. A twin-screw extruder is used for extrusion granulation, and then the plastic particles are injection molded into dumbbell splines and rectangular splines by an injection molding machine, and tensile and bending tests are performed using a universal testing machine. For comparison, the pure PA66 used in Comparative Examples 1-3 and Examples 1-5 is used to replace the PA66 / MWCNT composite materials and short glass fibers obtained in the above Comparative Examples 1-3 and Examples 1-5 to perform the above blending modification as a blank test. The specific test results are as follows:
[0114] Table 1: Mechanical test results corresponding to Comparative Examples 1-3 and Examples 1-3
[0115]
[0116] From the mechanical test results, the following conclusions can be drawn:
[0117] 1. In Comparative Example 1, adding unmodified and undispersed multi-walled carbon nanotubes to PA66 did not improve the mechanical properties of PA66 / glass fiber. Instead, the tensile strength and bending strength decreased slightly, indicating that the agglomerated carbon nanotubes not only failed to improve the performance of the original material, but also reduced the performance of the material;
[0118] 2. In Comparative Example 2, MWCNT-OH is used and formed into an aerogel form after treatment. Compared with the agglomerated original carbon nanotubes, the performance is greatly improved, but the improvement is not large when referring to the original PA66 / glass fiber material, indicating that the interface performance between MWCNT-OH and PA66 needs to be further improved;
[0119] 3. Comparative Example 3: Although the amino group was introduced into MWCNT-OH to improve the interface performance between MWCNT-OH and PA66, Figure 4 As shown in the figure, due to the reagglomeration of carbon nanotubes during the drying process, the improvement of the mechanical properties of the PA66 / glass fiber original material is limited.
[0120] 4. In Examples 1-5, not only the introduction of amino groups can improve the interfacial properties of MWCNT-OH and PA66, but also the drying of MWCNT-OH under vacuum conditions to form aerogels enhances its dispersion in the resin, thereby greatly improving the mechanical properties of PA66 / glass fiber.
[0121] 5. When the mass of carbon nanotube aerogel powder in PA66 / MWCNT accounts for 0.1%-0.5% of the mass of PA66, the mechanical properties are improved by 10%-30% and the flexural strength is improved by 9%-22% compared with the blank test. Especially when the mass of carbon nanotube aerogel powder is controlled to account for 0.2%-0.4% of the mass of PA66, the mechanical properties are improved by 20%-30% and the flexural strength is improved by 14%-22%.
[0122] The above-described embodiments provide a detailed description of the technical solutions of the present invention. It should be understood that the above descriptions are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a nylon carbon nanotube composite material, characterized in that: The steps include: (1) using a silanization solution, wherein the silanization solution is obtained by dissolving KH550 in an alcohol solvent, placing hydroxylated multi-walled carbon nanotubes in the silanization solution, and introducing amino groups on the surface of the hydroxylated multi-walled carbon nanotubes; (2) dispersing the multi-walled carbon nanotubes obtained in step (1) in a solvent to prepare a suspension, and then adding a non-thickening surfactant to uniformly disperse the multi-walled carbon nanotubes to obtain a multi-walled carbon nanotube slurry; (3) filtering the multi-walled carbon nanotube slurry obtained in step (2) and vacuum drying it to obtain carbon powder, and then air flow pulverizing it to obtain multi-walled carbon nanotube aerogel powder; (4) The multi-walled carbon nanotube aerogel powder obtained in step (3) is blended and extruded with PA66 resin to obtain a nylon carbon nanotube composite material, wherein the mass of the PA66 resin in the blend is 100 parts, and the mass of the multi-walled carbon nanotube aerogel powder is 0.1 part to 1.0 part.
2. The preparation method according to claim 1, characterized in that: In the step (1), in terms of weight, KH550 accounts for 10-20 parts in the silanization solution, and the alcohol solvent accounts for 85-95 parts; Preferably, the silanization solution includes an acid, preferably 0.5 to 5 parts by weight of the acid; Preferably, the silanization solution includes deionized water, preferably 1 part to 10 parts by weight of deionized water; Preferably, in step (1), the acid comprises one or more of hydrochloric acid, acetic acid, and sulfuric acid; Preferably, in step (1), the temperature of the silanization solution is 15°C-25°C; Preferably, in step (1), the hydroxylated multi-walled carbon nanotubes are placed in the silanization solution for 30 min to 120 min.
3. The preparation method according to claim 1, characterized in that: In the step (1), the alcohol solvent includes one or more of methanol, ethanol and isopropanol.
4. The preparation method according to claim 1, characterized in that: In the step (2), the carbon nanotubes are dissolved in a solvent to prepare a suspension having a mass percent concentration of 0.1% to 1%; Preferably, in step (2), the carbon nanotubes are dissolved in a solvent to prepare a suspension having a mass percent concentration of 0.3% to 1%; Preferably, the non-thickening surfactant includes one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, dodecyltrimethylammonium bromide, didodecyldimethylammonium bromide, dioctadecyldimethylammonium bromide, hexadecyltrimethylammonium bromide, sodium lignin sulfonate, alkali lignin, and sodium dodecyl sulfate; Preferably, the mass of the non-thickening surfactant accounts for 10%-50% of the mass of the multi-walled carbon nanotubes.
5. The preparation method according to claim 1, characterized in that: In the step (2), the dispersion method includes homogeneous dispersion; Preferably, the pressure during the homogenization dispersion process is 5000psi-30000ps; Preferably, the number of cycles during the homogeneous dispersion process is 2 to 4 times.
6. The preparation method according to claim 1, characterized in that: In the step (3), the vacuum drying temperature is 80°C-150°C; Preferably, in step (3), the vacuum drying time is 30 min-120 min.
7. The preparation method according to claim 1, characterized in that: In the step (4), the weight of the multi-walled carbon nanotube aerogel powder in the blend is 0.1-0.5 parts, preferably 0.2-0.4 parts.
8. The preparation method according to claim 1, characterized in that: In the step (4), the blend further includes a dehydrating agent, and the mass of the dehydrating agent is 0.5 parts to 2 parts; Preferably, the dehydrating agent includes one or more of DDC (dicyclohexylcarbodiimide), DIC (N,N'-diisopropylcarbodiimide), and EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride).
9. The preparation method according to claim 1, characterized in that: In the step (4), a twin-screw extruder is used for blending and extrusion, and the rotation speed of the twin-screw extruder is preferably 150 rpm-220 rpm; Preferably, in step (4), the temperature of the co-extrusion from the feed port to the discharge port is controlled at 200° C.-300° C.; Preferably, in step (4), multiple temperature control zones are set from the feed port to the discharge port during the co-extrusion; Preferably, in step (4), six temperature control zones are set from the feed port to the discharge port for the co-extrusion, which are 225°C, 235°C, 250°C, 260°C, 255°C, and 250°C, respectively.
10. A nylon carbon nanotube composite material with enhanced mechanical properties, characterized by: The nylon carbon nanotube composite material prepared by the preparation method of any one of claims 1 to 9 is blended with glass fiber to obtain a nylon carbon nanotube composite material with enhanced mechanical properties; Preferably, the glass fiber is short glass fiber; Preferably, the length of the short glass fibers is in the range of 0.01 mm to 3 mm; Preferably, the mass of the short glass fibers accounts for 20%-40% of the mass of the nylon carbon nanotube composite material, and more preferably 30%.
11. The nylon carbon nanotube composite material with enhanced mechanical properties as claimed in claim 10, characterized in that: The mass of the short glass fibers accounts for 30% of the mass of the nylon carbon nanotube composite material; The PA66 is blended with the short glass fibers to obtain PA66 with enhanced mechanical properties, wherein the mass of the short glass fibers accounts for 30% of the mass of the PA66; Compared with the mechanically-property-enhanced PA66, the mechanically-property-enhanced nylon carbon nanotube composite material has improved mechanical properties; Preferably, when the mass of the multi-walled carbon nanotube aerogel powder in the blend is 0.1-0.5 parts, the tensile strength is increased by 10%-30%, and the bending strength is increased by 9%-22%; Preferably, when the mass of the multi-walled carbon nanotube aerogel powder in the blend is 0.2-0.4 parts, the tensile strength is increased by 20%-30%, and the bending strength is increased by 14%-22%.
Citation Information
Cited By
Preparation system of carbon nanotube reinforced metal matrix composite material
CN122252610A