Preparation method of super-hydrophobic coating

By using ammonia, deionized water, ethanol and other materials to prepare a combined coating of silica sol and silicon carbide particles on a superhydrophobic surface, the problems of complex preparation processes and poor stability in the existing technology are solved, and an efficient and low-cost coating is achieved. Preparation of superhydrophobic coatings with excellent antifouling and corrosion resistance properties.

CN118725690APending Publication Date: 2024-10-01JIANGSU UNIV OF TECH

Patent Information

Application Number
CN202410912848.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The preparation process of existing superhydrophobic surfaces is cumbersome, costly, and has poor stability. It is easily damaged by external impact and harsh environments, resulting in weakening or loss of hydrophobic properties, making it difficult to use outdoors for a long time.

Method used

Ammonia, deionized water, ethanol, and tetraethyl silicate are used to prepare silica sol, and silicon carbide particles of different particle sizes are mixed with octadecyltrimethoxysilane, epoxy resin, and polyetheramine curing agent, and cured at room temperature. Form a superhydrophobic coating.

Benefits of technology

The prepared superhydrophobic coating has excellent antifouling, self-cleaning, mechanical stability, physical/chemical stability and corrosion resistance, can be mass-produced on a variety of substrates, and is suitable for construction, transportation and other fields, and Performs well under friction, grit impact, corrosion and extreme temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725690A_ABST
    Figure CN118725690A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a super-hydrophobic coating. Comprising the following steps: preparing silica sol from ammonia water, deionized water, ethanol and tetraethyl silicate; adding silicon carbide particles with different particle sizes into ethyl acetate to obtain a mixed solution A; adding octadecyl trimethoxy silane, epoxy resin and a polyether amine curing agent into the mixed solution A to obtain a mixed solution B; adding silica sol into the mixed solution B to obtain a mixed solution C, coating the surface of a matrix with the mixed solution C, and curing at room temperature to obtain the super-hydrophobic coating. The coating can be prepared on various substrates made of different materials, and shows excellent antifouling and self-cleaning properties; good mechanical stability, adhesive force, physical / chemical stability, corrosion resistance, anti-icing performance, deicing performance and the like are shown; the preparation method is simple and low in cost, can be used for large-scale preparation, and is expected to be widely applied to the fields of buildings, transportation, chemical engineering and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a hydrophobic coating, and in particular to a method for preparing a bionic super-hydrophobic coating. Background Art

[0002] The biomimetic super-hydrophobic surface is characterized by a contact angle greater than 150° and a rolling angle less than 10°. Its special wettability makes it show significant advantages in interface problems. Therefore, a large number of super-hydrophobic surfaces have been designed and widely used in various fields, including self-cleaning, anti-fouling, anti-biological adhesion, anti-icing and oil-water separation. Its unique super-hydrophobicity also plays an important role in reducing the corrosion of solid surfaces in the ocean, soil and other environments. Although super-hydrophobic surfaces have great application potential, they are still subject to great limitations in actual preparation and application. There are many methods for preparing super-hydrophobic surfaces at present, such as etching, template method, sol-gel method, chemical vapor deposition method, hydrothermal method and electrochemical deposition method, but most of the super-hydrophobic surfaces prepared by these methods have complicated preparation processes, long preparation cycles, high costs, and are difficult to prepare on a large scale; In addition, the stability of the prepared partial super-hydrophobic surfaces is poor, and in practical applications, it is likely to be subjected to some inevitable external force impacts, such as finger pressing, surface friction, gravel impact and rain impact, etc., and its fragile micro / nano structure is easy to collapse, break or disappear, which not only leads to a decrease in local roughness, but also leads to the disappearance of the bottom surface energy material; Finally, when some super-hydrophobic surfaces are in some harsh environments, such as ultraviolet radiation, acid rain corrosion, high / low temperature working environment and extremely cold weather, the low surface energy materials on its surface may be decomposed or consumed step by step, and hydrophilic polar groups are produced, thereby causing the super-hydrophobic performance to weaken or even completely lose. Therefore, when preparing and actually using the super-hydrophobic surface, the stability and versatility of the surface must be taken into account to extend its service life and scope of application.

[0003] Linjing Cui et al. prepared a super-hydrophobic concrete surface with excellent corrosion resistance and self-cleaning properties by mixing silica, methyltrimethoxysilane, cement and sand. It can effectively reduce the direct contact between pollutants and the concrete surface and enhance the surface's resistance to dust and dirt. However, its weak stability makes it difficult to use outdoors for a long time (L. Cui, T. Xiang, B. Hu, et al. Colloids and Surfaces A: Physicochemical and Engineering Aspects, 2023, 685: 133345).

[0004] Chinese patent CN117384533A discloses a method for preparing a super-hydrophobic composite coating based on SiC of different particle sizes. The method uses SiC particles of different particle sizes to construct a super-hydrophobic structure. However, the preparation of the hydrophobic structure depends on the spray solution system. When a component in the spray solution system is changed, for example, when the fluorinated silane or butyl acetate in the system is replaced by other analogs, the hydrophobic film structure cannot be formed normally, thereby affecting the hydrophobic performance. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a super-hydrophobic coating, so as to solve the problem of how to prepare a coating with super-hydrophobic properties.

[0006] Technical solution: A method for preparing a super-hydrophobic coating according to the present invention comprises the following steps:

[0007] (1) preparing silica sol using ammonia water, deionized water, ethanol and tetraethyl silicate;

[0008] (2) adding silicon carbide particles of different particle sizes into ethyl acetate to obtain a mixed solution A;

[0009] (3) adding octadecyltrimethoxysilane, epoxy resin and polyetheramine curing agent to the mixed solution A to obtain a mixed solution B;

[0010] (4) Adding silica sol to mixed solution B to obtain mixed solution C, coating the mixed solution C on the surface of the substrate, and curing at room temperature to obtain a super hydrophobic coating.

[0011] Preferably, in step (1), the silica sol is prepared by adding ammonia water and deionized water to anhydrous ethanol, stirring continuously for 15-45 minutes at 40-60° C., and then adding tetraethyl silicate and stirring continuously for 1-3 hours to obtain the silica sol.

[0012] Preferably, the volume ratio of the ammonia water, deionized water, anhydrous ethanol and tetraethyl silicate is 4-8:7-13:90-110:4-8.

[0013] Preferably, in step (2), the silicon carbide particles of different particle sizes are composed of micron silicon carbide particles with a particle size of 1-500 μm and nano silicon carbide particles with a particle size of 50-500 nm, and the weight ratio of the micron silicon carbide particles to the nano silicon carbide particles is 1-2:1-2.

[0014] Preferably, in step (2), the mass ratio of the silicon carbide particles of different particle sizes to ethyl acetate is 1-4:10-20.

[0015] Preferably, in step (3), the weight ratio of octadecyltrimethoxysilane, epoxy resin and polyetheramine curing agent is 0.1-0.3:1.5-3.0:0.5-0.9.

[0016] Preferably, in step (3), the epoxy resin is E-51, and the polyetheramine curing agent is D-230.

[0017] Preferably, in step (4), the mass ratio of the silica sol to the mixed solution B is 0.3-0.7:13-28.

[0018] Preferably, in step (4), the mixed solution C is coated on the substrate surface and cured at room temperature by spraying the mixed solution C onto the substrate surface with a spray gun at a position 25-35 cm perpendicular to the substrate surface at an air pressure of 0.4-0.6 MPa for 15-25 seconds, and curing at room temperature for 12-48 hours.

[0019] Preferably, in step (4), the material of the substrate is at least one of metal, wood, and paper. The substrate can be an aluminum sheet, a copper sheet, an iron sheet, or an alloy sheet, as well as a cardboard, white paper, or a wooden board.

[0020] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0021] (1) The super-hydrophobic coating can be prepared on substrates of various materials and exhibits excellent anti-fouling and self-cleaning properties;

[0022] (2) The superhydrophobic coating exhibits good mechanical stability, adhesion, physical / chemical stability, corrosion resistance, anti-icing, deicing and other properties;

[0023] (3) The preparation method of this superhydrophobic coating is simple, low-cost, and can be prepared on a large scale. It is expected to be widely used in the fields of construction, transportation, and chemical industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Characterization diagram of surface wettability and surface structure of super-hydrophobic coatings prepared at different μ-SiC / n-SiC ratios;

[0025] Figure 2 The morphology of different liquid pollutants on super-hydrophobic coatings prepared on different substrates;

[0026] Figure 3 The self-cleaning test results of the super-hydrophobic coating and the untreated aluminum sheet after being contaminated by sand and gravel;

[0027] Figure 4 The wettability change test results of the super-hydrophobic coating after different times of friction;

[0028] Figure 5 The SEM images of the super-hydrophobic coating at different magnifications after 300 frictions;

[0029] Figure 6 The test results of wettability change of super hydrophobic coating after different times of sand impact;

[0030] Figure 7 The SEM images of the super-hydrophobic coating at different magnifications after 25 times of sand impact;

[0031] Figure 8 The results of the adhesion test of the super hydrophobic coating and the morphology of water droplets on the coating surface after the adhesion test;

[0032] Fig. 9 The wettability change curve of the super-hydrophobic coating after different tape peeling times;

[0033] Fig.10 The wettability change test results of super hydrophobic coating under different corrosive conditions;

[0034] Fig.11 is the TG curve of super-hydrophobic coating;

[0035] Fig.12 The wettability change test results of the super-hydrophobic coating after being kept at different temperatures for 2 hours;

[0036] Fig.13 Tafel curves of super-hydrophobic coating and untreated aluminum sheet;

[0037] Fig.14 The freezing images and time of water droplets on the untreated aluminum sheet surface and the super-hydrophobic coating surface at -10°C;

[0038] Fig.15 The curves of the surface temperature of the untreated aluminum sheet and the super-hydrophobic coating changing with the irradiation time;

[0039] Fig.16 is the melting time of the ice layer on the surface of untreated aluminum sheet and super-hydrophobic coating under xenon lamp irradiation. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0041] Example 1: A method for preparing a super hydrophobic coating is as follows:

[0042] (1) 6 mL of ammonia water and 10 mL of deionized water were added to 100 mL of anhydrous ethanol, and the mixture was stirred at 400 r / min for 30 min at 50° C., and then 6 mL of tetraethyl silicate was added and stirred at 400 r / min for 2 h to obtain a silica sol;

[0043] (2) Add silicon carbide particles of different particle sizes to 15 g of ethyl acetate, stir at 400 r / min for 2 h at room temperature to obtain a mixed solution A, and then ultrasonically oscillate for 30 min to prevent the particles from agglomerating. The silicon carbide particles of different particle sizes are composed of micron silicon carbide (μ-SiC) particles and nano silicon carbide (n-SiC) particles. The ratio and particle size of the silicon carbide particles of different particle sizes are shown in Table 1.

[0044] (3) 0.2 g of octadecyltrimethoxysilane, 2.1 g of epoxy resin E-51 and 0.7 g of polyetheramine curing agent D-230 were added to the mixed solution A, and the mixture was stirred at a speed of 400 r / min for 2 h to obtain a mixed solution B.

[0045] (4) 0.5 g of silica sol was added to 20 g of mixed solution B, and the mixture was stirred at a speed of 400 r / min for 1 h to obtain mixed solution C. The mixed solution C was sprayed onto the surface of the aluminum sheet at a pressure of 0.5 MPa for 20 s at a position 30 cm from the surface of the aluminum sheet using a spray gun with a nozzle of 3 mm, and cured at room temperature for 24 h to obtain a super-hydrophobic coating. The surface wettability and surface structure of the super-hydrophobic coating were as shown in FIG. Figure 1 shown. Figure 1 Figures (a), (b), (c), (d), and (e) are optical photographs and contact angles of the coating; Figures (f), (g), (h), (i), and (j) are SEM images of the coating at different magnifications.

[0046] Table 1 Ratio and particle size of silicon carbide particles with different particle sizes

[0047]

[0048] Depend on Figure 1 The results show that when the weight of μ-SiC and n-SiC is 1g, there are a large number of protrusions, pits and holes on the coating surface. The holes can capture air to form a stable air layer, thereby forming a better hydrophobic layer structure. The appropriate ratio of μ-SiC and n-SiC provides a micro / nano rough structure for the coating. The hierarchical rough structure of the coating surface can meet the Cassie-Baxter state, which is a key factor in achieving superhydrophobicity of the coating, ensuring a low contact area and penetration depth of the droplets on the coating.

[0049] Example 2: A method for preparing a super hydrophobic coating is as follows:

[0050] (1) 4 mL of ammonia water and 7 mL of deionized water were added to 90 mL of anhydrous ethanol, and the mixture was stirred at 400 r / min for 15 min at 60° C., and then 4 mL of tetraethyl silicate was added and stirred at 400 r / min for 1 h to obtain silica sol;

[0051] (2) 1 g of micron silicon carbide (μ-SiC) particles and 1 g of nano silicon carbide (n-SiC) particles were added to 10 g of ethyl acetate, stirred at 400 r / min for 2 h at room temperature to obtain a mixed solution A, and then ultrasonically oscillated for 30 min to prevent the particles from agglomerating.

[0052] (3) 0.1 g of octadecyltrimethoxysilane, 1.5 g of epoxy resin E-51 and 0.5 g of polyetheramine curing agent D-230 were added to the mixed solution A, and the mixture was stirred at a speed of 400 r / min for 2 h to obtain a mixed solution B.

[0053] (4) 0.3 g of silica sol was added to 13 g of mixed solution B, and the mixture was stirred at 400 r / min for 1 h to obtain mixed solution C. The mixed solution C was sprayed onto the surface of the aluminum sheet at a pressure of 0.4 MPa for 15 s at a distance of 25 cm from the surface of the aluminum sheet using a spray gun with a nozzle of 3 mm, and cured at room temperature for 12 h to obtain a super hydrophobic coating.

[0054] Example 3: A method for preparing a super hydrophobic coating is as follows:

[0055] (1) 8 mL of ammonia water and 13 mL of deionized water were added to 110 mL of anhydrous ethanol, and the mixture was stirred at 400 r / min for 45 min at 40° C., and then 8 mL of tetraethyl silicate was added and stirred at 400 r / min for 3 h to obtain a silica sol;

[0056] (2) 1 g of micron silicon carbide (μ-SiC) particles and 1 g of nano silicon carbide (n-SiC) particles were added to 20 g of ethyl acetate, stirred at 400 r / min for 2 h at room temperature to obtain a mixed solution A, and then ultrasonically oscillated for 30 min to prevent the particles from agglomerating.

[0057] (3) 0.3 g of octadecyltrimethoxysilane, 3.0 g of epoxy resin E-51 and 0.9 g of polyetheramine curing agent D-230 were added to the mixed solution A, and the mixture was stirred at a speed of 400 r / min for 2 h to obtain a mixed solution B.

[0058] (4) 0.7 g of silica sol was added to 28 g of mixed solution B, and the mixture was stirred at 400 r / min for 1 h to obtain mixed solution C. The mixed solution C was sprayed onto the surface of the aluminum sheet at a pressure of 0.6 MPa for 25 s at a position 35 cm from the surface of the aluminum sheet using a spray gun with a nozzle of 3 mm, and cured at room temperature for 48 h to obtain a super hydrophobic coating.

[0059] Embodiment 4: A method for preparing a super hydrophobic coating is as follows:

[0060] (1) 6 mL of ammonia water and 10 mL of deionized water were added to 100 mL of anhydrous ethanol, and the mixture was stirred at 400 r / min for 30 min at 50° C., and then 6 mL of tetraethyl silicate was added and stirred at 400 r / min for 2 h to obtain a silica sol;

[0061] (2) 1 g of micron silicon carbide (μ-SiC) particles and 1 g of nano silicon carbide (n-SiC) particles were added to 15 g of different organic solvents (see Table 2), stirred at 400 r / min for 2 h at room temperature to obtain a mixed solution A, and then ultrasonically oscillated for 30 min to prevent the particles from agglomerating.

[0062] (3) 0.2 g of octadecyltrimethoxysilane, 2.1 g of epoxy resin E-51 and 0.7 g of polyetheramine curing agent D-230 were added to the mixed solution A, and the mixture was stirred at a speed of 400 r / min for 2 h to obtain a mixed solution B.

[0063] (4) 0.5 g of silica sol was added to 20 g of mixed solution B, and the mixture was stirred at 400 r / min for 1 h to obtain mixed solution C. The mixed solution C was sprayed onto the surface of the aluminum sheet at a pressure of 0.5 MPa for 20 s at a position 30 cm from the surface of the aluminum sheet using a spray gun with a nozzle of 3 mm, and cured at room temperature for 24 h to obtain a super hydrophobic coating.

[0064] Table 2 Effect of different organic solvents on the hydrophobic properties of coatings

[0065] Types of organic solvents Contact angle (°) Roll angle (°) Ethanol 88.1 Unable to measure Ethyl acetate 159.3 3.6 Butyl acetate 131.1 35.9

[0066] It can be seen from the results in Table 2 that neither ethanol nor butyl acetate can form a hydrophobic coating that meets the requirements. Only when the organic solvent is ethyl acetate, the prepared coating has the required biomimetic hydrophobic properties, that is, the contact angle is greater than 150° and the rolling angle is less than 10°. Therefore, in step (2), it is determined that silicon carbide particles of different particle sizes are suspended in ethyl acetate.

[0067] Embodiment 5: All other aspects are the same as Embodiment 4, except that:

[0068] The aluminum sheet was replaced with cardboard, white paper and wood board to prepare the coating. Different liquid pollutants (coffee, white vinegar, juice, methylene blue solution and sewage) were dropped on the coating on the surface of different substrates to observe the droplet morphology. Figure 2 shown. Figure 2 The morphology of different liquid pollutants (coffee, white vinegar, juice, methylene blue solution and sewage) on super-hydrophobic coatings prepared on different substrates (aluminum sheet, cardboard, white paper and wood board) is shown. These droplets are spherical on the super-hydrophobic coatings on different substrates.

[0069] At the same time, the self-cleaning performance of the super-hydrophobic coating on the aluminum sheet was compared and tested. The results are as follows Figure 3 As shown in the figure, the upper figure is an aluminum sheet coated with a super-hydrophobic coating, and the lower figure is an untreated aluminum sheet. It can be seen that the sand on the super-hydrophobic coating can slide off with the water droplets, but a large amount of sand still remains on the untreated aluminum sheet.

[0070] The super hydrophobic coating prepared in Example 4 was subjected to a wear resistance test. In the experiment, the coating was placed face down on 1000 mesh SiC sandpaper, a 100 g weight was loaded on the sample, and it was pushed horizontally for 10 cm at a speed of 5 cm / s, which was defined as one friction. The results are shown in FIG. Figure 4 and Figure 5 As shown, Figure 4 The wettability curve of the super-hydrophobic coating after different friction times shows that after 250 frictions, the coating still exhibits super-hydrophobicity, with a contact angle of 150.2° and a rolling angle of 17.1°. Figure 5 It shows that after 300 frictions, the protrusions on the superhydrophobic surface are almost worn away, leaving only a small number of protrusions and pits, and the fluorine-containing substances on the surface are also greatly reduced, causing the coating to lose its superhydrophobicity.

[0071] The super hydrophobic coating prepared in Example 4 was subjected to a gravel impact test, where 150 g of gravel with a particle size of 150 μm was dropped at a certain speed from a height of 40 cm from the coating (the coating was tilted at 45°) to impact the surface of the super hydrophobic coating. Figure 6 and Figure 7 As shown, Figure 6 It was shown that after 20 times of sand impact, the coating still remained superhydrophobic. Figure 7 It shows that the continuous impact of sand and gravel makes it difficult for the hierarchical rough structure of the superhydrophobic surface to continue to maintain its integrity. Most of the protrusions and low surface energy materials are destroyed by the impact, weakening the surface roughness. In addition, the sand and gravel may also fill into the grooves on the coating surface, making it difficult for the coating to capture air to form an air layer, increasing the solid-liquid contact area, and making it difficult for the coating to continue to maintain its superhydrophobicity.

[0072] The super-hydrophobic coating prepared in Example 4 was subjected to a single standard cross-cut tape test, and the results were as follows: Figure 8As shown, Figure 8 (a) shows the coating after being scratched by a grid knife; (b) shows a schematic diagram of 3M tape adhering to the coating; (c) shows a sample of the coating and tape after a standard cross-cut tape test; (d) shows a wettability test of the coating after a standard cross-cut tape test. Figure 8 It can be seen that the area of ​​the super-hydrophobic coating that has been peeled off is significantly less than 5%, and it still has excellent super-hydrophobicity, and the coating exhibits good adhesion.

[0073] Attach 3M tape to the coating surface, place a 100g weight on the surface and roll it back and forth, then quickly remove the tape and repeat the above process. Fig. 9 As shown, from Fig. 9 It can be observed that the coating still maintains superhydrophobicity after 30 tape peelings.

[0074] The super hydrophobic coating prepared in Example 4 was subjected to a corrosion resistance test, and the results are as follows: Fig.10 As shown, Fig.10 In the figure, (a), (b), (c), and (d) are images of wettability changes of the super-hydrophobic coating immersed in acid (pH=1) / alkali (pH=14) / salt (3.5wt% NaCl) solution and under ultraviolet radiation. After the super-hydrophobic coating was immersed in an acid solution for 84 hours, an alkaline solution for 60 hours, and a salt solution for 72 hours, the coating still maintained super-hydrophobicity; and the coating still maintained super-hydrophobicity after being subjected to ultraviolet radiation for 144 hours. The main reason why the coating can obtain high chemical stability is that the air layer in the micro-nano pores can prevent the corrosive ions in the solution from corroding the coating. Over time, the solution will gradually invade the air layer, affecting the super-hydrophobic effect of the coating.

[0075] The super hydrophobic coating prepared in Example 4 was subjected to a thermal stability test, and the results were as follows: Fig.11 and Fig.12 shown. Fig.11 It shows that the superhydrophobic coating loses 45.89% of its mass between 220°C and 660°C, exhibiting good thermal stability. Fig.12 The wettability curve of the super-hydrophobic coating after being kept at different temperatures for 2 hours. The coating lost its super-hydrophobicity after being kept at 350℃ for 2 hours. But this is enough to show that the coating has good thermal stability.

[0076] The super-hydrophobic coating prepared in Example 4 and the untreated aluminum sheet were immersed in a 3.5 wt% NaCl solution for 30 min and then subjected to potentiodynamic polarization curve test. p ) is calculated by the formula The potentiodynamic polarization parameters of the superhydrophobic coating and the untreated aluminum sheet are shown in Table 3. Fig.13As shown in the figure, the super-hydrophobic coating exhibits good corrosion resistance. When the super-hydrophobic surface is immersed in a corrosive solution, the pore structure of the super-hydrophobic coating surface with a micro / nano graded rough structure can capture a large amount of air to form a dense air layer that can exist stably for a certain period of time, effectively avoiding the contact between the highly corrosive ions and the aluminum plate, thereby blocking the penetration of the highly corrosive ions.

[0077] Table 3 Effect of different organic solvents on the hydrophobic properties of coatings

[0078] sample <![CDATA[E corr (mV)]]> <![CDATA[I corr (A / cm 2 )]]> <![CDATA[η p (%)]]> Untreated aluminum sheet -821 <![CDATA[1.27×10 -8 ]]> - Super hydrophobic coating -496 <![CDATA[6.06×10 -11 ]]> 99.52%

[0079] Fig.14 The upper middle picture shows water droplets on the surface of an untreated aluminum sheet, and the lower picture shows an optical photograph and freezing time of water droplets on the surface of the super-hydrophobic coating prepared in Example 4 freezing at -10°C. The water droplets on the surface of the untreated aluminum sheet completely freeze at 102s, while the water droplets on the surface of the super-hydrophobic coating completely freeze at 242s, and the super-hydrophobic coating exhibits excellent anti-icing performance.

[0080] Fig.15 The temperature change curves of the super-hydrophobic coating prepared in Example 4 and the untreated aluminum sheet under xenon lamp irradiation in the same time period show that the surface temperature of the super-hydrophobic coating is higher.

[0081] Fig.16 The deicing performance test results of the super hydrophobic coating prepared in Example 4 and the untreated aluminum sheet. Fig.16 It can be seen that the ice layer on the super-hydrophobic surface can melt more quickly, and it only takes 475 seconds for the ice layer to melt completely. However, the ice layer on the untreated aluminum sheet surface takes 621 seconds to melt completely.

Claims

1. A method for preparing a super hydrophobic coating, characterized in that, The steps include: (1) preparing silica sol using ammonia water, deionized water, ethanol and tetraethyl silicate; (2) adding silicon carbide particles of different particle sizes into ethyl acetate to obtain a mixed solution A; (3) adding octadecyltrimethoxysilane, epoxy resin and polyetheramine curing agent to the mixed solution A to obtain a mixed solution B; (4) Adding silica sol to mixed solution B to obtain mixed solution C, coating the mixed solution C on the surface of the substrate, and curing at room temperature to obtain a super hydrophobic coating.

2. The method for preparing a super hydrophobic coating according to claim 1, wherein In step (1), the silica sol is prepared by adding ammonia water and deionized water to anhydrous ethanol, stirring continuously for 15-45 minutes at 40-60° C., and then adding tetraethyl silicate and stirring continuously for 1-3 hours to obtain the silica sol.

3. The preparation method of super hydrophobic coating according to claim 2, wherein The volume ratio of the ammonia water, deionized water, anhydrous ethanol and tetraethyl silicate is 4-8:7-13:90-110:4-8.

4. The method for preparing a super hydrophobic coating according to claim 1, wherein In step (2), the silicon carbide particles of different particle sizes are composed of micron silicon carbide particles with a particle size of 1-500 μm and nano silicon carbide particles with a particle size of 50-500 nm, and the weight ratio of the micron silicon carbide particles to the nano silicon carbide particles is 1-2:1-2.

5. The preparation method of super hydrophobic coating according to claim 1, characterized in that, In step (2), the mass ratio of the silicon carbide particles of different particle sizes to ethyl acetate is 1-4:10-20.

6. The method for preparing a super hydrophobic coating according to claim 1, wherein In step (3), the weight ratio of octadecyltrimethoxysilane, epoxy resin and polyetheramine curing agent is 0.1-0.3:1.5-3.0:0.5-0.

9.

7. The method for preparing a super hydrophobic coating according to claim 1, wherein In step (3), the epoxy resin is E-51, and the polyetheramine curing agent is D-230.

8. The method for preparing a super hydrophobic coating according to claim 1, wherein In step (4), the mass ratio of the silica sol to the mixed solution B is 0.3-0.7:13-28.

9. The method for preparing a super hydrophobic coating according to claim 1, wherein In step (4), the mixed solution C is coated on the substrate surface and cured at room temperature by spraying the mixed solution C onto the substrate surface at a pressure of 0.4-0.6 MPa for 15-25 seconds at a position 25-35 cm perpendicular to the substrate surface with a spray gun, and curing at room temperature for 12-48 hours.

10. The method for preparing a super hydrophobic coating according to claim 1, wherein: In step (4), the material of the substrate is at least one of metal, wood, and paper.

Citation Information

Patent Citations

  • Super-hydrophobic surface with moisture evacuating function and preparation method thereof

    CN104073031A

  • Super-hydrophobic coating with high adhesive force as well as preparation method and application thereof

    CN109306225A

  • Preparation method of super-hydrophobic composite coating based on SiC with different particle sizes

    CN117384533A

  • High-efficiency corrosion-resistant super-hydrophobic coating prepared by one-step spraying method

    CN117586683A

Cited By

  • Anti-bonding nanometer coating for cathode wire and preparation method of anti-bonding nanometer coating

    CN122278241A