Infrared energy-saving coating for high-temperature furnace kiln and preparation process of infrared energy-saving coating
Through nano-rare earth lanthanum oxide doping solid solution treatment and multi-material combination, the problems of performance attenuation and poor thermal shock resistance of infrared radiation coatings at high temperatures are solved, and high-temperature infrared energy-saving coatings are prepared, achieving high energy saving and extending the life of the kiln. Effect.
Patent Information
- Application Number
- CN202310314782.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing infrared radiation coatings have problems such as low operating temperature at high temperatures, rapid attenuation of infrared radiation performance, and poor thermal shock resistance.
Nano-rare earth lanthanum oxide doped solid solution treatment is used, combined with materials such as quartz powder, calcined alumina, silica sol, hydroxymethyl cellulose and inorganic bentonite, to form a multi-phase doped spinel solid solution through high-temperature solid phase reaction, improving the Infrared radiation performance, and through stirring, dispersion and sand mill grinding and homogenization, a high-temperature furnace infrared energy-saving coating is prepared.
It achieves the stability of infrared radiation performance and long-term use at high temperatures, saves more than 8% of energy consumption, extends the life of the kiln by more than 50%, and can be used continuously at 1600°C.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of infrared radiation ceramic materials, and in particular to a high-temperature furnace infrared energy-saving coating and a preparation process thereof. Background Art
[0002] The development and rational use of energy is an important national policy of our country. Radiant heating is the primary way to heat materials because it is insensitive to the atmosphere (oxygen and nitrogen) in the furnace room and has low heat loss. The furnace body materials of high-temperature industrial furnaces are mostly silicon, aluminum refractory bricks and amorphous castables, which are both the structural materials of the furnace and the
[0003] It is also a heat preservation material. The heating temperature of these kilns is generally above 1000℃, and its energy is generally concentrated in the 1-5μm band. The emissivity of ordinary kiln materials in the above band is 0.45-0.5, so the utilization rate of radiation heating is generally not high. By painting the inner wall of the kiln with high emissivity infrared radiation paint, part of the convection heat will be converted into radiation heat, the heat transfer loss of the furnace wall will be reduced, the radiation heat exchange will be strengthened, and the heating efficiency will be improved. It is not only beneficial to the heating of materials, such as making the temperature in the furnace more uniform, but also helps to decompose the carbon and nitrogen oxides produced in the high-temperature kiln. Therefore, the use of high-temperature infrared energy-saving paint to save energy is increasingly valued by enterprises and scientific research institutions.
[0004] At present, the radiation fillers used in foreign infrared radiation coatings with good performance generally use oxygen-containing compounds, nitrides, carbides or borides with small absorption index and refractive index to obtain high emissivity in the infrared band. For example, the main components of infrared radiation coatings reported in patent CN1037613C are titanium oxide, magnesium oxide, niobium oxide and zirconium sand; the radiation fillers in infrared radiation coatings reported in patent CN102219496A are mainly transition metal oxides of multiphase composite systems, such as iron oxide, manganese oxide, copper oxide, cobalt oxide, etc.; the main components of the CRC series of infrared energy-saving coatings produced by Japan CRC Company are also manganese oxide, chromium oxide, and iron oxide, etc.; Encoat jointly launched by HarbertBeven Company of the United Kingdom and many European countries, and BJ infrared coatings of Beijing University of Science and Technology contain silicon carbide. Patent CN1844277A reported a high-temperature far-infrared insulation energy-saving coating, the main components of which are rare earth oxides and boron nitride. Patent CN1318526C reported an infrared radiation coating composed of organic and inorganic film-forming substances, blackening agents, glass powder and additives, which is only used at 1200°C. The above-mentioned publicly reported infrared energy-saving coatings have achieved certain energy-saving effects when applied to various heating furnaces. However, since most of them are simple mechanical mixing of radiation filler powders, there are still problems such as unstable energy-saving effects, poor thermal shock resistance and low operating temperature. Summary of the invention
[0005] The main purpose of the present invention is to address the technical problems of low operating temperature and fast attenuation of infrared radiation performance of existing domestic infrared radiation coatings. Through nano-rare earth lanthanum oxide doping solid solution treatment, an energy-saving coating with stable infrared radiation performance and suitable for use in high-temperature furnace lining refractory base materials and its preparation process are proposed.
[0006] The invention provides an infrared energy-saving coating for high-temperature furnaces. The raw materials thereof are formulated by weight as follows: 10 to 30 parts of infrared radiation filler, 30 to 40 parts of filler, 20 to 30 parts of alkaline silica sol with a solid content of 30%, 4 to 5 parts of hydroxymethyl cellulose, 2 to 7 parts of inorganic bentonite, 2 to 8 parts of sodium hexametaphosphate and 10 to 15 parts of water; the silica sol provides high-temperature bonding performance for the coating, the hydroxymethyl cellulose provides leveling property for the coating, the inorganic bentonite provides anti-settling effect, and the sodium hexametaphosphate provides dispersion effect.
[0007] Preferably, the filler provides high refractoriness and wear resistance for the coating, and the raw materials thereof are formulated by weight as follows: 50 to 80 parts of quartz powder, 10 to 20 parts of calcined alumina powder, and 20 to 30 parts of refractory clinker.
[0008] Preferably, the infrared radiation filler has the following raw material formula by weight: 10-20 parts of ferric oxide, 5-10 parts of cobalt oxide, 0-30 parts of nickel oxide, 20-50 parts of manganese oxide, and 5-10 parts of nano-grade lanthanum oxide. The infrared radiation filler provides high infrared radiation and absorption characteristics, and the nano-lanthanum oxide is doped through a high-temperature solid-phase reaction to increase the emissivity.
[0009] Preferably, the particle size D50 of the added nano-sized lanthanum oxide powder is 50-100 nm.
[0010] Preferably, the preparation process of the infrared radiation filler consists of the following steps:
[0011] Accurately weighed oxide powders are mixed evenly and ground in a ball mill with a ball-to-material ratio of 10:1 for 2 to 3 hours. The ground powders are heated to 1200-1350°C at a rate of 3-5°C / min and then air-cooled to room temperature to obtain a spinel solid solution doped with nano-rare earth oxides. The obtained sintered body is crushed, pulverized and passed through a 350-mesh sieve to make an infrared radiation filler.
[0012] Preferably, the montmorillonite content in the inorganic bentonite should be above 65%.
[0013] Preferably, the particle size of the quartz powder is greater than 325 mesh, and the SiO2 content in the quartz powder is greater than 95%.
[0014] Preferably, the particle size of the calcined alumina powder is greater than 325 mesh, and the Al2O3 content in the calcined alumina powder is greater than 95%.
[0015] Preferably, the refractory clinker is specifically refractory clay.
[0016] The present invention also provides a preparation process of a high-temperature furnace infrared energy-saving coating, comprising the following steps:
[0017] Firstly, the infrared radiation filler, filler, silica sol, hydroxymethyl cellulose, inorganic bentonite, sodium hexametaphosphate and water are fully mixed, dispersed in a stirring disperser at a speed of 2500-4500 r / min for 1-2 hours, then put into a sand mill for grinding for 2-4 hours, homogenized to make the average particle size reach 350-500 mesh, filtered and packaged.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] In the above technical scheme, quartz powder and calcined alumina are used as fillers to have good thermal expansion matching with silicon, aluminum refractory bricks and amorphous castable base materials, ensuring the high-temperature density of the coating; transition metal oxides are used to form a multi-phase doped spinel solid solution through sintering, which has stable performance in an oxidizing atmosphere and will not cause rapid attenuation of the emissivity; lanthanum oxide has abundant d and f orbital spaces, which are easy to occupy and replace other element ions. Adding it to the spinel structure will cause a large amount of lattice distortion, and the nanoscale makes it have higher reaction and diffusion activity. The impurity ions that have diffused at high temperature are fixed due to rapid cooling, forming a spinel structure with high-concentration defects, reducing the lattice vibration of the powder after firing, and enhancing the high-temperature infrared radiation characteristics of the material.
[0020] The infrared radiation coating prepared by the present invention can achieve a normal emissivity of 0.89 to 0.93 in the full band of 1 to 25 μm. The coating can be sintered into a multi-phase composite ceramic layer in the lining of an inorganic kiln when heated, can be used for a long time at 1600°C, can save energy consumption by more than 8%, and extend the life of the kiln by more than 50%. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with specific embodiments.
[0022] Example 1
[0023] First, weigh 4.3 kg of iron oxide, 2.0 kg of cobalt oxide, 2.89 kg of nickel oxide, 8.7 kg of manganese oxide, and 2.0 kg of nano lanthanum oxide, mix the accurately weighed oxide powders evenly and grind them in a ball mill with a ball-to-material ratio of 10:1 and a grinding time of 2 hours. Heat the ground powder to 1200°C at 3°C / min, keep it warm for 4 hours, and then air-cool it to room temperature to obtain a spinel solid solution doped with nano rare earth oxides. Crush, pulverize and pass the resulting sintered body through a 350-mesh sieve to make an infrared radiation powder.
[0024] Then weigh 25 kg of silica sol, 2 kg of inorganic bentonite, 21 kg of quartz powder, 5.25 kg of calcined alumina, 8.75 kg of refractory clinker, 4 kg of hydroxycellulose, 3 kg of sodium hexametaphosphate, and 12 kg of water.
[0025] First, the infrared radiation filler, filler, silica sol, hydroxymethyl cellulose, inorganic bentonite, sodium hexametaphosphate and water are fully mixed, dispersed in a stirring disperser at a speed of 4500r / min for 2 hours, and then put into a sand mill for grinding for 3 hours, and homogenized to make the average particle size reach more than 350 meshes, filtered, and packaged before coating operation.
[0026] Example 2
[0027] First, weigh 3.8 kg of iron oxide, 2.2 kg of cobalt oxide, 2.5 kg of nickel oxide, 7.8 kg of manganese oxide, and 1.8 kg of nano lanthanum oxide. Mix the accurately weighed oxide powders evenly and grind them in a ball mill with a ball-to-material ratio of 10:1. The grinding time is 2 hours. The ground powder is heated to 1200°C at 3°C / min, kept warm for 4 hours, and then air-cooled to room temperature to obtain a spinel solid solution doped with nano rare earth oxides. The obtained sintered body is crushed, pulverized, and sieved through a 350-mesh sieve to make an infrared radiation powder.
[0028] Then weigh 27 kg of silica sol, 2.2 kg of inorganic bentonite, 25 kg of quartz powder, 5.5 kg of calcined alumina, 9.2 kg of refractory clinker, 3.8 kg of hydroxycellulose, 2.8 kg of sodium hexametaphosphate, and 10 kg of water.
[0029] First, the infrared radiation filler, filler, silica sol, hydroxymethyl cellulose, inorganic bentonite, sodium hexametaphosphate and water were fully mixed and then rotated at 4500r / min.
[0030] The mixture is dispersed in a high-speed stirring disperser for 3 hours, then put into a sand mill for grinding for 2.5 hours, homogenized, and the average particle size reaches more than 350 meshes, filtered, and packaged before coating.
[0031] Example 3
[0032] First, weigh 4.5 kg of iron oxide, 2.7 kg of cobalt oxide, 1.8 kg of nickel oxide, 8 kg of manganese oxide, and 1.5 kg of nano lanthanum oxide. Mix the accurately weighed oxide powders evenly and grind them in a ball mill with a ball-to-material ratio of 10:1. The grinding time is 2 hours. The ground powder is heated to 1200°C at 3°C / min, kept warm for 4 hours, and then air-cooled to room temperature to obtain a spinel solid solution doped with nano rare earth oxides. The obtained sintered body is crushed, pulverized, and sieved through a 350-mesh sieve to make an infrared radiation powder.
[0033] Then weigh 30 kg of silica sol, 2.6 kg of inorganic bentonite, 26 kg of quartz powder, 5.5 kg of calcined alumina, 8.5 kg of refractory clinker, 3.5 kg of hydroxycellulose, 2.5 kg of sodium hexametaphosphate, and 11 kg of water.
[0034] First, the infrared radiation filler, filler, silica sol, hydroxymethyl cellulose, inorganic bentonite, sodium hexametaphosphate and water are fully mixed, dispersed in a stirring disperser at a speed of 4500r / min for 3 hours, and then put into a sand mill for grinding for 3.5 hours, and homogenized to make the average particle size reach more than 350 meshes. After filtering and packaging, the coating operation can be carried out.
[0035] Example 4
[0036] First, weigh 5.5 kg of iron oxide, 2 kg of cobalt oxide, 2.3 kg of nickel oxide, 7.9 kg of manganese oxide, and 2.5 kg of nano lanthanum oxide, mix the accurately weighed oxide powders evenly and grind them in a ball mill with a ball-to-material ratio of 10:1 and a grinding time of 2 hours. Heat the ground powder to 1200°C at 3°C / min, keep it warm for 4 hours, and then air-cool it to room temperature to obtain a spinel solid solution doped with nano rare earth oxides. Crush the resulting sintered body, grind it, and pass it through a 350-mesh sieve to make an infrared radiation powder.
[0037] Then weigh 29 kg of silica sol, 2.0 kg of inorganic bentonite, 23 kg of quartz powder, 5.4 kg of calcined alumina, 9 kg of refractory clinker, 4.5 kg of hydroxycellulose, 2.8 kg of sodium hexametaphosphate, and 9 kg of water.
[0038] First, the infrared radiation filler, filler, silica sol, hydroxymethyl cellulose, inorganic bentonite, sodium hexametaphosphate and water are fully mixed, dispersed in a stirring disperser at a speed of 4500r / min for 3 hours, and then put into a sand mill for grinding for 3.5 hours, homogenized, and the average particle size reaches more than 350 meshes, filtered, and packaged before coating operation.
[0039] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high-temperature furnace infrared energy-saving coating, characterized in that: The raw materials are formulated by weight as follows: 10-30 parts of infrared radiation filler, 30-40 parts of filler, 20-30 parts of alkaline silica sol with a solid content of 30%, 4-5 parts of hydroxymethyl cellulose, 2-7 parts of inorganic bentonite, 2-8 parts of sodium hexametaphosphate and 10-15 parts of water.
2. The high temperature furnace infrared energy-saving coating according to claim 1, characterized in that: The raw materials of the filler are formulated as follows by weight: 50 to 80 parts of quartz powder, 10 to 20 parts of calcined alumina powder, and 20 to 30 parts of refractory clinker.
3. The high temperature furnace infrared energy-saving coating according to claim 1, characterized in that: The infrared radiation filler has the following raw material formula by weight: 10-20 parts of ferric oxide, 5-10 parts of cobalt oxide, 0-30 parts of nickel oxide, 20-50 parts of manganese oxide and 5-10 parts of nano-grade lanthanum oxide.
4. The high temperature furnace infrared energy-saving coating according to claim 3, characterized in that: The particle size D50 of the added nano-grade lanthanum oxide powder is 50 to 100 nm.
5. The high temperature furnace infrared energy-saving coating according to claim 4, characterized in that: The preparation process of infrared radiation filler consists of the following steps: Accurately weighed oxide powders are mixed evenly and ground in a ball mill with a ball-to-material ratio of 10:1 for 2 to 3 hours. The ground powders are heated to 1200-1350°C at a rate of 3-5°C / min and then air-cooled to room temperature to obtain a spinel solid solution doped with nano-rare earth oxides. The obtained sintered body is crushed, pulverized and passed through a 350-mesh sieve to make an infrared radiation filler.
6. The high temperature furnace infrared energy-saving coating according to claim 1, characterized in that: The montmorillonite content in the inorganic bentonite must be above 65%.
7. The high temperature furnace infrared energy-saving coating according to claim 1, characterized in that: The particle size of the quartz powder is greater than 325 meshes, and the SiO2 content in the quartz powder is greater than 95%.
8. The high temperature furnace infrared energy-saving coating according to claim 1, characterized in that: The particle size of the calcined alumina powder is greater than 325 meshes, and the Al2O3 content in the calcined alumina powder is greater than 95%.
9. The high temperature furnace infrared energy-saving coating according to claim 1, characterized in that: The refractory clinker is specifically refractory clay.
10. A process for preparing the infrared energy-saving coating for high-temperature furnaces according to claim 1, characterized in that: The steps include: Firstly, the infrared radiation filler, filler, silica sol, hydroxymethyl cellulose, inorganic bentonite, sodium hexametaphosphate and water are fully mixed, dispersed in a stirring disperser at a speed of 2500-4500 r / min for 1-2 hours, then put into a sand mill for grinding for 2-4 hours, homogenized to make the average particle size reach 350-500 mesh, filtered and packaged.