Organic silicon heat-proof coating based on hollow nano-microspheres and preparation method of organic silicon heat-proof coating
By using nano hollow microspheres and modified silicone resin in the heat-proof coating, combined with other fillers and additives, the problem of existing coatings being difficult to balance high elongation, low density, and low thermal conductivity is solved, and a better The high performance balance and usage scenario expansion provide efficient external heat protection for the new generation of aircraft.
Patent Information
- Application Number
- CN202410848938.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing heat-resistant coatings to meet the performance requirements of high elongation, low density, and low thermal conductivity at the same time, resulting in limited usage scenarios for the coating.
Using silicone heat-proof coating based on nano-hollow microspheres, modified silicone resin and nano-hollow microspheres are used as the main fillers, combined into porcelain fillers, fluxes, flame retardants and other components to prepare low-density, low thermal conductivity , high toughness coating, achieving room temperature curing.
It significantly reduces the coating density and thermal conductivity, while increasing the elongation at break, meeting the technical requirements of lightweight, high toughness, and high heat protection for aircraft, and providing technical support for the external thermal protection of new generation aircraft.
Smart Images

Figure CN118725733A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermal protection of tactical weapons and equipment, and relates to a low-density, low-thermal-conductivity, high-toughness, ceramic-able organic silicon thermal-protective coating for a solid rocket engine. More specifically, the present invention relates to a low-density, low-thermal-conductivity, high-toughness, ceramic-able external thermal-protective coating based on nano hollow microspheres and a preparation method thereof. Background Art
[0002] Heat protection is a key technical issue that cannot be ignored in the aerospace field. With the rapid upgrading of weapons and equipment, aircraft are facing a service environment with higher heat flux density, longer action time, and stronger aerodynamic scour, which puts forward a lower density (density ≤ 0.60g / cm 3 ), higher toughness (elongation ≥ 20%), stronger thermal insulation (thermal conductivity ≤ 0.10W / (m·K)), and more erosion resistance (mass loss rate tends to 0) comprehensive performance requirements. At present, in the formulation design of thermal protective coatings, in order to achieve micro-ablation of the coating surface under high heat flow service environment without powdering and layer-by-layer erosion, silicone resin is generally used as the matrix material. Although the use of silicone resin can significantly improve the erosion resistance of the coating, due to its three-dimensional molecular structure and high rigidity, the elongation of the coating based on this is low, and in order to avoid further deterioration of the elongation, the amount of hollow filler added is significantly limited. Therefore, it is difficult to take into account the performance requirements of high elongation, low density and low thermal conductivity of the coating at the same time, resulting in limited coating usage scenarios. Summary of the invention
[0003] The purpose of the present invention is to overcome the above-mentioned defects and provide a silicone heat-resistant coating based on nano hollow microspheres and a preparation method thereof, which solves the technical problem that the existing heat-resistant coating is difficult to simultaneously meet the performance requirements of high elongation, low density and low thermal conductivity of the coating, resulting in limited use scenarios of the coating. The coating provided by the present invention has lower density, higher elongation and lower thermal conductivity, which meets the technical requirements of aircraft for lightweight, high toughness and high heat-resistant coatings, and provides technical support for the external heat protection of a new generation of aircraft.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention discloses a kind of organic silicon heat-proof coating based on nano hollow microspheres and its preparation method. The heat-proof coating of the present invention comprises: modified organic silicon resin, ceramic filler, flux, heat-insulating filler, dimensional filler, flame retardant, diluent, curing agent, catalyst. The heat-proof coating of the present invention adopts modified organic silicon resin as matrix and nano hollow microspheres as main filler. The preparation process is simple and the coating is cured and formed at room temperature. Compared with the existing organic silicon resin heat-proof coating, under the premise of maintaining the excellent anti-aerodynamic scour ability of the coating, by adding a large number of nano hollow microspheres, it has both heat insulation and toughening effects, greatly reducing the addition amount of other solid fillers, so that the coating has lower density, lower thermal conductivity and higher toughness, providing technical support for the external heat protection of the new generation of aircraft.
[0006] A nano hollow microsphere-based organic silicon heat-resistant coating comprises the following components in parts by mass:
[0007]
[0008] The modified organic silicone resin is a terminal hydroxyl methyl phenyl silicone resin including a three-dimensional structure molecular chain segment and a linear structure molecular chain segment.
[0009] Furthermore, the heat insulating filler is nano hollow glass microspheres, or a combination of nano hollow glass microspheres and one or more of expanded perlite, expanded vermiculite, micron-sized hollow microspheres or silica aerogel.
[0010] Furthermore, the average particle size of the nano hollow glass microspheres is 70nm to 90nm, the melting point is 550℃ to 650℃, and the bulk density is 0.30g / cm 3 ~0.43g / cm 3 .
[0011] Furthermore, the molecular structure of the hydroxy-terminated methylphenyl silicone resin is:
[0012]
[0013] Wherein, R1, R2, R3 and R4 are alkyl or phenyl groups, and m, p, q, and n are positive integers greater than 0;
[0014] The viscosity of the terminal hydroxymethylphenyl silicone resin is 2000-3500 cps.
[0015] Furthermore, the preparation method of the hydroxy-terminated methylphenyl silicone resin is as follows:
[0016] The polyalkoxysilane containing phenyl groups and the polyalkoxysilane are hydrolyzed and polycondensed to obtain a silsesquioxane having a three-dimensional structure;
[0017] The silsesquioxane is grafted and copolymerized with the linear polysiloxane to obtain the terminal hydroxyl methyl phenyl silicone resin.
[0018] Furthermore, the porcelain-forming filler is one or more of mica powder, talc powder, fumed silica, silica powder or kaolin;
[0019] The flame retardant is one or more of aluminum hydroxide, magnesium hydroxide, antimony trioxide or zinc borate.
[0020] Furthermore, the flux is one or more of glass powder, red lead or borax;
[0021] The dimensional filler is one or more of chopped quartz fiber, chopped glass fiber, high silica fiber or mullite fiber;
[0022] The curing agent is one or more of ethyl orthosilicate, propyl orthosilicate, vinyl trimethoxy silane or methyl trimethoxy silane;
[0023] The catalyst comprises a first catalyst and a second catalyst, the first catalyst is one or more of chelated tin, a zirconium catalyst or an aminosilane coupling agent, and the second catalyst is one or more of dibutyltin dilaurate, tetrabutyl titanate or stannous octoate;
[0024] The diluent is one or more of hexamethyldisiloxane and 120# gasoline.
[0025] Further, the flux is glass powder having a melting point in the range of 250°C to 350°C;
[0026] The length of the dimensional filler is 0.45 to 0.50 mm;
[0027] The catalyst is a composition of 3-(2-aminoethyl)-aminopropyltrimethoxysilane and dibutyltin dilaurate in a mass ratio of 1:1;
[0028] The diluent is hexamethyldisiloxane.
[0029] The above-mentioned method for preparing the organic silicon heat-resistant coating based on nano hollow microspheres comprises:
[0030] Premixing and grinding and dispersing the modified organic silicone resin, the ceramic filler, the flux, the flame retardant and a portion of the diluent to obtain a premixed liquid;
[0031] Add the heat-insulating filler, the dimensional filler and another part of the diluent into the premixed liquid to prepare component A;
[0032] The curing agent and the catalyst are mixed evenly to form component B;
[0033] After mixing component A and component B, spraying is performed to obtain an organic silicone heat-resistant coating.
[0034] Furthermore, after mixing component A and component B, the specific method of spraying to obtain the organic silicon heat-resistant coating is as follows:
[0035] preparing a dispersion of component A;
[0036] Add component B to the above dispersion to obtain a coating with a viscosity of 28 to 40 seconds;
[0037] The coating is sprayed and cured at room temperature to obtain an organic silicon heat-resistant coating; when the coating is sprayed, the spraying time is less than or equal to 3 hours; the room temperature curing time is more than 120 hours; the Shore A hardness of the organic silicon heat-resistant coating is ≥70.
[0038] Compared with the prior art, the present invention has at least one of the following beneficial effects:
[0039] (1) The present invention creatively proposes a silicone heat-resistant coating based on nano hollow microspheres, which is the first time that nano hollow microspheres are introduced into the thermal protection coating formula, effectively reducing the coating density and thermal conductivity, while greatly improving the coating elongation at break, and effectively balancing the key properties of the coating;
[0040] (2) The present invention provides a terminal hydroxymethylphenyl silicone resin having two molecular chain segment structures, namely, "bulk" and "linear", which significantly improves the coating's resistance to aerodynamic shear and achieves room temperature curing of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 is the average particle size distribution diagram of the hollow nanoparticles of the present invention;
[0042] Figure 2 The transmission electron microscope images of the hollow nanospheres of the present invention are shown in Figure 1; (a) is a 1000-fold electron microscope image, and (b) is a 50,000-fold electron microscope image. DETAILED DESCRIPTION
[0043] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.
[0044] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.
[0045] The present invention provides an organosilicon heat-resistant coating based on nano hollow microspheres and a preparation method thereof. The heat-resistant coating of the present invention adopts a modified organosilicon resin as a matrix and nano hollow microspheres as a main filler, has a simple preparation process, and is cured and formed at room temperature. Compared with the current organosilicon heat-resistant coating, the coating provided by the present invention has lower density, higher elongation, and lower thermal conductivity under the condition of comparable heat resistance, anti-scouring and interface bonding performance, and meets the technical requirements of aircraft for lightweight, high toughness, and high heat-resistant coatings.
[0046] The present invention discloses an organosilicon heat-resistant coating based on hollow nano-microspheres, comprising the following components in parts by weight:
[0047]
[0048] The modified silicone resin is a terminal hydroxyl methyl phenyl silicone resin having both "bulk" molecular chain segments and "linear" molecular chain segments.
[0049] Furthermore, the molecular structure of the hydroxy-terminated methylphenyl silicone resin is:
[0050]
[0051] Wherein, R1, R2, R3 and R4 are alkyl or phenyl groups, and m, p, q, and n are positive integers greater than 0;
[0052] The viscosity of the terminal hydroxymethylphenyl silicone resin is 2000cps to 3500cps.
[0053] Further, the preparation method of the hydroxy-terminated methylphenyl silicone resin is:
[0054] The first step: hydrolyzing and polycondensing the polyalkoxysilane containing phenyl groups and the polyalkoxysilane to obtain a silsesquioxane with a three-dimensional structure; preferably, the polyalkoxysilane containing phenyl groups and the polyalkoxysilane are hydrolyzed and polycondensed in a molar ratio of 1:1;
[0055] The second step: graft copolymerizing silsesquioxane with a linear polysiloxane to obtain the terminal hydroxy methyl phenyl silicone resin; preferably, graft copolymerizing silsesquioxane with a linear polysiloxane at a molar ratio of 1:2.
[0056] Furthermore, the porcelain-forming filler is one or more combinations of mica powder, talc powder, fumed silica, silica powder or kaolin;
[0057] The heat-insulating filler is nano hollow glass microspheres, or a combination of nano hollow glass microspheres and one or more of expanded perlite, expanded vermiculite, hollow microspheres (micrometer-sized) or silica aerogel;
[0058] The flame retardant is one or more combinations of aluminum hydroxide, magnesium hydroxide, antimony trioxide or zinc borate.
[0059] Furthermore, the flux is any one of glass powder, red lead or borax;
[0060] The dimensional filler is one or more combinations of chopped quartz fibers, chopped glass fibers, high silica fibers or mullite fibers;
[0061] The curing agent is any one of ethyl orthosilicate, propyl orthosilicate, vinyl trimethoxy silane or methyl trimethoxy silane;
[0062] The catalyst comprises a first catalyst and a second catalyst, wherein the first catalyst is any one of chelated tin, zirconium catalyst or aminosilane coupling agent, and the second catalyst is any one of dibutyltin dilaurate, tetrabutyl titanate or stannous octoate.
[0063] The diluent is hexamethyldisiloxane or 120# gasoline or one or more combinations thereof.
[0064] Furthermore, the average particle size of the nano hollow microspheres is 70nm to 90nm, the melting point is 550℃ to 650℃, and the bulk density is 0.30g / cm 3 ~0.43g / cm 3 ;
[0065] The length of the dimensional filler is 0.45mm to 0.50mm;
[0066] The flux is glass powder having a melting point in the range of 250°C to 350°C.
[0067] Further, the catalyst is 3-(2-aminoethyl)-aminopropyltrimethoxysilane and dibutyltin dilaurate in a mass ratio of 1:1;
[0068] The diluent is hexamethyldisiloxane.
[0069] The above-mentioned organic silicon heat-resistant coating based on nano hollow microspheres and its preparation method include:
[0070] Premixing and grinding and dispersing the modified organic silicone resin, the ceramic filler, the flux, the flame retardant and a portion of the diluent to obtain a premixed liquid;
[0071] Add the heat-insulating filler, the dimensional filler and another part of the diluent into the premixed liquid to prepare component A;
[0072] The curing agent and the catalyst are mixed evenly to form component B;
[0073] After mixing component A and component B, spraying to obtain the organic silicon heat-resistant coating, the specific method is as follows:
[0074] preparing a dispersion of component A;
[0075] Add component B to the above dispersion to obtain a coating with a viscosity of 28s to 40s;
[0076] The coating is sprayed and cured at room temperature to obtain an organic silicon heat-resistant coating; when the coating is sprayed, the spraying time is less than or equal to 3 hours; the room temperature curing time is more than 120 hours; the Shore A hardness of the organic silicon heat-resistant coating is ≥70.
[0077] Example:
[0078] The purpose of the present invention is to make up for the shortcomings of existing silicone resin-based heat-resistant coatings, provide a silicone heat-resistant coating based on nano hollow microspheres and a preparation method thereof, which is used for external heat protection of solid rocket engines, resists the harsh aerodynamic thermal environment during flight, and ensures the normal operation of engine structural materials. The external heat-resistant coating of the present invention has a simple construction process. First, the various components are mixed evenly in proportion, formed by spraying, and can be completely cured at room temperature.
[0079] The components of the organic silicon heat-proof coating based on nano hollow microspheres provided by the present invention are mixed in the following weight ratios: 90-150 parts of modified organic silicon resin, 8-15 parts of ceramic filler, 5-10 parts of flux, 55-75 parts of heat-insulating filler, 5-15 parts of dimensional filler, 7-15 parts of flame retardant, 10-15 parts of curing agent, 0.5-1.0 part of catalyst and 200-300 parts of diluent.
[0080] The modified silicone resin is a terminal hydroxymethylphenyl silicone resin (molecular structure shown below) with two molecular chain segment structures of "bulk" and "linear", with a viscosity of 2000cps to 3500cps. The silicone resin is prepared by two-step reaction. First, silsesquioxane with a "bulk" structure is obtained by hydrolyzing and polycondensing polyalkoxysilane containing phenyl groups and polyalkoxysilane; then, silsesquioxane and polysiloxane with a "linear" structure are grafted and copolymerized to finally obtain a terminal hydroxymethylphenyl silicone resin with two molecular chain segment structures of "bulk" and "linear".
[0081]
[0082] Wherein, R1, R2, R3 and R4 are alkyl or phenyl groups, and m, p, q, and n are positive integers greater than 0;
[0083] The modified silicone resin not only has the "linear" soft segment structure of silicone rubber, but also has the "bulky" hard segment structure of conventional silicone resin. Therefore, it has better mechanical properties and thermal stability, thereby further enhancing the coating's anti-aerodynamic erosion effect.
[0084] The above-mentioned ceramic filler is one or more combinations of mica powder, talc powder, fumed silica, silicon micropowder or kaolin, preferably mica powder and kaolin. The ceramic filler can not only improve the thermal stability of the coating, but also can be ceramicized in situ after the organic polymer is degraded, adhere to the upper surface of the coating, and further improve the thermal protection performance.
[0085] The above-mentioned flux is any one of glass powder, red lead or borax, preferably low-melting point glass powder. The initial decomposition temperature of low-melting point glass powder is similar to that of modified silicone resin (250°C~350°C). The liquid phase produced by the melting of glass powder coats and connects the porcelain filler and the decomposition products of silicone rubber, limits the loss of decomposition products, and helps to form a denser ceramic body.
[0086] The above-mentioned heat-insulating filler is nano hollow glass microspheres, or a combination of nano hollow glass microspheres and one or more of expanded perlite, expanded vermiculite, hollow microspheres (micrometer level) or silica aerogel, preferably nano hollow microspheres. The heat-insulating filler is the main filler and key component of the heat-resistant coating, which can significantly reduce the density and thermal conductivity of the coating. Figure 1 and Figure 2 The nano hollow microspheres of the present invention have an average particle size of 70nm to 90nm and a large specific surface area, and have excellent reinforcement and toughening effects. At the same time, the internal hollow structure can effectively reduce the coating density and thermal conductivity. Therefore, they have the dual advantages of reinforcing fillers and thermal insulation fillers.
[0087] The above-mentioned dimensional filler is one or more combinations of chopped quartz fibers, chopped glass fibers, high silica fibers or mullite fibers, preferably chopped quartz fibers or chopped glass fibers, with a size of 0.45 mm to 0.50 mm. The role of the dimensional filler is to play a role in wear resistance and reinforcement after the organic polymer is carbonized at high temperature, forming a spatial link between the carbonized layers to prevent the coating from falling off over a large area under pneumatic heating.
[0088] The flame retardant is one or more combinations of aluminum hydroxide, magnesium hydroxide, antimony trioxide or zinc borate, preferably aluminum hydroxide or magnesium hydroxide. The flame retardant prevents the coating from burning violently under high temperature conditions and avoids damage to the coating due to burning. Different flame retardants have different flame retardant mechanisms.
[0089] The above diluent is hexamethyldisiloxane or 120# gasoline, both of which are environmentally friendly and non-toxic solvents. Considering the compatibility with the system and construction safety, hexamethyldisiloxane is preferred.
[0090] The curing agent is any one of ethyl orthosilicate, propyl orthosilicate, vinyl trimethoxy silane or methyl trimethoxy silane.
[0091] The catalysts are 3-(2-aminoethyl)-aminopropyltrimethoxysilane and dibutyltin dilaurate, and the addition ratio of the two is 1:1. The two catalysts are matched with the curing agent to achieve room temperature curing of the coating formula. Specifically, the former has a higher catalytic activity, and the latter is helpful for the room temperature curing of the modified silicone resin. The former catalyst can also be a zirconium catalyst or a chelated tin, and the latter catalyst can also be tetrabutyl titanate or stannous octoate.
[0092] The method for preparing the organosilicon heat-resistant coating based on nano hollow microspheres of the present invention is as follows:
[0093] Step 1: Premix the modified silicone resin, ceramic filler, flux, flame retardant and appropriate diluent in proportion, grind and disperse them in a sand mill at a speed of 1500 rpm to 2000 rpm for 20 min to 30 min to prepare a premixed liquid;
[0094] Step 2: Add the heat-insulating filler, dimensional filler and appropriate amount of diluent in proportion to the premixed liquid, and disperse them in a high-speed disperser at a speed of 1000 rpm to 2000 rpm for 20 min to 40 min to prepare coating component A;
[0095] Step 3: Evenly mix the curing agent and two catalysts according to the proportion to form component B, and store it in a sealed container.
[0096] The construction process of the organosilicon heat-resistant coating based on nano hollow microspheres of the present invention is as follows:
[0097] Step 1: Weigh the coating component A and the diluent in proportion, disperse them in a high-speed disperser for 15 to 30 minutes, and then filter them through a 30-mesh metal filter;
[0098] Step 2, weigh component B according to the proportion and add it into the above dispersion liquid, and disperse it evenly to obtain the coating;
[0099] Step 3: Use a 4-cup viscometer to test the coating viscosity and control the viscosity between 28s and 40s;
[0100] Step 4: Pour the coating into the material tank and spray the test piece with manual or automatic spraying equipment. The spraying time shall not exceed 3 hours;
[0101] Step 5: The sprayed coating specimen is cured at room temperature (10°C to 35°C) for more than 120 hours to be completely cured, and the Shore A hardness reaches more than 70.
[0102] The present invention adopts modified silicone resin as the matrix. The prepared silicone thermal protection coating maintains excellent resistance to aerodynamic scour. By adding a large number of nano hollow microspheres as thermal insulation materials, the addition amount of other solid fillers is greatly reduced, so that the coating has lower density, lower thermal conductivity and higher toughness, providing technical support for the external thermal protection of the new generation of aircraft.
[0103] The present invention is further described below by way of Examples 1 to 3.
[0104] Table 1 shows the components of the organic silicon heat-resistant coating based on nano hollow microspheres provided in Examples 1 to 3 of the present invention and the weight ratio of each component. The amounts in Table 1 are expressed in parts by mass. Among them, the measured values of the key parameters of the nano hollow microspheres used are as follows: the average particle size is about 80nm, the melting point is about 575℃, and the bulk density is about 0.39g / cm 3 .
[0105] Table 1
[0106]
[0107]
[0108] In other embodiments of the present invention, the components may also be made of other materials listed in the present invention.
[0109] Example 1
[0110] The specific preparation method of the above-mentioned organic silicon heat-resistant coating based on nano hollow microspheres is as follows:
[0111] (1) Modified silicone resin, mica powder, low melting point glass powder, aluminum hydroxide, magnesium hydroxide and hexamethyldisiloxane are weighed in proportion and blended, and then ground by a basket sand mill at a grinding speed of 1800 rpm for 30 minutes to prepare a premixed liquid; (2) Nano hollow microspheres, hollow microspheres (micrometer level), short quartz fibers and hexamethyldisiloxane are added to the premixed liquid, and dispersed by a high-speed disperser at a speed of 1200 rpm for 30 minutes to prepare a coating component A; (3) Propylene orthosilicate, chelated tin and dibutyltin dilaurate are mixed to obtain a component B.
[0112] In the modified silicone resin used in this embodiment, R1 to R4 are all methyl groups.
[0113] The construction process of the above-mentioned organic silicon heat-resistant coating based on nano hollow microspheres is as follows:
[0114] (1) First, the coating component A and hexamethyldisiloxane were weighed in proportion, dispersed for 20 minutes using a high-speed disperser, and then filtered using a 30-mesh metal filter; (2) Component B was then added to the above dispersion, dispersed for 5 minutes, and 4 cups were coated with the viscosity controlled at 35 seconds; (3) The coating was poured into a material tank, and various coating specimens were prepared and tested by manual spraying. The results are shown in Table 2.
[0115] Example 2
[0116] The specific preparation method of the above-mentioned organic silicon heat-resistant coating based on nano hollow microspheres is as follows:
[0117] (1) Modified silicone resin, mica powder, low melting point glass powder, aluminum hydroxide and hexamethyldisiloxane are weighed in proportion and blended, and then ground by a basket sand mill at a grinding speed of 1800 rpm for 30 min to prepare a premixed liquid; (2) Hollow glass microspheres, expanded vermiculite, chopped quartz fibers and an appropriate amount of hexamethyldisiloxane are added to the premixed liquid, and dispersed by a high-speed disperser at a speed of 1200 rpm for 30 min to prepare a coating component A; (3) Propyl orthosilicate, 3-(2-aminoethyl)-aminopropyltrimethoxysilane and dibutyltin dilaurate are mixed to obtain a coating component B.
[0118] The construction process of the above-mentioned organic silicon heat-resistant coating based on nano hollow microspheres is as follows:
[0119] (1) First, the coating component A and hexamethyldisiloxane were weighed in proportion, dispersed for 20 minutes using a high-speed disperser, and then filtered using a 30-mesh metal filter; (2) Component B was then added to the above dispersion, dispersed for 5 minutes, and 4 cups were coated with a viscosity controlled at 38 seconds; (3) The coating was poured into a material tank, and various coating specimens were prepared and tested by manual spraying. The results are shown in Table 2.
[0120] Example 3
[0121] The specific preparation method of the above-mentioned organic silicon heat-resistant coating based on nano hollow microspheres is as follows:
[0122] (1) Modified silicone resin, fumed silica, red lead, magnesium hydroxide and hexamethyldisiloxane are weighed in proportion and blended, and then ground by a basket sand mill at a grinding speed of 1800 rpm for 30 min to prepare a premixed liquid; (2) Hollow glass microspheres, expanded perlite, chopped glass fibers and an appropriate amount of hexamethyldisiloxane are added to the premixed liquid, and dispersed by a high-speed disperser at a speed of 1200 rpm for 30 min to prepare a coating component A; (3) Vinyltrimethoxysilane, 3-(2-aminoethyl)-aminopropyltrimethoxysilane and dibutyltin dilaurate are mixed to obtain component B.
[0123] The construction process of the above-mentioned organic silicon heat-resistant coating based on nano hollow microspheres is as follows:
[0124] (1) First, the coating component A and hexamethyldisiloxane were weighed in proportion, dispersed for 20 minutes using a high-speed disperser, and then filtered using a 30-mesh metal filter; (2) Component B was then added to the above dispersion, dispersed for 5 minutes, and 4 cups were coated with a viscosity controlled at 31 seconds; (3) The coating was poured into a material tank, and various coating specimens were prepared and tested by manual spraying. The results are shown in Table 2.
[0125] Comparative Example
[0126] The difference between this comparative example and Example 1 is that the types of hollow microspheres used are different, and the other components are the same. The specific parameters of the hollow microspheres are as follows: average particle size of about 50 μm, melting point of about 580°C, bulk density of about 0.32 g / cm 3 Comparative Example Various coating test pieces similar to those in Examples 1 to 3 were prepared and tested in accordance with the requirements of the process documents. The results are shown in Table 2.
[0127] Table 2
[0128]
[0129] As can be seen from Table 2, the heat-resistant coating prepared by the present invention using modified silicone resin as the matrix and nano hollow microspheres as the main filler has better performance than the comparative example in key indicators such as density, thermal conductivity, and elongation.
[0130] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0131] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.
Claims
1. A silicone heat-resistant coating based on hollow nanospheres, characterized in that: The composition includes the following components in parts by weight: The modified organic silicone resin is a terminal hydroxyl methyl phenyl silicone resin including a three-dimensional structure molecular chain segment and a linear structure molecular chain segment.
2. The organic silicon heat-resistant coating based on nano hollow microspheres according to claim 1, characterized in that: The heat-insulating filler is nano hollow glass microspheres, or a combination of nano hollow glass microspheres and one or more of expanded perlite, expanded vermiculite, micron-sized hollow microspheres or silica aerogel.
3. The organic silicon heat-resistant coating based on nano hollow microspheres according to claim 2, characterized in that: The average particle size of the nano hollow glass microspheres is 70nm~90nm, the melting point is 550℃~650℃, and the bulk density is 0.30g / cm 3 ~0.43g / cm 3 .
4. The organic silicon heat-resistant coating based on nano hollow microspheres according to claim 1, characterized in that: The molecular structure of the hydroxy-terminated methylphenyl silicone resin is: Wherein, R1, R2, R3 and R4 are alkyl or phenyl groups, and m, p, q, and n are positive integers greater than 0; The viscosity of the terminal hydroxymethylphenyl silicone resin is 2000-3500 cps.
5. The organic silicon heat-resistant coating based on nano hollow microspheres according to claim 1, characterized in that: The preparation method of the terminal hydroxymethylphenyl silicone resin is: The polyalkoxysilane containing phenyl groups and the polyalkoxysilane are hydrolyzed and polycondensed to obtain a silsesquioxane having a three-dimensional structure; The silsesquioxane is grafted and copolymerized with the linear polysiloxane to obtain the terminal hydroxyl methyl phenyl silicone resin.
6. The organic silicon heat-resistant coating based on hollow nano-microspheres according to claim 1, characterized in that: The porcelain-forming filler is one or more of mica powder, talc powder, fumed silica, silica powder or kaolin; The flame retardant is one or more of aluminum hydroxide, magnesium hydroxide, antimony trioxide or zinc borate.
7. The organic silicon heat-resistant coating based on nano hollow microspheres according to claim 1, characterized in that: The flux is one or more of glass powder, red lead or borax; The dimensional filler is one or more of chopped quartz fiber, chopped glass fiber, high silica fiber or mullite fiber; The curing agent is one or more of ethyl orthosilicate, propyl orthosilicate, vinyl trimethoxy silane or methyl trimethoxy silane; The catalyst comprises a first catalyst and a second catalyst, the first catalyst is one or more of chelated tin, a zirconium catalyst or an aminosilane coupling agent, and the second catalyst is one or more of dibutyltin dilaurate, tetrabutyl titanate or stannous octoate; The diluent is one or more of hexamethyldisiloxane and 120# gasoline.
8. The organic silicon heat-resistant coating based on nano hollow microspheres according to claim 7, characterized in that: The flux is glass powder with a melting point in the range of 250°C to 350°C; The length of the dimensional filler is 0.45 to 0.50 mm; The catalyst is a composition of 3-(2-aminoethyl)-aminopropyltrimethoxysilane and dibutyltin dilaurate in a mass ratio of 1:1; The diluent is hexamethyldisiloxane.
9. A method for preparing a heat-resistant silicone coating based on hollow nanospheres according to any one of claims 1 to 8, characterized in that: include: Premixing and grinding and dispersing the modified organic silicone resin, the ceramic filler, the flux, the flame retardant and a portion of the diluent to obtain a premixed liquid; Add the heat-insulating filler, the dimensional filler and another part of the diluent into the premixed liquid to prepare component A; The curing agent and the catalyst are mixed evenly to form component B; After mixing component A and component B, spraying is performed to obtain an organic silicone heat-resistant coating.
10. The method for preparing a heat-resistant silicone coating based on hollow nano-microspheres according to claim 9, characterized in that: After mixing component A and component B, the specific method of spraying to obtain the organic silicon heat-resistant coating is as follows: preparing a dispersion of component A; Add component B to the above dispersion to obtain a coating with a viscosity of 28 to 40 seconds; The coating is sprayed and cured at room temperature to obtain an organic silicon heat-resistant coating; when the coating is sprayed, the spraying time is less than or equal to 3 hours; the room temperature curing time is more than 120 hours; the Shore A hardness of the organic silicon heat-resistant coating is ≥70.
Citation Information
Patent Citations
Novel nano ceramic thermal insulation material
CN106366860A
Novel insulating material for coating bare overhead conductor and preparation method thereof
CN109021578A
Preparation and process of in-situ ceramic high-temperature resistance heat insulation coating
CN110479564A
High-performance heat-proof coating based on interpenetrating network structure and preparation method of high-performance heat-proof coating
CN115286995A
High-temperature-resistant and ablation-resistant thermal protection coating and preparation method thereof
CN116262866A
Cited By
Aerodynamic thermal environment-resistant low-absorption high-emission thermal control coating and preparation method thereof
CN119320601A
Organic silicon heat insulation coating and preparation method thereof