Trivalent chromium improved silane self-lubricating resin emulsion based on hot-rolled galvanized sheet and preparation method of trivalent chromium improved silane self-lubricating resin emulsion

By using trivalent chromium-modified silane self-lubricating resin emulsion on hot-rolled galvanized sheets, combined with nano-scale water-soluble molybdenum salt-modified acidic silica sol and water-based cationic acrylic emulsion, a composite film layer is formed to solve the problem of hot-rolled galvanized sheets. The problem of rough surface and insufficient corrosion resistance is achieved to achieve efficient wear and corrosion resistance.

CN118725671APending Publication Date: 2024-10-01NIPPON PAINT(SHANGHAI)CHEM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410954843.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Hot-rolled galvanized sheets have problems with poor shape, rough surface and oxidation in mass production. Traditional trivalent chromium passivators cannot meet its corrosion resistance and wear resistance requirements, and hexavalent chromium passivators are toxic and Due to environmental pollution issues, its use is restricted, and existing trivalent chromium passivators are suitable for cold-rolled plates but not for hot-rolled plates.

Method used

Using trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheets, a composite film layer is formed through the compounding of nano-scale water-soluble molybdenum salt-modified acidic silica sol and water-based cationic acrylic emulsion, combined with high-efficiency water-based wax to assist agent to improve the wear resistance and corrosion resistance of the film.

Benefits of technology

It achieves excellent corrosion resistance and wear resistance of hot-rolled galvanized sheets, meets performance requirements such as alkali resistance, solvent resistance, water resistance, and yellowing resistance, and overcomes the problem of traditional trivalent chromium passivation agents on hot-rolled sheets. performance is insufficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725671A_ABST
    Figure CN118725671A_ABST
Patent Text Reader

Abstract

The invention discloses a trivalent chromium improved silane self-lubricating resin emulsion based on a hot-rolled galvanized sheet and a preparation method of the trivalent chromium improved silane self-lubricating resin emulsion. Each liter of resin emulsion comprises the following components in percentage by weight: # imgabs0 #.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal surface treatment and protective film, and in particular to a trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet and a preparation method thereof. Background Art

[0002] With the development of hot strip rolling technology, the thin slab continuous casting and rolling process (CSP) has emerged, which has gradually reduced the thickness of hot-rolled strip steel, and the thinnest thickness has reached 0.8mm, so that hot-rolled plates can replace the functions of cold-rolled plates in certain fields. After pickling, the surface of hot-rolled plates is clean and the internal structure is equiaxed grains. There is no need for degreasing during hot-dip galvanizing, and the annealing furnace is shorter, and the original plate has one less cold rolling process, so the production cost is low and has market competitiveness. At present, hot-rolled galvanized plates are widely used in industries such as construction steel, welded pipes, and highway guardrails.

[0003] Since hot-rolled galvanized products are used outdoors for a long time, they have higher requirements for corrosion resistance and wear resistance. As downstream users' requirements for corrosion resistance and wear resistance continue to increase, the following problems usually occur after hot-rolled galvanizing process combined with ordinary trivalent chromium passivation:

[0004] First, in mass production, the hot-rolled galvanized thick plate often has a poor shape, often with large wave edges and warp defects, and inevitably has small particles similar to rice grains distributed on the plate surface, which are usually called zinc particles. The combined effect of the two causes the surface to be rough and uneven, which not only hinders the appearance, but also is harmful to the post-treatment coating process. Hot-rolled galvanized plates that have been passivated by ordinary methods are often prone to oxidation and rust during transportation;

[0005] Second, due to the need for stacking during transportation, the contact parts between materials often have relative displacement. Ordinary trivalent chromium passivation liquid usually fails to effectively give the film wear resistance, resulting in friction black spots, resulting in low comprehensive utilization of materials. Ordinary trivalent chromium film cannot meet the performance requirements after coating on hot-rolled thick plate with large roughness (usually greater than 1.2um).

[0006] Traditional metal surface passivation uses hexavalent chromium passivation process. Although hexavalent chromium passivation has the advantages of simple process and good passivation effect, hexavalent chromium is a highly toxic and carcinogenic substance, and it is easy to cause serious pollution to the environment. At present, it has been strictly restricted in developed countries in Europe and the United States. my country has also issued relevant policies to restrict the use of hexavalent chromium, and hexavalent chromium passivation agents are gradually withdrawing from the stage of history. The toxicity of trivalent chromium is only one percent of that of hexavalent chromium, and trivalent chromium passivation is not inferior to hexavalent chromium passivation in many aspects, so trivalent chromium passivation agents are widely used in the field of metal surface treatment.

[0007] At present, many trivalent chromium passivators have been reported both at home and abroad, but most of the trivalent chromium passivators reported in patents or other literature are suitable for passivation of cold-rolled galvanized components, such as CN100510178, WO2007 / 088030, JP2008 / 063963, etc.

[0008] This type of trivalent chromium passivation agent is not suitable for the passivation treatment of continuous hot-dip galvanized steel strips based on hot-rolled plates in steel plants. The reason is that this type of trivalent chromium passivation agent belongs to the inorganic impregnation reaction type, and a certain reaction time and treatment temperature are required to form a film on the surface of galvanized components; while the trivalent chromium passivation agent used on hot-rolled plates belongs to the coating and baking type. The passivation agent is applied to the surface of the strip by a rubber coating roller at room temperature, and then heated in a baking furnace for cross-linking and curing before it can finally form a film. The CSP hot-rolled galvanizing production line has a high production speed, and the passivation agents of patent types such as CN100510178 do not have sufficient reaction time and treatment temperature requirements when they come into contact with the surface of hot-rolled strip steel. Other reported patents or documents on trivalent chromium passivators suitable for uninterrupted rapid roller passivation treatment of steel plates mainly emphasize the corrosion resistance of the passivator based on cold-rolled hot-dip galvanized steel plates, and rarely involve the evaluation of wear resistance. For example, patent CN201610137541.8 reports a trivalent chromium passivator for uninterrupted rapid roller passivation treatment of cold-rolled hot-dip galvanized steel plates for automobiles. The passivator has good corrosion resistance, but does not evaluate the corrosion resistance and wear resistance of the steel plates after passivation of hot-rolled galvanized steel plates. Summary of the invention

[0009] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet and a preparation method thereof, wherein the emulsion can form a composite film layer after being coated on the hot-rolled galvanized sheet, wherein the composite film layer has excellent corrosion resistance and wear resistance, and also has excellent high temperature resistance, blackening resistance, alkali washing resistance, water resistance, defoaming resistance and solvent resistance. It is particularly worth mentioning that the trivalent chromium passivator studied in this patent belongs to an inorganic-organic composite system. The reason why it is suitable for hot-rolled sheet is that the acrylic emulsion with a high molecular wear-resistant hard segment prepared by the method can fully fill the rough and uneven areas of the hot-rolled sheet after film formation, and after being combined with a high-efficiency water-based wax additive, it plays a role in jointly improving the wear resistance of the film surface. In addition, due to the certain oxidizing properties of trivalent chromium salts, the trivalent chromium passivator of the traditional inorganic system often has poor adaptability after adding the organic resin emulsion. The present method greatly improves the stability of the agent by compounding it with an acrylic emulsion prepared by selecting modified silica sol and special functional monomers; the introduction of the organic resin part increases the actual effective thickness of the film after coating to a certain extent, providing a guarantee for the amount of film to fill the larger roughness areas of the hot-rolled plate.

[0010] In order to achieve at least one of the above advantages, the present invention provides a trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet, wherein each liter of the resin emulsion comprises:

[0011] To achieve at least one of the above advantages, the present invention provides a trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet, wherein each liter of the resin emulsion comprises the following % weight components:

[0012]

[0013]

[0014] Preferably, the preparation method of the nano-scale water-soluble molybdenum salt modified acidic silica sol includes: measuring the required deionized water into a beaker, then adding the prepared water-soluble molybdenum salt solution, and stirring moderately; then adding methanol and 7% volume ratio of vinyl silane, adjusting the pH value to 3.8-4.2, and stirring to fully hydrolyze, wherein the ratio of methanol to deionized water is 10:90.

[0015] Preferably, the preparation method of the aqueous cationic acrylic emulsion comprises: adding all acrylic monomers including acrylic hard monomer, acrylic soft monomer and acrylic functional monomer in the raw material, emulsifier and water into a pre-emulsification kettle, emulsifying for 30 to 40 minutes. Obtaining a non-stratified emulsion; then adding the remaining water, remaining emulsifier and buffer into a polymerization reactor, heating to 78 to 80°C, adding the emulsion, adding an initiator to react for 20 to 30 minutes, dripping the remaining emulsion and the remaining initiator prepared above, dripping for 3 to 4 hours; then heating the polymerization reactor to 85 to 90°C, keeping the temperature for 1 to 2 hours, cooling to 45 to 50°C, adding a pH adjuster to adjust the pH value of the reaction system to between 6 and 7, and obtaining an aqueous cationic acrylic emulsion.

[0016] Preferably, the trivalent chromium salt is a combination of 35% chromium nitrate aqueous solution and chromium phosphate.

[0017] Preferably, the compound acid is a combination of 75% phosphoric acid and citric acid.

[0018] Preferably, the water-soluble molybdenum salt is one or a combination of any of sodium molybdate, hydrated sodium dihydrogen phosphate, an appropriate amount of phosphoric acid and other additives.

[0019] According to another aspect of the present invention, the present invention provides a method for preparing a trivalent chromium-modified silane self-lubricating resin emulsion for hot-rolled galvanized sheet, which comprises the following steps:

[0020] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion in sequence, stir evenly, and obtain the trivalent chromium improved silane self-lubricating resin emulsion based on hot-rolled galvanized sheet.

[0021] Preferably, the preparation method of the water-soluble molybdenum salt solution comprises: first dissolving sodium molybdate with an appropriate amount of deionized water in a beaker to prepare a 5g / l sodium molybdate aqueous solution; then adding an appropriate amount of sodium dihydrogen phosphate and additives, supplementing deionized water and adjusting the pH value to 2.0-5.0 with phosphoric acid or sodium hydroxide.

[0022] Preferably, the preparation method of the nano-scale water-soluble molybdenum salt modified acidic silica sol is: measure the required deionized water into a beaker, then add the prepared water-soluble molybdenum salt solution, and stir moderately; then add methanol and 7% volume ratio of vinyl silane, adjust the pH value to 4, and stir to fully hydrolyze, wherein the ratio of methanol to deionized water is 10:90.

[0023] Preferably, the preparation method of the water-based cationic acrylic resin is as follows: add all acrylic monomers including acrylic hard monomer, acrylic soft monomer and acrylic functional monomer in the raw material, emulsifier and water into the pre-emulsification kettle, emulsify for 30 to 40 minutes. Obtain a non-stratified emulsion; then add the remaining water, remaining emulsifier and buffer into the polymerization kettle, heat it to 78 to 80°C, put in the emulsion, add the initiator to react for 20 to 30 minutes, drop the remaining emulsion and the remaining initiator prepared above, and drip it for 3 to 4 hours; then heat the polymerization kettle to 85 to 90°C to keep the temperature for 1 to 2 hours, cool it to 45 to 50°C, add the pH adjuster to adjust the pH value of the reaction system to between 6 and 7, and obtain the water-based cationic acrylic emulsion. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of a stamping part of a galvanized sheet according to Example 4 of the present invention is shown.

[0025] Figure 2 The defoaming performance schematic diagram of Example 4 and each comparative example is shown.

[0026] Figure 3 and Figure 4 A schematic diagram showing the salt spray results of galvanized sheets at different chromium contents in Example 4 of the present invention is shown. DETAILED DESCRIPTION

[0027] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0028] A trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet according to a preferred embodiment of the present invention will be described in detail below, wherein in the trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet, each liter of the resin emulsion includes the following % weight components:

[0029]

[0030] It is worth mentioning that in the resin emulsion, the trivalent chromium salt ion is the main component of the composite film when the resin emulsion forms a composite film in the later stage, and constitutes the skeleton of the composite film, so that the composite film has corrosion resistance.

[0031] In addition, the addition of molybdate ions is particularly beneficial for improving the corrosion resistance of the composite film, because molybdenum ions can be firmly combined with the surface of the hot-rolled galvanized sheet substrate by chemical bonding, which helps to improve the corrosion resistance.

[0032] It is also worth mentioning that the role of the nano-scale water-soluble molybdenum salt modified acidic silica sol is to give the composite film alkali resistance, high temperature resistance and further improve the corrosion resistance of the composite film. During the film formation process of the trivalent chromium composite film on the surface of the hot-rolled galvanized sheet, the silica sol is filled in the skeleton formed by the trivalent chromium ions, making the passivation film denser, thereby improving the alkali resistance, high temperature resistance and corrosion resistance of the passivation film.

[0033] In addition, the aqueous cationic acrylic emulsion is the film-forming substance in the composite film layer. By being intricately interwoven with trivalent chromium ions, molybdenum ions, and silica sol, the composite film is endowed with resistance to blackening, water resistance, solvent resistance, and better flexibility and density. Compared with the same type of resin, the homemade aqueous acrylic emulsion can overcome the shortcomings of the composite film, such as brittleness and poor ductility, and helps to improve the ductility of the upper composite film after being subjected to stress.

[0034] Furthermore, the high-efficiency water-based wax emulsion can improve the excellent wear resistance and water resistance of the composite film layer, improve the surface roughness of the hot-rolled galvanized thick plate, and increase the smoothness and scratch resistance of the composite film layer; in addition, the selected water-based wax emulsion must have good compatibility with the system, and the foam can be quickly and effectively eliminated after stirring.

[0035] That is to say, compared with the prior art, the advantages and beneficial effects of the present invention are as follows: trivalent chromium ions and nano-modified acidic silica sol give the trivalent chromium passivator basic properties such as corrosion resistance, high temperature resistance, and alkali resistance; molybdenum ions are firmly combined with the surface of the hot-rolled galvanized sheet substrate by chemical bonding, which helps to improve the corrosion resistance of the trivalent chromium composite film layer. The addition of aqueous cationic acrylic emulsion gives the composite film layer better flexibility and density, while the acrylic resin is intricately interwoven with trivalent chromium ions, molybdenum ions, and silica sol, giving the composite film layer resistance to blackening, water resistance, and solvent resistance. The introduction of high-efficiency aqueous wax emulsion gives the composite film layer excellent wear resistance and water resistance, improves the surface roughness of hot-rolled galvanized thick plates, and increases the smoothness and scratch resistance of the composite coating. In addition, the composite film layer formed by the trivalent chromium-modified silane self-lubricating resin emulsion based on the hot-rolled galvanized sheet has excellent corrosion resistance and wear resistance, and other various properties such as alkali resistance, solvent resistance, water resistance, yellowing resistance, and blackening resistance also fully meet the requirements, thereby overcoming the shortcomings of poor corrosion resistance and wear resistance of ordinary trivalent chromium passivation liquid for thick plates with greater roughness in the hot-rolled galvanizing process.

[0036] In one embodiment, the preparation method of the nano-scale water-soluble molybdenum salt modified acidic silica sol includes: measuring the required deionized water in a beaker, then adding the prepared water-soluble molybdenum salt solution, and stirring moderately; then adding methanol and 7% volume ratio of vinyl silane, adjusting the pH value to 3.8-4.2, stirring to fully hydrolyze, wherein the ratio of methanol to deionized water is 10:90. Methanol, as a polar protic solvent, can act as a physical latent solvent in hydrophilic silanes that can be hydrolyzed to increase their solubility in water and thus accelerate the hydrolysis rate; in addition, the addition of methanol can play a protective role, prevent the polymerization reaction between silane molecules, and make the hydrolysis product easier to control and separate. However, the amount of methanol added cannot be too high, usually accounting for about 10% of the water volume of the system, which can effectively control the volatile organic content of the entire system not to exceed the standard.

[0037] In one embodiment, the preparation method of the aqueous cationic acrylic emulsion comprises: adding all acrylic monomers including acrylic hard monomer, acrylic soft monomer and acrylic functional monomer in the raw material, emulsifier and water into a pre-emulsification kettle, emulsifying for 30 to 40 minutes. Obtaining a non-stratified emulsion; then adding the remaining water, remaining emulsifier and buffer into a polymerization reactor, heating to 78 to 80°C, adding the emulsion, adding an initiator to react for 20 to 30 minutes, dripping the remaining emulsion and the remaining initiator prepared above, dripping for 3 to 4 hours; then heating the polymerization reactor to 85 to 90°C to keep the temperature for 1 to 2 hours, cooling to 45 to 50°C, adding a pH adjuster to adjust the pH value of the reaction system to between 6 and 7, and obtaining an aqueous cationic acrylic emulsion.

[0038] Preferably, the trivalent chromium salt is a combination of 35% chromium nitrate aqueous solution and chromium phosphate.

[0039] Preferably, the compound acid is a combination of 75% phosphoric acid and citric acid.

[0040] Preferably, the water-soluble molybdenum salt is one or a combination of any of sodium molybdate, hydrated sodium dihydrogen phosphate, an appropriate amount of phosphoric acid and other additives.

[0041] According to another aspect of the present invention, the present invention also provides a trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet, which comprises the following steps:

[0042] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion in sequence, stir evenly, and obtain the trivalent chromium improved silane self-lubricating resin emulsion based on hot-rolled galvanized sheet.

[0043] In one embodiment, the preparation method of the water-soluble molybdenum salt solution includes: first dissolving sodium molybdate with an appropriate amount of deionized water in a beaker to prepare a 5g / l sodium molybdate aqueous solution; then adding an appropriate amount of sodium dihydrogen phosphate and additives, supplementing deionized water and adjusting the pH value to 2.0-5.0 with phosphoric acid or sodium hydroxide.

[0044] In one embodiment, the preparation method of the nano-scale water-soluble molybdenum salt modified acidic silica sol is: measure the required deionized water into a beaker, then add the prepared water-soluble molybdenum salt solution, and stir moderately; then add methanol and 7% volume ratio of vinyl silane, adjust the pH value to 3.8-4.2, and stir to fully hydrolyze, wherein the ratio of methanol to deionized water is 10:90.

[0045] In one embodiment, the preparation method of the water-based cationic acrylic resin is as follows: add all acrylic monomers including acrylic hard monomer, acrylic soft monomer and acrylic functional monomer in the raw material, emulsifier and water into the pre-emulsification kettle, emulsify for 30 to 40 minutes. Obtain a non-stratified emulsion; then add the remaining water, remaining emulsifier and buffer into the polymerization kettle, heat it to 78 to 80°C, put in the emulsion, add the initiator to react for 20 to 30 minutes, drop the remaining emulsion and the remaining initiator prepared above, and drip it for 3 to 4 hours; then heat the polymerization kettle to 85 to 90°C to keep the temperature for 1 to 2 hours, cool it to 45 to 50°C, add the pH adjuster to adjust the pH value of the reaction system to between 6 and 7, and obtain the water-based cationic acrylic emulsion.

[0046] Example 1

[0047] A trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet includes the components shown in the following table:

[0048] materials Weight Percent Pure water 33.53 35% chromium nitrate aqueous solution 21 Chromium phosphate 9 Phosphoric acid 75% 4 Citric acid 0.5 Pure water 24.47 Water-based cationic acrylic emulsion 6 Nano-scale modified acidic silica sol 1 AQUACER539 water-based wax emulsion 0.5

[0049] The preparation method of the above-mentioned trivalent chromium improved silane self-lubricating resin emulsion based on hot-rolled galvanized sheet is as follows:

[0050] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion AQUACER539 in sequence, stir evenly, and obtain the trivalent chromium-modified silane self-lubricating resin composite film layer based on hot-rolled galvanized sheet.

[0051] Example 2

[0052] A trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet includes the components shown in the following table:

[0053]

[0054]

[0055] The preparation method of the trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet comprises:

[0056] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion AQUACER539 in sequence, stir evenly, and obtain the trivalent chromium-modified silane self-lubricating resin composite film layer based on hot-rolled galvanized sheet.

[0057] Example 3

[0058] A trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet includes the components shown in the following table:

[0059] materials Weight Percent Pure water 33.53 35% chromium nitrate aqueous solution 21 Chromium phosphate 9 Phosphoric acid 75% 4 Citric acid 0.5 Pure water 17.47 Water-based cationic acrylic emulsion 10 Nano-scale modified acidic silica sol 3 AQUACER539 water-based wax emulsion 1.5

[0060] The preparation method of the trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet comprises:

[0061] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion AQUACER539 in sequence, stir evenly, and obtain the trivalent chromium-modified silane self-lubricating resin composite film layer based on hot-rolled galvanized sheet.

[0062] Example 4

[0063] A trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet includes the components shown in the following table:

[0064]

[0065]

[0066] The preparation method of the trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet comprises:

[0067] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion AQUACER539 in sequence, stir evenly, and obtain the trivalent chromium-modified silane self-lubricating resin composite film layer based on hot-rolled galvanized sheet.

[0068] Comparative Example 1

[0069] A lotion, composed of the following ingredients:

[0070] materials Weight Percent Pure water 33.53 35% chromium nitrate aqueous solution 21 Chromium phosphate 9 Phosphoric acid 75% 4 Citric acid 0.5 Pure water 17.97 Water-based cationic acrylic emulsion 10 Nano-scale modified acidic silica sol 3 Tianshi LW150 water-based wax emulsion 1.0

[0071] The preparation method of the above emulsion comprises:

[0072] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion LW150 in sequence, stir evenly, and obtain the trivalent chromium-modified silane self-lubricating resin composite film layer based on hot-rolled galvanized sheet.

[0073] Comparative Example 1

[0074] A lotion, composed of the following ingredients:

[0075]

[0076] The preparation method of the above emulsion comprises:

[0077] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion WR 40AD in sequence, stir evenly, and obtain the trivalent chromium modified silane self-lubricating resin composite film layer based on hot-rolled galvanized sheet.

[0078] Comparative Example 3

[0079] A lotion, composed of the following ingredients:

[0080]

[0081]

[0082] The preparation method of the above emulsion comprises:

[0083] Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion 846 in sequence, stir evenly to obtain the trivalent chromium-modified silane self-lubricating resin composite film layer based on hot-rolled galvanized sheet.

[0084] Effect evaluation of the film-forming effect of the trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet of the present invention:

[0085] 1. Passivation treatment method for hot-rolled galvanized steel sheet

[0086] a) Pre-cleaning

[0087] To ensure the passivation effect, the hot-rolled galvanized steel sheet is pre-cleaned before the passivation agent is applied. The purpose of pre-cleaning is to remove the adhered anti-rust oil and other grease components to ensure that the trivalent chromium-modified silane self-lubricating resin composite film is evenly distributed on the surface of the steel sheet. The reference method for pre-cleaning is: clean the hot-rolled galvanized steel sheet by soaking it in a moderately alkaline degreasing agent, then rinse it with tap water, then rinse it with deionized water, and then blow it dry with hot air;

[0088] b) Coating

[0089] The trivalent chromium-modified silane self-lubricating resin emulsion based on the hot-rolled galvanized sheet is coated on the surface of the hot-rolled galvanized steel sheet by using an Onkel rod scraping method, and the film layer formed by the trivalent chromium-modified silane self-lubricating resin emulsion based on the hot-rolled galvanized sheet has a dry film single-sided thickness of 30 to 70 mg / m2 of Cr content by adjusting the dilution ratio and the contact pressure between the scraper and the hot-rolled galvanized steel sheet;

[0090] c) Drying

[0091] Drying may be preferably carried out at a temperature range of from 50°C to 150°C peak metal temperature (PMT), preferably at a temperature range of 70 to 100°C;

[0092] 2. Test methods

[0093] 1) Salt spray resistance test

[0094] The salt spray test is carried out in accordance with the national standard "GB / T 10125-2012 Artificial atmosphere corrosion test salt spray test", the test temperature is 35±2°C, the NaCl concentration is 50±5g / l, and the test piece coated with the composite film layer formed by the trivalent chromium-modified silane self-lubricating resin emulsion based on the hot-rolled galvanized sheet of the present invention is recorded after 72 hours of salt spray resistance test to see whether the plate surface meets the requirement of white rust area less than 5%;

[0095] 2) Alkali resistance test

[0096] Soak the passivated sample in 1% degreasing agent at 55°C for 2 minutes. Take it out and blow it dry, observe whether the surface color of the sample changes, and measure the color difference before and after the test with Mirinda precision colorimeter;

[0097] 3)Solvent resistance test

[0098] Wipe the passivated sample surface back and forth 20 times with butanone and 80% alcohol at a force of 500g. Observe the appearance and use Mirinda precision colorimeter to measure the color difference of the sample before and after wiping;

[0099] 4) Water resistance test

[0100] Drop a few drops of water on the passivation film layer with 100°C boiling water. After the water drops are naturally dried in the air, no white powdery substance appears on the passivation film layer. The composite film layer formed by the trivalent chromium-modified silane self-lubricating resin emulsion based on the hot-rolled galvanized sheet is not damaged by water immersion and is qualified.

[0101] 5) Yellowing resistance test

[0102] Place the passivated galvanized sheet in a 250℃ hot air oven and bake for 20 minutes. Observe the appearance and use a Mirinda precision colorimeter to measure the color difference of the sample before and after baking.

[0103] 6) Moisture and heat resistance test

[0104] Place the passivated galvanized sheet in a constant temperature and humidity chamber at 50°C and 98% humidity for 120 hours, then take it out and use a Mirinda precision colorimeter to measure the color difference of the sample before and after storage;

[0105] 7) Abrasion resistance test

[0106] Use a special mold to conduct deep drawing test on the passivated galvanized sheet to observe whether the composite film layer on the surface of the deep-drawn part, especially in the stress deformation area, is intact and whether there is any friction black line;

[0107] 8) Defoaming performance of pharmaceuticals

[0108] Place 20ml of the original solution in a measuring cylinder, shake it up and down 10 times, and observe the foam height after standing for 10 minutes. The height should be less than 2ml.

[0109] 3. Evaluation criteria

[0110] The evaluation criteria for each relevant performance are shown in Table 1 below:

[0111] Table 1: Evaluation criteria for the composite film layer

[0112]

[0113]

[0114] 4. Sample testing

[0115] The solid content of the composite film layer prepared in Examples 1-4 and the trivalent chromium composite film layer prepared in Comparative Examples 1-3 was adjusted to 40% (adjusted by diluting with water), and the hot-rolled galvanized steel sheets with a thickness of 1.5 mm were tested with the trivalent chromium composite film layers prepared in Examples 1-4 and Comparative Examples 1-3. Each hot-rolled galvanized steel sheet was pre-cleaned first, and then coated with a passivating agent using a 3# Wengkel coating wire rod, and then dried at a drying temperature of 250°C and a peak metal temperature (PMT) of 77°C to obtain a single-sided dry film thickness with a Cr content of 30 to 70 mg / m2. After the passivation treatment of each hot-rolled galvanized steel sheet was completed, each related performance test was performed after being placed for 24 hours;

[0116] 5. Test results:

[0117] Table 2 Test results of the composite film layer formed by each emulsion

[0118]

[0119] It can be seen from the test data in Table 2 above that the trivalent chromium composite film layer of Example 4 prepared in the present invention meets the requirements in various film performance tests, has excellent corrosion resistance and wear resistance, and other various properties such as alkali resistance, solvent resistance, water resistance, yellowing resistance, and moisture and heat resistance also fully meet the requirements, and the defoaming performance of the agent is also excellent.

[0120] The corrosion resistance, alkali resistance, solvent resistance, water resistance, moisture and heat resistance and wear resistance of Example 1 and Example 2 do not meet the performance requirements; the yellowing resistance of Example 3 is poor; the defoaming performance of the agents of Comparative Examples 1, 2 and 3 is unqualified.

[0121] It is worth mentioning that the proportion of the aqueous emulsified wax added in Example 4 is 1%, and the stamping parts coated with the composite film layer formed by the emulsion have no film shedding and friction black lines. Figure 1 .

[0122] It should be understood by those skilled in the art that the embodiments of the present invention described above and shown in the accompanying drawings are only examples and do not limit the present invention. The advantages of the present invention have been fully and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.

Claims

1. Trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet, It is characterized in that Wherein each liter of the resin emulsion comprises the following % weight components:

2. The trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet according to claim 1, It is characterized in that The preparation method of the nano-scale water-soluble molybdenum salt modified acidic silica sol comprises: measuring the required deionized water into a beaker, then adding the prepared water-soluble molybdenum salt solution, and stirring moderately; then adding methanol and 7% by volume vinyl silane, adjusting the pH value to 3.8-4.2, and stirring to fully hydrolyze, wherein the ratio of methanol to deionized water is 10:

90.

3. The trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet according to claim 1, It is characterized in that The preparation method of the aqueous cationic acrylic emulsion comprises: adding all acrylic monomers including acrylic hard monomer, acrylic soft monomer and acrylic functional monomer in the raw materials, emulsifier and water into a pre-emulsification kettle, emulsifying for 30-40 minutes, obtaining an emulsion without stratification; then adding the remaining water, remaining emulsifier and buffer into a polymerization reactor, heating to 78-80°C, adding the emulsion, adding an initiator to react for 20-30 minutes, dripping the remaining emulsion and the remaining initiator prepared above, dripping for 3-4 hours; then heating the polymerization reactor to 85-90°C, keeping the temperature for reaction for 1-2 hours, cooling to 45-50°C, adding a pH adjuster to adjust the pH value of the reaction system to between 6 and 7, and obtaining the aqueous cationic acrylic emulsion.

4. The trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet according to claim 1, It is characterized in that The trivalent chromium salt is a combination of a 35% chromium nitrate aqueous solution and chromium phosphate.

5. The trivalent chromium improved silane self-lubricating resin emulsion based on hot-rolled galvanized sheet according to claim 1, It is characterized in that The compound acid is a combination of 75% phosphoric acid and citric acid.

6. The trivalent chromium-modified silane self-lubricating resin emulsion based on hot-rolled galvanized sheet according to claim 1, It is characterized in that The water-soluble molybdenum salt is one of sodium molybdate, hydrated sodium dihydrogen phosphate, an appropriate amount of phosphoric acid and other additives, or a combination of any of them.

7. A method for preparing a trivalent chromium-modified silane self-lubricating resin emulsion for hot-rolled galvanized sheet, The following steps are involved: Add trivalent chromium salt, compound acid and water into a reaction container, stir to dissolve, then add nano-scale water-soluble molybdenum salt modified acidic silica sol, aqueous cationic acrylic emulsion and aqueous wax emulsion in sequence, stir evenly, and obtain the trivalent chromium improved silane self-lubricating resin emulsion based on hot-rolled galvanized sheet.

8. The method for preparing the trivalent chromium improved silane self-lubricating resin emulsion for hot-rolled galvanized sheet according to claim 7, It is characterized in that The preparation method of the water-soluble molybdenum salt solution comprises: firstly dissolving sodium molybdate with an appropriate amount of deionized water in a beaker to prepare a 5g / l sodium molybdate aqueous solution; then adding an appropriate amount of sodium dihydrogen phosphate and additives, supplementing deionized water and adjusting the pH value to 2.0-5.0 with phosphoric acid or sodium hydroxide.

9. The method for preparing the trivalent chromium improved silane self-lubricating resin emulsion for hot-rolled galvanized sheet according to claim 7, It is characterized in that The preparation method of the nano-scale water-soluble molybdenum salt modified acidic silica sol is as follows: measure the required deionized water into a beaker, then add the prepared water-soluble molybdenum salt solution, and stir moderately; then add methanol and 7% by volume vinyl silane, adjust the pH value to 4, and stir to fully hydrolyze, wherein the ratio of methanol to deionized water is 10:

90.

10. The method for preparing the trivalent chromium improved silane self-lubricating resin emulsion for hot-rolled galvanized sheet according to claim 7, It is characterized in that The preparation method of the water-based cationic acrylic resin is as follows: all acrylic monomers including acrylic hard monomers, acrylic soft monomers and acrylic functional monomers in the raw materials, emulsifiers and water are added into a pre-emulsification kettle, emulsified for 30-40 minutes, and a non-stratified emulsion is obtained; then the remaining water, remaining emulsifiers and buffer are added into a polymerization reaction kettle, the temperature is raised to 78-80° C., the emulsion is added, an initiator is added to react for 20-30 minutes, the remaining emulsion prepared above and the remaining initiator are dripped, and the dripping is completed within 3-4 hours; then the polymerization reaction kettle is heated to 85-90° C., the temperature is kept to react for 1-2 hours, the temperature is lowered to 45-50° C., a pH adjuster is added to adjust the pH value of the reaction system to between 6 and 7, and the water-based cationic acrylic emulsion is obtained.

Citation Information

Patent Citations

  • Galvanized self-lubricating metal material

    CN101608311A

  • Hot galvanized plate coating solution and preparation and using methods thereof

    CN106283009A

  • Cationic metal surface treatment emulsion and preparation method thereof

    CN106543350A

  • Anti-rust anti-corrosion self-cleaning finishing paint preparation method

    CN107043581A

  • High-corrosion-resistance hot galvanizing passivation solution and preparation method thereof

    CN112481574A