Preparation method of functional coating based on self-polymerization of aminomalononitrile
By aldehydic modification of hyaluronic acid and copolymerization with aminomalononitrile, combined with oscillation reaction and antibacterial metal elements, a coating with anti-inflammatory and antibacterial functions was prepared, which solved the problem of single functionality of existing coatings. The coating's versatility expansion and process simplicity are achieved.
Patent Information
- Application Number
- CN202411004387.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The existing coatings based on aminomalononitrile surface modification technology have a relatively single functionality, making it difficult to impart multiple functionalities to the surface of the material, such as anti-inflammatory and antibacterial properties.
Hyaluronic acid is modified by aldehyde to give it the ability to copolymerize with aminomalononitrile-p-toluenesulfonate, and is mixed with aminomalononitrile-p-toluenesulfonate under alkaline conditions to deposit through a oscillation reaction. On the surface of the substrate, a functional coating with anti-inflammatory function is prepared, and antibacterial metal elements are further introduced to enhance the antibacterial property.
It expands the application fields of the coating and gives the coating anti-inflammatory and antibacterial functions. The process is simple and fast, suitable for industrial promotion, the material is safe and easy to obtain, and it is environmentally friendly.
Smart Images

Figure CN118725657A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, and in particular to a method for preparing a functional coating based on aminomalononitrile self-polymerization. Background Art
[0002] The surface modification technology of materials is widely used and plays an important role in the fields of medical devices, automobile industry, aerospace, electronics, nanotechnology, etc. By modifying the surface of materials, the corrosion resistance, friction and wear performance, biocompatibility, optical properties, etc. of the materials can be improved, and special functions such as antibacterial, antifouling, photocatalytic, etc. can also be achieved.
[0003] Currently available surface modification methods include dip coating, electroplating, layer-by-layer assembly, hydrolysis, plasma treatment, electron beam irradiation, organosilane chemistry, graft polymerization, and interfacial polymerization. Generally, these methods are time-consuming and complicated processes, and cannot be extended to a wider range of material surfaces, which are largely limited by the surface properties of the substrate. Therefore, a simple, efficient, and universal strategy is urgently needed to improve the surface of materials.
[0004] In recent years, a surface modification strategy based on the self-polymerization technology of aminomalononitrile p-toluenesulfonate has been developed. Under alkaline conditions, aminomalononitrile can be rapidly deposited on the surface of a wide range of materials. Compared with other technologies, this surface modification strategy has multiple advantages in deposition processing under mild conditions, and can be applied to various surfaces and a wide range of applications. The coating preparation has the advantages of simple operation, rapid and efficient, stable and uniform.
[0005] However, the functionality of the coating constructed based on the surface modification technology of aminomalononitrile is relatively single and not rich enough. At present, the surface modification of aminomalononitrile coating is mainly used to improve the hydrophilicity and biocompatibility of the material surface, which is not rich enough.
[0006] Therefore, how to give the coating more functionality (such as anti-inflammatory, antibacterial, etc.) based on aminomalononitrile surface modification technology is a topic that urgently needs in-depth research. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a method for preparing a functional coating based on aminomalononitrile self-polymerization. The present invention first performs formaldehyde modification on hyaluronic acid to give it the ability to copolymerize with aminomalononitrile p-toluenesulfonate, then mixes it with aminomalononitrile p-toluenesulfonate under alkaline conditions, and oscillates and reacts to deposit on the surface of the substrate to obtain a functional coating with anti-inflammatory function, which greatly expands the application field. And compared with conventional surface modification methods, the method of the present invention is simple, fast, and mild in conditions.
[0008] The specific technical solution of the present invention is: a method for preparing a functional coating based on aminomalononitrile self-polymerization, comprising the following steps:
[0009] S1: Modify hyaluronic acid to introduce aldehyde groups to obtain hyaluronic acid with aldehyde groups. S2: Dissolve aminomalononitrile p-toluenesulfonate and hyaluronic acid with aldehyde groups in a tris(hydroxymethyl)aminomethane hydrochloride buffer solution with a pH of 8.0-9.5, and adjust the pH of the system to 8-9 with an alkali to obtain a functional coating solution.
[0010] Wherein, the concentration of aminomalononitrile p-toluenesulfonate in the functional coating solution is 0.02-0.1 g / mL, and the concentration of hyaluronic acid with aldehyde group is 0.3-0.8 mg / mL;
[0011] S3: Immerse the substrate in the functional coating solution, take it out after shaking and incubating, wash and remove the residual unpolymerized precipitate or its derivatives on the surface of the substrate, and dry it to obtain a substrate with a surface uniformly coated with the functional coating.
[0012] Hyaluronic acid has excellent anti-inflammatory effects, so if it is introduced into a coating based on aminomalononitrile self-polymerization, the coating can be endowed with anti-inflammatory effects. However, the hyaluronic acid molecule itself does not have a group that can polymerize with aminomalononitrile. Therefore, in S1, the present invention first performs aldehyde modification on hyaluronic acid. After the modification of hyaluronic acid by the present invention, not only can it be endowed with the ability to copolymerize with aminomalononitrile p-toluenesulfonate, but the modification process will not destroy the functional active structure of hyaluronic acid, so the original activity can almost be maintained.
[0013] In S2, hyaluronic acid with an aldehyde group is mixed with aminomalononitrile p-toluenesulfonate under alkaline conditions to obtain a functional coating solution; in S3, a copolymerization reaction is carried out on the surface of the substrate by a dipping + oscillation incubation method to construct a functional coating with anti-inflammatory function.
[0014] Preferably, in S1, the method for modifying the hyaluronic acid with an aldehyde group is as follows: dissolving 2-6 g of sodium hyaluronate and 1-3 g of sodium periodate in phosphate buffered saline at pH = 4.5-5.5, and stirring for 2-6 h in the dark at 20-30°C; finally, adding ethylene glycol to terminate the reaction; dialyzing, and freeze-drying to obtain hyaluronic acid with an aldehyde group.
[0015] The principle of the above modification is: some hydroxyl groups on hyaluronic acid are oxidized to aldehyde groups by sodium periodate, and the aldehyde groups can be introduced into the main chain of hyaluronic acid. Therefore, in the process of forming the functional coating, the amino groups on aminomalononitrile p-toluenesulfonate and the aldehyde groups of the modified hyaluronic acid undergo a Schiff base reaction.
[0016] Preferably, in S3, the shaking incubation temperature is 15-45°C and the time is 8-24h.
[0017] Preferably, the method further comprises S4: immersing the substrate obtained in S3 and having the functional coating uniformly coated on the surface thereof in an antibacterial modification liquid containing copper chloride and / or silver nitrate, performing a secondary oscillation reaction, and obtaining a secondary modified functional coating after ultrasonic cleaning and drying; the number of amino groups in the aminomalononitrile p-toluenesulfonate is in excess compared to the aldehyde groups in the aldehyde-modified hyaluronic acid.
[0018] In order to further impart antibacterial function to the functional coating, antibacterial elements can be introduced into the functional coating by the method of immersion + oscillation reaction (the amino group in aminomalononitrile p-toluenesulfonate can chelate with the metal by coordination). In addition, in order to ensure that there are still redundant active groups in the functional coating that can react with copper chloride and / or silver nitrate, it is necessary to control the excess of the amino group on aminomalononitrile p-toluenesulfonate compared to the aldehyde group in the functional molecule in S2, and the preferred molar ratio of the amino group to the aldehyde group is (30-200):1.
[0019] More preferably, the temperature of the secondary oscillation reaction is 20-40° C. and the time is 12-24 h.
[0020] Further preferably, the total concentration of copper chloride and / or silver nitrate in the antibacterial modified liquid is 10-60 mg / mL.
[0021] Preferably, in S3, the substrate is a planar substrate.
[0022] Further preferably, the planar substrate is an aluminum sheet, a zinc sheet, a copper sheet, a nickel sheet, a titanium sheet, an iron sheet, a stainless steel substrate, a polytetrafluoroethylene plate, a polyvinyl chloride plate, a polypropylene plate, a polyester fiber fabric, a silicon sheet, a acetate fabric or a glass sheet.
[0023] Preferably, in S3, the cleaning is ultrasonic cleaning: ultrasonic cleaning is performed using deionized water for at least 30 minutes, with an ultrasonic frequency of 25-40 kHz and a power of 150-200 W. This step is used to remove polymers with weak bonding strength on the surface of the material.
[0024] Compared with the prior art, the beneficial effects of the present invention are:
[0025] (1) The present invention first performs formaldehyde modification on hyaluronic acid to give it the ability to copolymerize with aminomalononitrile p-toluenesulfonate, then mixes it with aminomalononitrile p-toluenesulfonate under alkaline conditions, and deposits it on the surface of a substrate through an oscillating reaction to obtain a functional coating with anti-inflammatory function, which can greatly expand the application field.
[0026] (2) The present invention further combines antibacterial metal elements on the surface of the functional coating to further impart antibacterial properties to the functional coating.
[0027] (3) Compared with conventional surface modification methods, the method of the present invention has safe and readily available materials, is environmentally friendly, has a simple and fast process, and has mild conditions, making it suitable for industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 These are digital photos of the coatings deposited on various organic and inorganic substrate surfaces in Example 1;
[0029] Figure 2 This is a scanning electron microscope image of polyester fiber fabric;
[0030] Figure 3 This is a scanning electron microscope image of the anti-inflammatory coating of polyester fiber fabric in Example 2;
[0031] Figure 4 This is a test chart of the anti-inflammatory function of polyester fiber fabric.
[0032] Figure 5 This is a photo of the inhibition zone of polyester fabric; DETAILED DESCRIPTION
[0033] The present invention is further described below in conjunction with the embodiments. In view of the fact that the existing functional coating preparation methods are complicated and cumbersome, the functional molecule modification process is complicated and cumbersome, and the reaction conditions are harsh, the present invention proposes a functional coating based on aminomalononitrile self-polymerization and its preparation method and application
[0034] Example 1
[0035] A method for preparing a polyaminomalononitrile coating on a planar substrate comprises the steps of:
[0036] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.
[0037] Step 2: Substrate pretreatment: The prepared aluminum sheet, zinc sheet, copper sheet, nickel sheet, titanium sheet, iron sheet, stainless steel sheet, polytetrafluoroethylene sheet (PTFE), polyvinyl chloride sheet (PVC), polypropylene sheet (PP), polyester fiber fabric (PET), acetate fiber fabric and silicon sheet were treated with acetone, anhydrous ethanol and ultrasound for 3 times, each time for 30 minutes; then ultrasonically cleaned with deionized water for 3 times, each time for 30 minutes; the ultrasonic frequency was 40kHz and the power was 200W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the substrate was placed in normal pressure ventilation conditions at 65°C for 4 hours.
[0038] Step 3: Prepare polyaminomalononitrile coating: add 1g of aminomalononitrile p-toluenesulfonate to Tris buffer solution (50ml, pH=8.5) to prepare an AMN solution with a concentration of 0.02g / mL; after sufficient dissolution, use 2M sodium hydroxide to adjust the pH of the aminomalononitrile solution to 8.5; immerse the cleaned substrate in the aminomalononitrile solution and place it in a water bath constant temperature oscillator for deposition for 10 hours. After the deposition is completed, take out and ultrasonically clean it with deionized water for 60 minutes (ultrasonic frequency is 40kHz, power is 200W), and dry it for use.
[0039] Figure 1 Digital photos of coatings deposited on various organic and inorganic substrates.
[0040] Example 2
[0041] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.
[0042] Step 2: Substrate pretreatment: The prepared polyester fiber fabric (PET) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonic cleaning was performed with deionized water for 3 times, each time for 30 minutes; the ultrasonic frequency was 40kHz and the power was 200W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the substrate was placed in normal pressure ventilation conditions at 65°C for 4 hours.
[0043] Step 3: Preparation of aldehyde hyaluronic acid: 4 g of sodium hyaluronate and 2 g of sodium periodate (SP) were dissolved in 200 mL of phosphate buffered saline (PBS, pH = 5.0) and stirred for 4 hours in the dark at 25°C. Finally, 3 ml of ethylene glycol was added to terminate the reaction. Finally, the reaction mixture was dialyzed and lyophilized to obtain dialdehyde-modified hyaluronic acid.
[0044] Step 4: Preparation of anti-inflammatory coating: Add 1g of aminomalononitrile p-toluenesulfonate and 25mg of aldehyde hyaluronic acid to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde hyaluronic acid are 20mg / mL and 0.5mg / mL, and the two are mixed evenly and the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10h, and then ultrasonically cleaned with deionized water for 60min (ultrasonic frequency is 40kHz, power is 200W), and then taken out and dried for use.
[0045] Example 3
[0046] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.
[0047] Step 2: Substrate pretreatment: The prepared polyester fiber fabric (PET) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonic cleaning was performed with deionized water for 3 times, each time for 30 minutes; the ultrasonic frequency was 40kHz and the power was 200W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the substrate was placed in normal pressure ventilation conditions at 65°C for 4 hours.
[0048] Step 3: Preparation of aldehyde hyaluronic acid: 4 g of sodium hyaluronate and 2 g of sodium periodate (SP) were dissolved in 200 mL of phosphate buffered saline (PBS, pH = 5.0) and stirred for 4 hours in the dark at 25°C. Finally, 3 ml of ethylene glycol was added to terminate the reaction. Finally, the reaction mixture was dialyzed and lyophilized to obtain dialdehyde-modified hyaluronic acid.
[0049] Step 4: Preparation of anti-inflammatory coating: Add 1g of aminomalononitrile p-toluenesulfonate and 25mg of aldehyde hyaluronic acid to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde hyaluronic acid are 0.02g / mL and 0.5mg / mL, and the two are mixed evenly and the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10 hours, and then ultrasonically cleaned with deionized water for 60 minutes (ultrasonic frequency is 40kHz, power is 200W), and then taken out and dried for use.
[0050] Step 5: Preparation of bactericidal and anti-inflammatory coating: First, prepare a silver nitrate solution with a concentration of 40 mg / mL under dark conditions, and then immerse the polyester fiber fabric deposited with the anti-inflammatory coating in silver nitrate and incubate for 24 hours. After obtaining the antibacterial and anti-inflammatory coating, use deionized water to ultrasonically clean and dry it for use.
[0051] Example 4
[0052] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.
[0053] Step 2: Substrate pretreatment: The prepared polyester fiber fabric (PET) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonic cleaning was performed with deionized water for 3 times, each time for 30 minutes; the ultrasonic frequency was 40kHz and the power was 200W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the substrate was placed in normal pressure ventilation conditions at 65°C for 4 hours.
[0054] Step 3: Preparation of aldehyde hyaluronic acid: 4 g of sodium hyaluronate and 2 g of sodium periodate (SP) were dissolved in 200 mL of phosphate buffered saline (PBS, pH = 5.0) and stirred for 4 hours in the dark at 25°C. Finally, 3 ml of ethylene glycol was added to terminate the reaction. Finally, the reaction mixture was dialyzed and lyophilized to obtain dialdehyde-modified hyaluronic acid.
[0055] Step 4: Preparation of anti-inflammatory coating: Add 1g of aminomalononitrile p-toluenesulfonate and 15mg of aldehyde hyaluronic acid to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde hyaluronic acid are 0.02g / mL and 0.3mg / mL, and the two are mixed evenly and the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10 hours, and then ultrasonically cleaned with deionized water for 60 minutes (ultrasonic frequency is 40kHz, power is 200W), and then taken out and dried for use.
[0056] Step 5: Preparation of bactericidal and anti-inflammatory coating: First, prepare a silver nitrate solution with a concentration of 40 mg / mL under dark conditions, and then immerse the polyester fiber fabric with the anti-inflammatory coating in silver nitrate and incubate for 24 hours. After obtaining the bactericidal and anti-inflammatory coating, use deionized water to ultrasonically clean and dry it for use.
[0057] Example 5
[0058] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.
[0059] Step 2: Substrate pretreatment: The prepared polyester fiber fabric (PET) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonic cleaning was performed with deionized water for 3 times, each time for 30 minutes; the ultrasonic frequency was 40kHz and the power was 200W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the substrate was placed in normal pressure ventilation conditions at 65°C for 4 hours.
[0060] Step 3: Preparation of aldehyde hyaluronic acid: 4 g of sodium hyaluronate and 2 g of sodium periodate (SP) were dissolved in 200 mL of phosphate buffered saline (PBS, pH = 5.0) and stirred for 4 hours in the dark at 25°C. Finally, 3 ml of ethylene glycol was added to terminate the reaction. Finally, the reaction mixture was dialyzed and lyophilized to obtain dialdehyde-modified hyaluronic acid.
[0061] Step 4: Preparation of anti-inflammatory coating: Add 1g of aminomalononitrile p-toluenesulfonate and 40mg of aldehyde hyaluronic acid to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde hyaluronic acid are 0.02g / mL and 0.8mg / mL, and the two are mixed evenly and the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10 hours, and then ultrasonically cleaned with deionized water for 60 minutes (ultrasonic frequency is 40kHz, power is 200W), and then taken out and dried for use.
[0062] Step 5: Preparation of bactericidal and anti-inflammatory coating: First, prepare a silver nitrate solution with a concentration of 40 mg / mL under dark conditions, and then immerse the polyester fiber fabric with the anti-inflammatory coating in silver nitrate and incubate for 24 hours. After obtaining the bactericidal and anti-inflammatory coating, use deionized water to ultrasonically clean and dry it for use.
[0063] Example 6
[0064] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.
[0065] Step 2: Substrate pretreatment: The prepared polyester fiber fabric (PET) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonic cleaning was performed with deionized water for 3 times, each time for 30 minutes; the ultrasonic frequency was 40kHz and the power was 200W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the substrate was placed in normal pressure ventilation conditions at 65°C for 4 hours.
[0066] Step 3: Preparation of aldehyde hyaluronic acid: 4 g of sodium hyaluronate and 2 g of sodium periodate (SP) were dissolved in 200 mL of phosphate buffered saline (PBS, pH = 5.0) and stirred for 4 hours in the dark at 25°C. Finally, 3 ml of ethylene glycol was added to terminate the reaction. Finally, the reaction mixture was dialyzed and lyophilized to obtain dialdehyde-modified hyaluronic acid.
[0067] Step 4: Preparation of anti-inflammatory coating: Add 2.5g of aminomalononitrile p-toluenesulfonate and 40mg of aldehyde hyaluronic acid to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde hyaluronic acid are 0.05g / mL and 0.8mg / mL, and the two are mixed evenly and the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10 hours, and then ultrasonically cleaned with deionized water for 60 minutes (ultrasonic frequency is 40kHz, power is 200W), and then taken out and dried for use.
[0068] Step 5: Preparation of bactericidal and anti-inflammatory coating: First, prepare a silver nitrate solution with a concentration of 40 mg / mL under dark conditions, and then immerse the polyester fiber fabric with the anti-inflammatory coating in silver nitrate and incubate for 24 hours. After obtaining the bactericidal and anti-inflammatory coating, use deionized water to ultrasonically clean and dry it for use.
[0069] Example 7
[0070] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.
[0071] Step 2: Substrate pretreatment: The prepared polyester fiber fabric (PET) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonic cleaning was performed with deionized water for 3 times, each time for 30 minutes; the ultrasonic frequency was 40kHz and the power was 200W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the substrate was placed in normal pressure ventilation conditions at 65°C for 4 hours.
[0072] Step 3: Preparation of aldehyde hyaluronic acid: 4 g of sodium hyaluronate and 2 g of sodium periodate (SP) were dissolved in 200 mL of phosphate buffered saline (PBS, pH = 5.0) and stirred for 4 hours in the dark at 25°C. Finally, 3 ml of ethylene glycol was added to terminate the reaction. Finally, the reaction mixture was dialyzed and lyophilized to obtain dialdehyde-modified hyaluronic acid.
[0073] Step 4: Preparation of anti-inflammatory coating: Add 5g of aminomalononitrile p-toluenesulfonate and 40mg of aldehyde hyaluronic acid to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde hyaluronic acid are 0.1g / mL and 0.8mg / mL, and the two are mixed evenly and the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10 hours, and then ultrasonically cleaned with deionized water for 60 minutes (ultrasonic frequency is 40kHz, power is 200W), and then taken out and dried for use.
[0074] Step 5: Preparation of bactericidal and anti-inflammatory coating: First, prepare a silver nitrate solution with a concentration of 60 mg / mL under dark conditions, and then immerse the polyester fiber fabric with the anti-inflammatory coating in silver nitrate and incubate for 24 hours. After obtaining the bactericidal and anti-inflammatory coating, use deionized water to ultrasonically clean and dry it for use.
[0075] Performance Testing
[0076] (1) Morphology observation: Figure 2 , 3 They are scanning electron microscope images of polyester fiber fabric and the polyester fiber fabric in Example 2 after functional coating is deposited on the surface.
[0077] (4) Anti-inflammatory function test: PET-AMN (Example 1), PET-AMN-HA (Example 2), PET-AMN-HA-Ag (Example 3) samples were placed in phosphate buffered saline (pH = 7.3) containing 0.4M NaCl, 0.5% bovine serum albumin (BSA), 0.05% Tween 20 and protease inhibitors for 12 hours. The solution was then centrifuged at 14000 rpm for 30 minutes. The concentrations of interleukin-1β (IL-1β) and tumor necrosis factor α (TNF-α) were detected using a commercially available enzyme-linked immunosorbent assay kit.
[0078] Figure 4 The anti-inflammatory function test diagram of the polyester fiber fabric obtained in Example 1, Example 2 and Example 3; TNF-α and IL-1β are inflammatory factors that can cause excessive infiltration of inflammatory cells on the wound surface and hinder wound repair. Figure 4 As shown, the expression of TNF-α and IL-1β was decreased in PET-AMN-HA and PET-AMN-HA-Ag coatings.
[0079] (5) Antibacterial zone test: Polyester fiber fabric (PET), PET-AMN-HA (Example 2), and PET-AMN-HA-Ag (Example 3) were cut and set aside. The polyester fiber fabrics were attached to the E. coli (10 7 CFU / mL) and coated with Staphylococcus aureus (S. aureus) (10 7 CFU / mL) in a culture dish, with 3 parallel samples in each group, and then placed in an incubator at 37°C and 95% humidity for 24 hours. After the experiment, the samples were taken out and the diameter of the inhibition zone was measured with a vernier caliper and photographed. Figure 5 As shown, the PET-AMN-HA-Ag (Example 3) coating material prepared by the present invention has excellent antibacterial effect.
[0080] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0081] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a functional coating based on aminomalononitrile self-polymerization, characterized in that The steps include: S1: modifying hyaluronic acid to introduce aldehyde groups to obtain hyaluronic acid with aldehyde groups; S2: dissolving aminomalononitrile p-toluenesulfonate and hyaluronic acid with aldehyde groups in a tris(hydroxymethyl)aminomethane hydrochloride buffer solution with a pH of 8.0-9.5, and adjusting the pH of the system to 8-9 with an alkali to obtain a coating solution; The concentration of aminomalononitrile p-toluenesulfonate in the functional coating solution is 0.02-0.1 g / mL, and the concentration of hyaluronic acid with an aldehyde group is 0.3-0.8 mg / mL; S3: Immerse the substrate in the functional coating solution, take it out after shaking and incubating, wash and remove the residual unpolymerized precipitate or its derivatives on the surface of the substrate, and dry it to obtain a substrate with a surface uniformly coated with the functional coating.
2. The preparation method according to claim 1, characterized in that: In S1, the method for modifying the hyaluronic acid with an aldehyde group is as follows: dissolving 2-6 g of sodium hyaluronate and 1-3 g of sodium periodate in phosphate buffered saline at pH = 4.5-5.5, and stirring for 2-6 h at 20-30° C. in the dark; finally, adding ethylene glycol to terminate the reaction; dialyzing, freeze-drying, and obtaining hyaluronic acid with an aldehyde group.
3. The preparation method according to claim 1, characterized in that: In S3, the shaking incubation temperature is 15-45°C and the time is 8-24h.
4. The preparation method according to claim 1, characterized in that: The method further comprises S4: immersing the substrate obtained in S3 and having the functional coating uniformly coated on the surface thereof into an antibacterial modification liquid containing copper chloride and / or silver nitrate, performing a secondary oscillation reaction, and obtaining a secondary modified functional coating after ultrasonic cleaning and drying; the number of amino groups in the aminomalononitrile p-toluenesulfonate is in excess compared to the aldehyde groups in the hyaluronic acid with aldehyde groups.
5. The preparation method according to claim 4, characterized in that: The temperature of the secondary oscillation reaction is 20-40°C and the time is 12-24h.
6. The preparation method according to claim 4, characterized in that: The total concentration of copper chloride and / or silver nitrate in the antibacterial modified liquid is 10-60 mg / mL.
7. The preparation method according to claim 1, characterized in that: In S3, the substrate is a planar substrate.
8. The preparation method according to claim 7, characterized in that: The flat substrate is an aluminum sheet, a zinc sheet, a copper sheet, a nickel sheet, a titanium sheet, an iron sheet, a stainless steel substrate, a polytetrafluoroethylene plate, a polyvinyl chloride plate, a polypropylene plate, a polyester fiber fabric, a silicon sheet, a acetate fabric or a glass sheet.
9. The preparation method according to claim 7 or 8, characterized in that: In S3, the cleaning is ultrasonic cleaning: ultrasonic cleaning is performed using deionized water for at least 30 minutes, with an ultrasonic frequency of 25-40 kHz and a power of 150-200 W.
Citation Information
Patent Citations
Hydrogen cyanide-based polymer surface coatings and hydrogels
CN104470998A
Antibacterial hydrogel based on imine bonds and acylhydrazone bonds and preparation method of antibacterial hydrogel
CN110894302A
Modified hyaluronic acid and application thereof in medical beauty filler
CN117843832A
Hydrogen cyanide-based polymer surface coatings and hydrogels
WO2013170308A1