Carbon nitride-initiated interface hydrogel coating as well as preparation method and application thereof
The interfacial hydrogel coating technology initiated by carbon nitride and dopamine adhesive polymers under visible light solves the problems of insufficient function of traditional hydrogel materials and harmful metal ions in extreme environments, and realizes the functionalization and biotechnology of the substrate. Compatibility, suitable for marine antifouling and medical devices.
Patent Information
- Application Number
- CN202410948074.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-16
AI Technical Summary
Traditional hydrogel materials cannot meet functional requirements such as anti-fouling, anti-corrosion, low friction, and high wear resistance in extremely harsh environments, and the existing technology uses metal ion initiators that are harmful to the human body and cannot achieve the purpose of protecting the substrate surface. Effective functionalization.
Using carbon nitride as the sole initiator, the interfacial hydrogel coating is formed by mixing with dopamine adhesive polymer and performing a second radical polymerization reaction under visible light irradiation to achieve functionalization and biocompatibility of the substrate.
It realizes the functionalization of the substrate surface, provides good lubrication ability and biocompatibility, is suitable for marine antifouling and biomedical devices, and avoids the problems of high energy and equipment cost caused by the use of ultraviolet light.
Smart Images

Figure CN118725675A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a carbon nitride-induced interfacial hydrogel coating and a preparation method and application thereof. Background Art
[0002] Hydrogel materials are a type of water-containing three-dimensional network formed by physical or chemical interactions of hydrophilic polymer chains. They are "soft" and "wet", but their own soft properties often cannot meet the needs of some extremely harsh application environments. Although traditional materials such as metals, glass, ceramics, plastics, silicone rubber, etc. can adapt to some harsh environments, their surface properties often cannot meet the special functional requirements of applications, such as anti-fouling, anti-corrosion, drag reduction, low friction and high wear resistance, which limits their respective application scopes. Hydrogel coating technology combines the characteristics of the substrate material with the functional surface properties. Without changing the bulk properties of the traditional material, the functional hydrogel is combined with the traditional material through surface bonding, giving the surface unique properties and making up for the shortcomings of the surface properties of traditional materials.
[0003] As one of the most promising metal-free photocatalysts, graphite carbon nitride (g-C3N4) has a suitable energy band gap (2.7 eV) and excellent physical and chemical stability. Existing technologies usually use g-C3N4 and co-initiators to initiate monomer polymerization for the preparation of bulk hydrogels. However, after the bulk hydrogel is prepared, it is impossible to modify the interface, and it is also impossible to achieve functionalization of the substrate surface, which has limitations in application. Furthermore, the current in situ growth of hydrogels mainly uses metal ions (Fe 3 + ) is achieved through redox, but in the medical field, metal ions (Fe 3+ ) is harmful to the human body. Summary of the invention
[0004] The purpose of the present invention is to provide an interfacial hydrogel coating initiated by carbon nitride, and a preparation method and application thereof. The present invention uses carbon nitride as the only initiator to prepare an interfacial hydrogel coating, which can realize the coating of hydrogel, can perform interface modification on different substrates, realize the functionalization of the substrate, and has a wide range of applications; and the interfacial hydrogel coating thus obtained has good lubricity and biocompatibility.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a carbon nitride-induced interfacial hydrogel coating, comprising the following steps:
[0007] The carbon nitride and the dopamine adhesion polymer are mixed and coated on the surface of the substrate to form a dopamine adhesion bonding layer containing an initiator on the surface of the substrate to obtain an initiator-modified substrate; the dopamine adhesion polymer is prepared by a first free radical polymerization reaction of dopamine methacrylamide and methoxyethyl acrylate;
[0008] The initiator-modified substrate is immersed in a polymer monomer solution, and a second free radical polymerization reaction is carried out under visible light irradiation to form an interfacial hydrogel coating initiated by carbon nitride on the surface of the substrate.
[0009] Preferably, the mass of the carbon nitride is 0.025-0.5% of the total mass of the carbon nitride and the dopamine adhesion polymer.
[0010] Preferably, the substrate includes a metal substrate, a glass substrate, a ceramic substrate, a plastic substrate or a silicone rubber substrate.
[0011] Preferably, the temperature of the first free radical polymerization reaction is 60-65° C., and the time is 12-15 hours.
[0012] Preferably, the polymer monomer in the polymer monomer-containing solution includes at least one of acrylic acid, acrylamide, hydroxyethyl methacrylate, N-isopropylacrylamide and sulfobetaine methacrylate.
[0013] Preferably, the concentration of the polymer monomer in the polymer monomer solution is 20 to 500 mg / mL.
[0014] Preferably, the wavelength of the visible light is 460-465 nm.
[0015] Preferably, the second free radical polymerization reaction is carried out under a nitrogen atmosphere, the temperature of the second free radical polymerization reaction is 20-35° C., and the time does not exceed 90 min.
[0016] The present invention provides a carbon nitride-induced interfacial hydrogel coating obtained by the preparation method described in the above technical solution.
[0017] The present invention provides the application of the carbon nitride-induced interfacial hydrogel coating described in the above technical solution in marine antifouling or biomedical devices.
[0018] The present invention provides a method for preparing an interfacial hydrogel coating initiated by carbon nitride, comprising the following steps: mixing carbon nitride with a dopamine adhesion polymer and coating the mixture on the surface of a substrate, forming a dopamine adhesion bonding layer containing an initiator on the surface of the substrate, and obtaining an initiator-modified substrate; the dopamine adhesion polymer is prepared by a first free radical polymerization reaction of dopamine methacrylamide and methoxyethyl acrylate; immersing the initiator-modified substrate in a polymer monomer solution, and performing a second free radical polymerization reaction under visible light irradiation to form a hydrogel coating on the surface of the substrate. The present invention uses carbon nitride as the only initiator, and induces the polymer monomer to produce free radical polymerization under visible light irradiation to form an interfacial hydrogel coating; at the same time, the dopamine adhesion polymer can promote the absorption of visible light by carbon nitride and the rapid separation and transfer of charges, and the network topological entanglement between the hydrogel and the dopamine adhesion bonding layer ensures good bonding between stable interfaces, thereby improving the versatility of the substrate. The present invention avoids using ultraviolet light for initiation, but uses visible light for initiation, wherein visible light initiation requires lower energy, has higher irradiation safety, is more conducive to realizing engineering applications, and reduces equipment costs; and polymerization reaction and hydrogel growth only occur at the solid-liquid contact interface, and no polymerization reaction occurs in the bulk reaction solution. Furthermore, the preparation method of the present invention is simple to operate and has a wide range of applications. The interfacial hydrogel coating obtained thereby has good lubrication ability. The examples show that the average friction coefficient of the acrylamide / acrylic acid hydrogel coating prepared by the present invention is below 0.05.
[0019] Moreover, the present invention introduces metal-free photocatalyst carbon nitride as an initiator into the dopamine adhesion bonding layer to grow a hydrogel coating in situ, so that the hydrogel is combined with traditional materials, giving the traditional material surface unique properties. Specifically, the present invention uses carbon nitride as the only initiator, utilizes the adhesion of dopamine adhesion polymer and the role of enhancing the separation and transfer of photogenerated electrons and holes, and initiates the polymerization reaction of the hydrogel at the interface to make it grow in situ. The present invention uses carbon nitride as an initiator to achieve hydrogel coating, and can perform interface modification on different substrates to achieve functionalization of the substrate, with a wide range of applications. The interfacial hydrogel coating obtained according to the preparation method provided by the present invention has good lubrication ability and biocompatibility, is environmentally friendly, and has good anti-fouling properties. Therefore, the interfacial hydrogel coating has broad application prospects in marine anti-fouling, biomedicine and other aspects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0021] Figure 1 This is a graph showing the growth process of the interfacial hydrogel coating obtained in Example 1 over time;
[0022] Figure 2 is a growth kinetic diagram of the interfacial hydrogel coating obtained in Examples 1 to 5;
[0023] Figure 3 This is a graph showing the test results of the surface average friction coefficient of the interfacial hydrogel coating obtained in Example 1 at different growth times;
[0024] Figure 4 This is a graph showing the antifouling effect of a blank glass sheet and the interfacial hydrogel coating obtained in Example 1 of the present invention on Ampelopsis pilosa. DETAILED DESCRIPTION
[0025] The present invention provides a method for preparing a carbon nitride-induced interfacial hydrogel coating, comprising the following steps:
[0026] The carbon nitride and the dopamine adhesion polymer are mixed and coated on the surface of the substrate to form a dopamine adhesion bonding layer containing an initiator on the surface of the substrate to obtain an initiator-modified substrate; the dopamine adhesion polymer is prepared by a first free radical polymerization reaction of dopamine methacrylamide and methoxyethyl acrylate;
[0027] The initiator-modified substrate is immersed in a polymer monomer solution, and a second free radical polymerization reaction is carried out under visible light irradiation to form an interfacial hydrogel coating initiated by carbon nitride on the surface of the substrate.
[0028] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or are prepared by methods well known to those skilled in the art.
[0029] In the present invention, the substrate preferably includes a metal substrate, a glass substrate, a ceramic substrate, a plastic substrate or a silicone rubber substrate; the metal substrate is preferably an iron substrate, a copper substrate or an aluminum substrate; the plastic substrate is preferably a polypropylene substrate, a polyethylene substrate or a polytetrafluoroethylene substrate; the silicone rubber substrate is preferably a polydimethylsiloxane substrate.
[0030] In the present invention, the carbon nitride is used as an initiator. The method for preparing carbon nitride according to the present invention preferably comprises the following steps: calcining urea to obtain the carbon nitride. In the present invention, the calcination temperature is preferably 500-550°C, more preferably 525-550°C; the holding time is preferably 2-4h, more preferably 4h; the rate of heating to the calcination temperature is preferably 5-10°C / min, more preferably 10°C / min. After the calcination is completed, the present invention preferably cools the obtained material to room temperature and obtains the carbon nitride after grinding. The particle size of the carbon nitride according to the present invention is preferably 100-200nm, more preferably 100-150nm.
[0031] In the present invention, the dopamine adhesion polymer is prepared by a first free radical polymerization reaction of dopamine methacrylamide and methoxyethyl acrylate. The preparation method of the dopamine adhesion polymer of the present invention preferably comprises the following steps: mixing dopamine hydrochloride, triethylamine and methacryloyl chloride, and performing an amidation reaction to obtain dopamine methacrylamide; mixing the dopamine methacrylamide with methoxyethyl acrylate and azobisisobutyronitrile, and performing a first free radical polymerization reaction to obtain the dopamine adhesion polymer. The preparation method of the dopamine adhesion polymer of the present invention refers to the following literature: Zhang Y, Xu R, Zhao W, et al. Successive redox-reaction-triggered interface radical polymerization for growing hydrogel coatings on diverse substrates. Angewandte Chemie, 2022, 134(39): e202209741.
[0032] The present invention mixes dopamine hydrochloride, triethylamine and methacryloyl chloride, and performs an amidation reaction to obtain dopamine methacrylamide. In the present invention, the material-liquid ratio of dopamine hydrochloride, triethylamine and methacryloyl chloride is preferably 8-10g:7-7.5g:5-6mL, and more preferably 10g:7.2g:6mL. In the present invention, dopamine hydrochloride and triethylamine are preferably dissolved in methanol, and ice-bathed in a nitrogen atmosphere to obtain a mixed solution; then methacryloyl chloride solution is dripped into the mixed solution, and the timing is started after the methacryloyl chloride solution is dripped, and the amidation reaction is performed. In the present invention, the ice bath time is preferably 10-20min, and more preferably 20min; the dripping time is preferably 0.5-1h, and more preferably 1h; the methacryloyl chloride solution preferably includes methacryloyl chloride and dichloromethane, and the volume ratio of methacryloyl chloride and dichloromethane is preferably 4-6:3-4, and more preferably 6:4. In the present invention, the temperature of the amidation reaction is preferably 0-5°C, more preferably 0°C; the time is preferably 1-2h, more preferably 2h. In an embodiment of the present invention, the amidation reaction is carried out under ice bath conditions. After the amidation reaction is completed, the present invention preferably removes the solvent of the obtained feed solution, dissolves the obtained material in ethyl acetate and extracts it with hydrochloric acid and saturated brine respectively, collects the organic phase and sequentially dries and recrystallizes it to obtain dopamine methacrylamide. In the present invention, the method of removing the solvent of the obtained feed solution is preferably rotary evaporation; the number of extractions with hydrochloric acid is preferably 3 times; the number of extractions with saturated brine is preferably 3 times. The drying of the present invention preferably includes sequential drying of anhydrous MgSO4 and rotary evaporation; after the drying of anhydrous MgSO4, anhydrous MgSO4 is preferably removed by filtration. In the present invention, the purpose of drying anhydrous MgSO4 is to remove water in the system; the purpose of rotary evaporation is to remove ethyl acetate in the system. The reagent used for recrystallization of the present invention is preferably a mixed solvent of ethyl acetate and n-hexane; in the mixed solvent, the volume ratio of ethyl acetate to n-hexane is preferably 1-2:1-2, more preferably 1:2.
[0033] After obtaining dopamine methacrylamide, the present invention mixes the dopamine methacrylamide with methoxyethyl acrylate and azobisisobutyronitrile to perform a first free radical polymerization reaction to obtain the dopamine adhesion polymer. In the present invention, the mass ratio of dopamine methacrylamide, methoxyethyl acrylate and azobisisobutyronitrile is preferably 0.01-8.3:4.8-9.6:0.1-0.11, and more preferably 1.7:7.5:0.106. In the present invention, dopamine methacrylamide, methoxyethyl acrylate and azobisisobutyronitrile are preferably mixed with N,N-dimethylformamide to perform a first free radical polymerization reaction. In the present invention, the first free radical polymerization reaction is preferably carried out under a nitrogen atmosphere; the temperature is preferably 60-65°C, and more preferably 65°C; the time is preferably 12-15h, and more preferably 12h. After the first free radical polymerization reaction, the present invention preferably sequentially performs petroleum ether precipitation, ethyl acetate dissolution and drying on the obtained feed liquid to obtain a dopamine adhesion polymer. In the present invention, the number of precipitation and dissolution is preferably 3 times independently; and the drying is preferably vacuum drying.
[0034] The present invention mixes carbon nitride with a dopamine adhesion polymer and then applies it to the surface of a substrate, forming a dopamine adhesion bonding layer containing an initiator on the surface of the substrate to obtain an initiator-modified substrate. The present invention preferably dissolves the dopamine adhesion polymer in dichloromethane to obtain a dissolving solution; adds carbon nitride to the dissolving solution and then ultrasonically disperses it, applies the obtained mixed material on the surface of the substrate, and dries it to obtain a dopamine adhesion bonding layer containing carbon nitride on the surface of the substrate. In the present invention, the mass of the carbon nitride is preferably 0.025-0.5% of the total mass of the carbon nitride and the dopamine adhesion polymer, and more preferably 0.05-0.3% of the total mass of the carbon nitride and the dopamine adhesion polymer. In the present invention, the time of the ultrasonic dispersion is preferably 10-30 minutes, and more preferably 30 minutes; the coating thickness of the mixed material is preferably 5-35 μm, and more preferably 5-20 μm; the drying is preferably vacuum drying, and the drying time is preferably 24 hours.
[0035] After obtaining the initiator-modified substrate, the present invention immerses the initiator-modified substrate in a polymer monomer solution, performs a second free radical polymerization reaction under visible light irradiation, and forms a hydrogel coating on the surface of the substrate.
[0036] In the present invention, the polymer monomer in the polymer monomer solution preferably includes at least one of acrylic acid, acrylamide, hydroxyethyl methacrylate, N-isopropyl acrylamide and sulfobetaine methacrylate, and the concentration of the polymer monomer in the polymer monomer solution is preferably 20-500 mg / mL, more preferably 30-300 mg / mL. In one embodiment of the present invention, the polymer monomer in the polymer monomer solution is acrylic acid and acrylamide; the polymer monomer solution includes acrylic acid, acrylamide, N,N'-methylenebisacrylamide and water, wherein the concentration of acrylic acid is 30 mg / mL, and the concentration of acrylamide is 300 mg / mL. In another embodiment of the present invention, the polymer monomer in the polymer monomer solution is acrylic acid and hydroxyethyl methacrylate; the polymer monomer solution includes acrylic acid, hydroxyethyl methacrylate, N,N'-methylenebisacrylamide and water, wherein the concentration of acrylic acid is 30 mg / mL, and the concentration of hydroxyethyl methacrylate is 300 mg / mL. In another embodiment of the present invention, the polymer monomers in the polymer monomer solution are acrylic acid and N-isopropylacrylamide; the polymer monomer solution includes acrylic acid, N-isopropylacrylamide, N,N'-methylenebisacrylamide and water, wherein the concentration of acrylic acid is 30 mg / mL, and the concentration of N-isopropylacrylamide is 300 mg / mL. In another embodiment of the present invention, the polymer monomers in the polymer monomer solution are acrylic acid and sulfobetaine methacrylate; the polymer monomer solution includes acrylic acid, sulfobetaine methacrylate, N,N'-methylenebisacrylamide and water, wherein the concentration of acrylic acid is 30 mg / mL, and the concentration of sulfobetaine methacrylate is 300 mg / mL.
[0037] In the present invention, the wavelength of the visible light is preferably 460 to 465 nm, more preferably 460 to 462 nm. The second free radical polymerization reaction of the present invention is preferably carried out under a nitrogen atmosphere; the temperature is preferably 20 to 35° C., more preferably 25° C.; the time is preferably no more than 90 min, more preferably 20 to 90 min, more preferably 60 min.
[0038] The present invention also provides a carbon nitride-induced interfacial hydrogel coating obtained by the preparation method described in the above technical solution.
[0039] The present invention also provides the use of the carbon nitride-induced interfacial hydrogel coating described in the above technical solution in marine antifouling or biomedical devices. The present invention can polymerize the interfacial hydrogel coating on marine equipment, and can play an antifouling role without compounding with other reagents. At the same time, the interfacial hydrogel coating of the present invention can be applied to the surface of medical catheters, artificial joints, scalpels and other medical devices without the introduction of metal ions (Fe3+ ), good biocompatibility.
[0040] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Example 1
[0042] (1) Preparation of carbon nitride powder: Weigh 50 g of urea and put it into a crucible. Cover the crucible and put it into a muffle furnace. Heat it from room temperature to 550°C at a rate of 10°C / min and calcine it at 550°C for 4 h. Then, cool the obtained material naturally to room temperature and grind it to obtain carbon nitride powder (particle size is 100-200 nm).
[0043] (2) Preparation of dopamine adhesion polymer (reference: Zhang Y, Xu R, Zhao W, et al. Successive redox-reaction-triggered interface radical polymerization for growing hydrogel coatings on diverse substrates. Angewandte Chemie, 2022, 134 (39): e202209741.): 10 g dopamine hydrochloride and 7.2 g triethylamine were dissolved in 100 mL methanol and placed in an ice bath in a N2 atmosphere for 20 min. Then, methacryloyl chloride solution (containing 6 mL methacryloyl chloride and 4 mL dichloromethane) was uniformly added dropwise thereto. The dropping rate was controlled so that the dropping time of the methacryloyl chloride solution was 1 h. The timing was started from the completion of the dropping of the methacryloyl chloride solution. The resulting mixed solution was subjected to amidation reaction for 2 h in an ice bath to obtain a reaction solution (brown yellow). The reaction liquid was subjected to rotary evaporation, and the obtained material was dissolved with 200 mL of ethyl acetate, extracted three times with 1 mol / L hydrochloric acid and saturated brine, and the organic phase was retained and dried with anhydrous MgSO4, filtered, and the filtrate was subjected to rotary evaporation to remove ethyl acetate. The residue was recrystallized with a mixed solvent of ethyl acetate and n-hexane (the volume ratio of ethyl acetate and n-hexane in the mixed solvent was 1:2) to obtain dopamine methacrylamide (DMA). Then 1.7 g DMA, 7.5 g methoxyethyl acrylate and 106 mg azobisisobutyronitrile were added to a reaction tube containing 18 mL N,N-dimethylformamide, and the polymerization reaction was carried out at 65°C in a N2 atmosphere for 12 hours. The obtained mixture was precipitated with petroleum ether and dissolved with ethyl acetate in turn, and the precipitation and dissolution operation was cycled 3 times. The solution obtained from the last dissolution operation was precipitated with petroleum ether, and the obtained precipitate was vacuum dried to obtain a dopamine adhesion polymer.
[0044] (3) Preparation of dopamine adhesion bonding layer containing carbon nitride: The dopamine adhesion polymer is dissolved in dichloromethane to obtain a solution. Carbon nitride powder is then added to the solution and ultrasonically dispersed for 30 minutes (the concentration of the carbon nitride powder is 0.2 wt%). The resulting mixture is coated on the surface of a glass substrate with a coating thickness of 5 μm. The coated glass sheet is dried in a vacuum drying oven for 24 hours to obtain a dopamine adhesion bonding layer containing carbon nitride on the surface of the glass substrate, i.e., a carbon nitride modified substrate is obtained.
[0045] (4) Construction of interfacial hydrogel coating: acrylamide, acrylic acid, N,N'-methylenebisacrylamide and 10 mL of water were mixed to obtain a polymer monomer solution (the concentration of acrylamide in the polymer monomer solution was 300 mg / mL, the concentration of acrylic acid was 30 mg / mL, and the concentration of N,N'-methylenebisacrylamide was 0.3 mg / mL). The polymer monomer solution was poured into a reaction tank, and the carbon nitride modified substrate was immersed in the polymer monomer solution. The polymerization reaction was carried out under N2 atmosphere, 460 nm LED light irradiation, and 25°C for 20 min, 30 min, 60 min, and 90 min, respectively, to form an interfacial hydrogel coating in situ on the surface of the dopamine adhesion bonding layer.
[0046] Example 2
[0047] The substrate was adjusted to a ceramic substrate, and the other conditions were the same as in Example 1 to prepare an interfacial hydrogel coating.
[0048] Example 3
[0049] The substrate was adjusted to a polypropylene (PP) substrate, and the other conditions were the same as those in Example 1 to prepare an interfacial hydrogel coating.
[0050] Example 4
[0051] The substrate was adjusted to an iron sheet (Fe) substrate, and the other conditions were the same as in Example 1 to prepare an interfacial hydrogel coating.
[0052] Example 5
[0053] The substrate was adjusted to a polydimethylsiloxane (PDMS) substrate, and the other conditions were the same as those in Example 1 to prepare an interfacial hydrogel coating.
[0054] Example 6
[0055] The substrate was adjusted to a polypropylene (PP) substrate, the polymer monomers were adjusted to hydroxyethyl methacrylate and acrylic acid, and the other conditions were the same as in Example 1 (the concentration of hydroxyethyl methacrylate in the polymer monomer solution was 300 mg / mL, the concentration of acrylic acid was 30 mg / mL, and the concentration of N,N'-methylenebisacrylamide was 0.3 mg / mL), and an interfacial hydrogel coating was prepared.
[0056] Example 7
[0057] The substrate was adjusted to a polypropylene (PP) substrate, the polymer monomers were adjusted to N-isopropylacrylamide and acrylic acid, and the other conditions were the same as in Example 1 (the concentration of N-isopropylacrylamide in the polymer monomer solution was 300 mg / mL, the concentration of acrylic acid was 30 mg / mL, and the concentration of N,N'-methylenebisacrylamide was 0.3 mg / mL), to prepare an interfacial hydrogel coating.
[0058] Example 8
[0059] The substrate was adjusted to a polypropylene (PP) substrate, the polymer monomers were adjusted to betaine sulfonate methacrylate and acrylic acid, and the other conditions were the same as in Example 1 (the concentration of betaine sulfonate methacrylate in the polymer monomer solution was 300 mg / mL, the concentration of acrylic acid was 30 mg / mL, and the concentration of N,N'-methylenebisacrylamide was 1.5 mg / mL), and an interfacial hydrogel coating was prepared.
[0060] Test Example 1
[0061] The growth process of the interfacial hydrogel coating over time in Example 1 is as follows Figure 1 As shown. Figure 1 It can be seen that with the extension of reaction time, the thickness of the interfacial hydrogel coating gradually increases, and the surface of the interfacial hydrogel coating grows more and more uniformly and smoothly.
[0062] The data of the thickness of the interfacial hydrogel coating changing with time in Examples 1 to 5 are as follows: Figure 2 As shown. Figure 2 It can be seen that by controlling the time for the polymer monomer to generate free radical polymerization (surface grafting growth), the thickness of the resulting interfacial hydrogel coating can be regulated between tens and hundreds of microns. And at the beginning of the reaction, the number of free radicals generated by carbon nitride on the interface under light is limited, resulting in a very slow polymerization reaction, and the interfacial hydrogel coating generated on the surface is very thin or almost non-existent. As the reaction time increases, the number of free radicals generated by carbon nitride increases, and the interfacial polymerization reaction occurs rapidly, but the rapidly growing interfacial hydrogel coating will inhibit the transfer and diffusion of free radicals, resulting in a slower growth rate of the entire interface. As the thickness of the interfacial hydrogel coating further increases, the diffusion barrier increases, and the growth rate gradually slows down.
[0063] In addition, Examples 1 to 8 show that the interfacial hydrogel coating can be successfully constructed on different substrates (glass, ceramic, metal iron, polypropylene, polydimethylsiloxane) by the method of the present invention, which proves the universality of the method of the present invention.
[0064] Test Example 2 Tribological Performance Test:
[0065] The friction properties of the samples obtained in Examples 1 to 8 of the present invention were characterized on a conventional ball-disc reciprocating friction machine (CSM). The test method is as follows: fix the sample on the sample table and collect the coefficient of friction (COF). The friction pair uses a steel ball with a diameter of 6 mm, a sliding distance of 4 mm, a frequency of 1 Hz, a load of 0.25 N, and deionized water as a lubricant. A micro-syringe is used to add water at the interface that can only wet the surface of the sample to keep the hydrogel hydrated during the test and prevent the interface from dehydrating and drying. The test results of the interfacial hydrogel coating obtained in Example 1 are shown in Figure 2. Figure 3 As shown ( Figure 3 The Blank in the figure is a dopamine adhesion bonding layer containing carbon nitride).
[0066] Depend on Figure 3 It can be seen that the friction coefficient of the dopamine adhesion layer containing carbon nitride is very high, and the friction coefficient is significantly reduced after the growth of the hydrogel coating, with an average friction coefficient between 0.04 and 0.06, indicating that the hydration lubrication of the surface interface hydrogel coating reduces the interface friction. Therefore, the substrate modified with the interface hydrogel coating has good lubrication ability.
[0067] Table 1 shows the average surface friction coefficient of the interfacial hydrogel coating in Examples 1 to 8 when grown for 60 minutes.
[0068] Table 1 Average surface friction coefficient of the interfacial hydrogel coating when grown for 60 min in Examples 1 to 8
[0069]
[0070] It can be seen from Table 1 that without changing the properties of the substrate itself, the growth of the interfacial hydrogel gives the substrate surface lubrication properties, and the average friction coefficient is below 0.05. Compared with the adhesive bonding layer, after the interfacial hydrogels of different polymer monomers are grown, the average friction coefficients of different substrates are reduced.
[0071] Test Example 3 Antifouling performance test:
[0072] The antifouling performance of the interfacial hydrogel coating obtained in Example 1 was investigated by using dichaete (the test method refers to the following documents: Zhang J, Wang X, Zhang C, et al. Self-lubricating interpenetrating polymer networks with functionalized nanoparticles enhancement for quasi-static and dynamic antifouling [J]. Chemical Engineering Journal, 2022, 429: 132300). Some test results are shown in Figure 4 .
[0073] Depend on Figure 4 It can be seen that a large number of algae are attached to the glass substrate, and after the acrylic acid / acrylamide hydrogel coating is grown, almost no algae attachment appears on the surface. The results show that the interfacial hydrogel coating prepared by the present invention has excellent anti-algae adhesion performance and can be used for marine antifouling.
[0074] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a carbon nitride-induced interfacial hydrogel coating, characterized in that: The following steps are involved: The carbon nitride and the dopamine adhesion polymer are mixed and coated on the surface of the substrate to form a dopamine adhesion bonding layer containing an initiator on the surface of the substrate to obtain an initiator-modified substrate; the dopamine adhesion polymer is prepared by a first free radical polymerization reaction of dopamine methacrylamide and methoxyethyl acrylate; The initiator-modified substrate is immersed in a polymer monomer solution, and a second free radical polymerization reaction is carried out under visible light irradiation to form an interfacial hydrogel coating initiated by carbon nitride on the surface of the substrate.
2. The preparation method according to claim 1, characterized in that: The mass of the carbon nitride is 0.025-0.5% of the total mass of the carbon nitride and the dopamine adhesion polymer.
3. The preparation method according to claim 1, characterized in that: The substrate includes a metal substrate, a glass substrate, a ceramic substrate, a plastic substrate or a silicone rubber substrate.
4. The preparation method according to claim 1, characterized in that: The temperature of the first free radical polymerization reaction is 60-65° C. and the time is 12-15 hours.
5. The preparation method according to claim 1, characterized in that: The polymer monomer in the polymer monomer solution includes at least one of acrylic acid, acrylamide, hydroxyethyl methacrylate, N-isopropylacrylamide and sulfobetaine methacrylate.
6. The preparation method according to claim 1 or 5, characterized in that: The concentration of the polymer monomer in the polymer monomer solution is 20 to 500 mg / mL.
7. The preparation method according to claim 1, characterized in that: The wavelength of the visible light is 460-465 nm.
8. The preparation method according to claim 1, characterized in that: The second free radical polymerization reaction is carried out under a nitrogen atmosphere, the temperature of the second free radical polymerization reaction is 20-35° C., and the time does not exceed 90 minutes.
9. The carbon nitride-induced interfacial hydrogel coating obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the carbon nitride-induced interfacial hydrogel coating according to claim 9 in marine antifouling or biomedical devices.
Citation Information
Patent Citations
Modification method for functionalizing surface of material
CN103435830A
Carbon nitride composite hydrogel as well as preparation method and application thereof
CN112646069A
Method for modifying hydrogel lubricating coating on surface of general device and general device modified with hydrogel lubricating coating
CN114031714A
Method for modifying hydrogel lubricating coating on surface of general device and general device modified with hydrogel lubricating coating
CN114163925A
Thermal initiator as well as synthesis method and application thereof
CN116836087A
Cited By
Inorganic hybrid ultraviolet barrier coating and preparation method thereof
CN121495420A
An inorganic hybrid ultraviolet blocking coating and its preparation method
CN121495420B
Protein-initiated self-growing transparent hydrogel antifouling coating and preparation method thereof
CN121673954A