Fluorescent powder, preparation method thereof and LED light-emitting device
By doping A2B4O8 with Ce element, blue cyan light under near-ultraviolet excitation is produced, which solves the problem of cyan gap in the spectrum of near-ultraviolet LED chips, provides a cyan phosphor adapted to the 410nm wavelength, and realizes full-spectrum lighting and Improvement of color rendering index.
Patent Information
- Application Number
- CN202410707743.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the white LED spectrum obtained by combining near-ultraviolet LED chips and phosphors has an obvious cyan gap, and lacks high-performance blue-cyan phosphors suitable for wavelengths around 410 nm, which affects the flatness and color rendering index of the spectrum.
By doping A2B4O8 with Ce element, Ce3+ ions undergo a 4f → 5d transition under near-ultraviolet light excitation, producing blue-cyan light, thus providing a blue-cyan phosphor for white light LEDs, which is prepared using a simple sintering process Develop phosphors suitable for LED chips with a wavelength of around 410nm.
It fills the shortcomings of cyan emission in the spectrum of near-ultraviolet excitation white light LED technology, provides full-spectrum illumination, and has a simple preparation process and low cost. The resulting phosphor particles have uniform size and smooth surface, making them suitable for subsequent packaging.
Smart Images

Figure CN118725862A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to a fluorescent powder and a preparation method thereof, and an LED luminescent device. Background Art
[0002] White light LEDs based on LED (light-emitting diode) chip technology have the advantages of low energy consumption, long life and good stability, and have become the most widely used lighting and display light source. There are two main ways to realize white light LEDs. One is a white light LED device composed of red, cyan and blue primary color LED chips, but the manufacturing process is relatively complex and the cost is high. The other is a combination of LED chips and luminescent materials to achieve white light emission (fluorescent conversion LED, pc-LED). This method has a simpler process and lower cost, and the white light obtained has the advantages of high color rendering index, wide color gamut and good stability.
[0003] There are two main ways to achieve white light emission by combining LED chips with luminescent materials. One is to obtain white light by combining (near) ultraviolet LED chips with three types of phosphors that effectively absorb (near) ultraviolet light and emit red, green and blue light. The second is to coat the blue light LED chip with a wavelength of 420-480nm with phosphors that can effectively absorb blue light and emit yellow light.
[0004] CN114883471A discloses an LED device for synthesizing a white light source from a perovskite quantum dot solution, wherein the white light is formed by mixing part of the blue light, the yellow light and the red light. 3-x Br x The photoluminescence property of the light source absorbs part of the blue light and excites a mixture of yellow and red light. Then, part of the blue light is mixed with the mixture of yellow and red light to synthesize white light.
[0005] CN106848039A discloses a white light emitting device, which uses an organic semiconductor polymer highly isotactic poly 3-hexylthiophene as a light conversion layer, which absorbs blue light emitted by a light emitting diode and converts it into yellow light, and the yellow light and blue light are mixed to form white light.
[0006] At present, most of the blue light chips on the market use 450nm combined with yttrium aluminum garnet yellow phosphor (YAG:Ce 3+) and a red phosphor to obtain white light. CN102367383A discloses a white light emitting diode with high color rendering property, using indium gallium nitride as a blue chip, and using a compound that is stable and easily obtained in air as a raw material. A novel silicon-based nitride oxide prepared at a lower temperature and normal pressure is used as a red fluorescent material, and doped with yttrium aluminum garnet yellow phosphor and epoxy resin to prepare a resin glue layer. After assembly, a white light emitting diode with high color rendering property is obtained. However, in this combination method, blue light is likely to overflow, which has an adverse effect on the human eye, and has poor color rendering property and high color temperature, belonging to cold white light. Researchers often use a novel yellow phosphor with more red components to replace YAG or combine YAG with a red phosphor to improve the color rendering index of the obtained white light.
[0007] In recent years, with the development of chip technology, the "ultraviolet / near-ultraviolet LED chip + trichromatic phosphor" scheme has more and more advantages. The white light LED obtained by this method can achieve a flat spectral distribution in the entire visible light range, and has advantages such as high color rendering index and color stability. In this approach, the phosphor has an important influence on the performance of the white light LED. However, the spectrum obtained by this method usually has an obvious cyan gap. Therefore, it is necessary to develop a variety of high-performance blue-cyan emitting phosphors that match near-ultraviolet LED chips, especially a phosphor system that adapts to LED chips with a wavelength of about 410 nm.
[0008] Therefore, providing a phosphor that can match near-ultraviolet LED chips, especially a phosphor that can adapt to LED chips with a wavelength of about 410 nm, is an urgent problem to be solved at present. Summary of the Invention
[0009] To solve the above technical problems, the purpose of the present invention is to provide a phosphor, its preparation method and an LED lighting device. The present invention provides a blue-cyan phosphor for white light LED by doping Ce element in A2B4O8. The Ce 3+ ions undergo a 4f→5d transition under near-ultraviolet light excitation and emit blue-cyan light, thus filling the deficiency of cyan emission in the spectrum of near-ultraviolet excited white light LED technology in the prior art, and can be used for full-spectrum lighting. Moreover, the phosphor provided by the present invention can also well adapt to LED chips with a wavelength of about 410 nm.
[0010] To achieve this purpose, the present invention adopts the following technical solutions:
[0011] In the first aspect, the present invention provides a phosphor, and the chemical formula of the phosphor is: A2B4O8:xCe 3+ ; wherein, 0 < x ≤ 0.1, A includes alkaline earth metal elements, and B includes rare earth elements.
[0012] In the present invention, 0 < x ≤ 0.1, such as 0.002, 0.004, 0.006, 0.008, 0.010, 0.012, 0.015, 0.020, 0.025, 0.030, 0.035, 0.040, 0.045, 0.050, 0.055, 0.060, 0.065, 0.070, 0.075, 0.080, 0.085, 0.090, 0.095 or 0.1, etc.
[0013] In the present invention, by doping Ce element into A2B4O8, Ce 3+ ions undergo 4f→5d transitions under near-ultraviolet light excitation, emitting blue-cyan light, thereby providing a blue-cyan phosphor for white LEDs, filling the deficiency of cyan emission in the spectrum of the existing near-ultraviolet-excited white LED technology, and can be used for full-spectrum lighting. Moreover, the phosphor provided by the present invention can also be well adapted to LED chips with a wavelength of about 410 nm.
[0014] The present invention provides a composition of a blue-cyan phosphor for white LEDs. In the present invention, if the value of x is greater than 0.1, the luminous intensity will be too low; if the alkaline earth metal element is not used at the A site or the rare earth element is not used at the B site in the present invention, the structure of the compound cannot be maintained, and thus a blue-cyan phosphor cannot be obtained.
[0015] Preferably, the alkaline earth metal element includes any one or a combination of at least two of Be, Mg, Ca, Sr, Ba or Ra. Among them, typical but non-limiting combinations are combinations of Be and Mg, Mg and Ca, Ca and Sr, Ca and Ba, Sr and Ba, or Sr and Ra, etc.
[0016] Preferably, the rare earth element includes any one or a combination of at least two of La, Nd, Sm, Gd, Eu, Dy, Ho, Y, Er, Tm, Yb, Sc or Lu. Among them, typical but non-limiting combinations are combinations of Gd and Y, La and Y, Nd and Gd, Gd and Ho, Sm and Y, Gd and Yb, or Y and Lu, etc.
[0017] Preferably, the phosphor is orthorhombic.
[0018] Preferably, the space group of the phosphor is Pnma.
[0019] Preferably, the structure of the phosphor is a spinel structure, where A is filled in the tetrahedral voids and B is filled in the octahedral voids.
[0020] Preferably, the wavelength at which the phosphor is effectively excited by near-ultraviolet light is 400-420 nm, for example, 400 nm, 402 nm, 404 nm, 406 nm, 408 nm, 410 nm, 412 nm, 414 nm, 416 nm, 418 nm or 420 nm.
[0021] Preferably, the strongest emission peak of the phosphor is 450-480 nm, for example, 450 nm, 453 nm, 456 nm, 459 nm, 462 nm, 465 nm, 468 nm, 471 nm, 474 nm, 477 nm or 480 nm.
[0022] In a second aspect, the present invention provides a method for preparing the phosphor according to the first aspect, the preparation method comprising:
[0023] Mixing raw material A, raw material B and raw material Ce to obtain a mixture;
[0024] The mixture is sintered to obtain the phosphor.
[0025] The fluorescent powder preparation method of the present invention has a simple process and is pollution-free. Furthermore, the fluorescent powder with uniform particle size and smooth surface can be obtained by adopting the preparation method of the present invention, which is beneficial to the subsequent encapsulation of the fluorescent powder.
[0026] Preferably, the A raw material includes any one of A oxide, A hydroxide or A salt, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of A oxide and A hydroxide, a combination of A hydroxide and A salt, a combination of A oxide and A salt, or a combination of A oxide, A hydroxide and A salt, etc.
[0027] Preferably, the B raw material includes any one of B oxide, B hydroxide or B salt, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of B oxide and B hydroxide, a combination of B hydroxide and B salt, a combination of B oxide and B salt, or a combination of B oxide, B hydroxide and B salt, etc.
[0028] Preferably, the Ce raw material includes any one of Ce oxide, Ce hydroxide or Ce salt, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of Ce oxide and Ce hydroxide, a combination of Ce hydroxide and Ce salt, a combination of Ce oxide and Ce salt, or a combination of Ce oxide, Ce hydroxide and Ce salt, etc.
[0029] Preferably, the A salt, B salt or Ce salt independently includes any one of carbonate, halide salt, sulfate, chlorate, acetate or nitrate, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of carbonate and halide salt, a combination of halide salt and sulfate, a combination of sulfate and chlorate, a combination of chlorate and acetate, a combination of chlorate, acetate and nitrate, or a combination of carbonate, halide salt and sulfate, etc.
[0030] Preferably, the mixing comprises grinding.
[0031] Preferably, the sintering temperature is 1200-1600°C, for example, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C, 1550°C or 1600°C.
[0032] In the present invention, if the sintering temperature is higher than 1600°C, the hardness of the obtained phosphor will be high, and it will be difficult to grind. It will be impossible to form a phosphor with uniform particle size and smooth surface, which is not conducive to subsequent packaging and other treatments of the phosphor. If the sintering temperature is lower than 1200°C, the low temperature conditions make it impossible for the raw materials to react, resulting in the inability to synthesize the phosphor.
[0033] Preferably, the sintering time is 1 to 10 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h.
[0034] In the present invention, if the sintering time is too short, the reaction will be incomplete, and the phosphor cannot be prepared; when the sintering time is too long, energy will be wasted.
[0035] Preferably, the sintering atmosphere includes a reducing atmosphere.
[0036] Preferably, the reducing atmosphere comprises a reducing gas.
[0037] Preferably, the reducing gas comprises a mixed gas of nitrogen and hydrogen.
[0038] Preferably, the reducing gas comprises carbon monoxide gas.
[0039] Optionally, when the present invention adopts a mixed gas of nitrogen and hydrogen as the reducing gas, the specific composition content is 10 vol% hydrogen (H2) and 90 vol% nitrogen (N2).
[0040] Preferably, the sintering process further includes grinding the sintered product.
[0041] In a third aspect, the present invention provides an LED light-emitting device, comprising a light-emitting device and a phosphor composition located in the light-emitting device, wherein the phosphor composition comprises the phosphor described in the first aspect.
[0042] Preferably, among the light-emitting devices, at least one light-emitting device is capable of emitting light in the near-ultraviolet wavelength region.
[0043] Preferably, the phosphor composition further includes any one of blue phosphor, green phosphor, yellow phosphor or red phosphor that can be effectively excited by near-ultraviolet light, or a combination of at least two of them, wherein a typical but non-limiting combination is a combination of blue phosphor, green phosphor and red phosphor, or a combination of blue phosphor, yellow phosphor and red phosphor, etc.
[0044] Preferably, the central emission wavelength of the blue phosphor is 440-470 nm, for example, 440 nm, 445 nm, 450 nm, 455 nm, 460 nm, 465 nm or 470 nm.
[0045] Preferably, the central emission wavelength of the green phosphor is 500-540 nm, for example, 500 nm, 505 nm, 510 nm, 515 nm, 520 nm, 525 nm, 530 nm, 535 nm or 540 nm.
[0046] Preferably, the central emission wavelength of the yellow phosphor is 550-590 nm, for example, 550 nm, 555 nm, 560 nm, 565 nm, 570 nm, 575 nm, 580 nm, 585 nm or 590 nm.
[0047] Preferably, the central emission wavelength of the red phosphor is 620-650 nm, for example, 620 nm, 627 nm, 629 nm, 631 nm, 635 nm or 650 nm.
[0048] Optionally, the chemical formula of the blue phosphor used in the present invention includes BaMgAl 10 O 17 :Eu 2+ or (Sr,Ba) 10 (PO4)6Cl2:Eu 2+ Any one or a combination of two.
[0049] Optionally, the chemical formula of the green phosphor used in the present invention includes (Ba, Sr)SiO4:Eu 2+ Or (Y,Lu)3(Ga,Al)5O 12 :Ce 3+ Any one or a combination of two.
[0050] Optionally, the chemical formula of the yellow phosphor used in the present invention includes (Y, Gd)3Al5O 12 :Ce 3+ .
[0051] Optionally, the chemical formula of the red phosphor used in the present invention includes (Ca, Sr)AlSiN3:Eu 2+ 、(Ca,Sr,Ba)2Si5N8:Eu 2+ or KSiF6:Mn 4+ Any one or a combination of at least two of the following.
[0052] Preferably, the correlated color temperature of the LED light-emitting device is 2500-7000K, and there is an uninterrupted continuous spectrum in the wavelength range of 400-750nm, wherein the range of the correlated color temperature is "2500-7000K", for example, 2500K, 3000K, 3500K, 4000K, 4500K, 5000K, 5500K, 6000K, 6500K or 7000K, etc.
[0053] Compared with the prior art, the present invention has at least the following beneficial effects:
[0054] (1) The present invention doped Ce element into A2B4O8, Ce 3+ When excited by near-ultraviolet light, the ions undergo a 4f→5d transition and emit blue-cyan light, thereby providing a blue-cyan phosphor for white light LEDs, which fills the deficiency of cyan emission in the spectrum of near-ultraviolet excited white light LED technology in the prior art and can be used for full-spectrum lighting. In addition, the phosphor provided by the present invention can also be well adapted to LED chips with a wavelength of about 410nm.
[0055] (2) The preparation method of the phosphor of the present invention is simple, pollution-free, and has low preparation cost. The preparation method of the present invention can obtain phosphor with uniform particle size and smooth surface, which is beneficial to the subsequent encapsulation of the phosphor. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 is the XRD pattern of the phosphor in Example 1;
[0057] Figure 2 This is the emission spectrum of the phosphor obtained in Example 1;
[0058] Figure 3 This is the excitation spectrum of the phosphor obtained in Example 1;
[0059] Figure 4 This is the emission spectrum of the phosphor obtained in Example 3;
[0060] Figure 5 This is the excitation spectrum of the phosphor obtained in Example 3;
[0061] Figure 6 This is the emission spectrum of the phosphor obtained in Example 6;
[0062] Figure 7 This is the excitation spectrum of the phosphor obtained in Example 6;
[0063] Figure 8 This is the electroluminescence spectrum of the phosphor obtained in Example 1 in the LED light-emitting device. DETAILED DESCRIPTION
[0064] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0065] Example 1
[0066] This embodiment provides a phosphor, the chemical formula of which is: CaSrLu4O8:0.01Ce 3+ The phosphor is an orthorhombic crystal with a space group of Pnma and a spinel structure, in which Ca 2+ and Sr 2+ Ions fill the tetrahedral voids, Lu 3+ Fill in the octahedral voids.
[0067] This embodiment also provides a method for preparing the phosphor, including:
[0068] CaCO3, SrCO3, Lu2O3 and CeO2 are uniformly mixed by grinding in the stoichiometric ratio of Ca, Sr, Lu and Ce elements of 1:1:3.99:0.01, and the mixed product is sintered in a reducing atmosphere composed of 10vol% H2 and 90vol% N2 at a sintering temperature of 1350°C for 5h, and then ground to obtain a phosphor.
[0069] The XRD pattern of the phosphor obtained in this example is as follows: Figure 1 As shown by Figure 1 It can be seen that the synthesized phosphor is pure phase and has no impurities.
[0070] The emission spectrum of the phosphor in this embodiment is shown in FIG. Figure 2 As shown, through Figure 2 It can be seen that the emission peak obtained by excitation with near-ultraviolet light of 408 nm wavelength is 478 nm; the excitation spectrum of the phosphor in this embodiment is as follows Figure 3 As shown, through Figure 3It can be seen that when light with a wavelength of 478 nm is used as the emission light source, the excitation peak is measured at 408 nm.
[0071] Example 2
[0072] This embodiment provides a phosphor, the chemical formula of which is: CaSrLu4O8:0.03Ce 3+ The phosphor is an orthorhombic crystal with a space group of Pnma and a spinel structure, in which Ca 2+ and Sr 2+ Ions fill the tetrahedral voids, Lu 3+ Fill in the octahedral voids.
[0073] This embodiment also provides a method for preparing the phosphor, including:
[0074] CaCO3, SrCO3, Lu2O3 and CeO2 are uniformly mixed by grinding in the stoichiometric ratio of Ca, Sr, Lu and Ce elements of 1:1:3.97:0.03. The mixed product is sintered in a reducing atmosphere consisting of 10 vol% H2 and 90 vol% N2 at a sintering temperature of 1350°C for 5 hours. The phosphor is then obtained by grinding.
[0075] Example 3
[0076] This embodiment provides a fluorescent powder, the chemical formula of which is: Ca 0.5 Sr 1.5 Lu4O8:0.01Ce 3+ The phosphor is an orthorhombic crystal with a space group of Pnma and a spinel structure, in which Ca 2+ and Sr 2+ Ions fill the tetrahedral voids, Lu 3+ Fill in the octahedral voids.
[0077] This embodiment also provides a method for preparing the phosphor, including:
[0078] CaCO3, SrCO3, Lu2O3 and CeO2 are uniformly mixed by grinding in the stoichiometric ratio of Ca, Sr, Lu and Ce elements of 0.5:1.5:3.99:0.01. The mixed product is sintered in a reducing atmosphere composed of 10 vol% H2 and 90 vol% N2 at a sintering temperature of 1250°C for 6 hours. The phosphor is then obtained by grinding.
[0079] The emission spectrum of the phosphor in this embodiment is shown in FIG. Figure 4 As shown, through Figure 4It can be seen that the emission peak obtained by excitation with near-ultraviolet light of 406 nm wavelength is 465 nm; the excitation spectrum of the phosphor in this embodiment is as follows Figure 5 As shown, through Figure 5 It can be seen that when light with a wavelength of 465 nm is used as the emission light source, the excitation peak is measured at 406 nm.
[0080] Example 4
[0081] This embodiment provides a phosphor, the chemical formula of which is: Sr2Lu4O8:0.01Ce 3+ The phosphor is an orthorhombic crystal with a space group of Pnma and a spinel structure. 2+ Ions fill the tetrahedral voids, Lu 3+ Fill in the octahedral voids.
[0082] This embodiment also provides a method for preparing the phosphor, including:
[0083] SrCO3, Lu2O3 and CeO2 are uniformly mixed by grinding in the stoichiometric ratio of Sr, Lu and Ce elements of 2:3.99:0.01, and the mixed product is sintered in a reducing atmosphere consisting of 10 vol% H2 and 90 vol% N2 at a sintering temperature of 1600°C for 10 hours. The phosphor is then obtained by grinding.
[0084] Example 5
[0085] This embodiment provides a fluorescent powder, the chemical formula of which is: Ba 0.5 Sr 1.5 Lu4O8:0.01Ce 3+ The phosphor is an orthorhombic crystal with a space group of Pnma and a spinel structure. 2+ and Sr 2+ Ions fill the tetrahedral voids, Lu 3+ Fill in the octahedral voids.
[0086] This embodiment also provides a method for preparing the phosphor, including:
[0087] BaCO3, SrCO3, Lu2O3 and CeO2 are uniformly mixed by grinding in the stoichiometric ratio of Ba, Sr, Lu and Ce elements of 0.5:1.5:3.99:0.01. The mixed product is sintered in a reducing atmosphere composed of 10 vol% H2 and 90 vol% N2 at a sintering temperature of 1250°C for 5 hours. The phosphor is then obtained by grinding.
[0088] Example 6
[0089] This embodiment provides a phosphor, the chemical formula of which is: BaSrLu4O8:0.01Ce 3+ The phosphor is an orthorhombic crystal with a space group of Pnma and a spinel structure. 2+ and Sr 2+ Ions fill the tetrahedral voids, Lu 3+ Fill in the octahedral voids.
[0090] This embodiment also provides a method for preparing the phosphor, including:
[0091] BaCO3, SrCO3, Lu2O3 and CeO2 are uniformly mixed by grinding in the stoichiometric ratio of Ba, Sr, Lu and Ce elements of 1:1:3.99:0.01. The mixed product is sintered in a reducing atmosphere consisting of 10 vol% H2 and 90 vol% N2 at a sintering temperature of 1350°C for 6 hours. The phosphor is then obtained by grinding.
[0092] The emission spectrum of the phosphor in this embodiment is shown in FIG. Figure 6 As shown, through Figure 6 It can be seen that the emission peak obtained by excitation with near-ultraviolet light of 400 nm wavelength is 451 nm; the excitation spectrum of the phosphor in this embodiment is as follows Figure 7 As shown, through Figure 7 It can be seen that when light with a wavelength of 451 nm is used as the emission light source, the excitation peak is measured at 400 nm.
[0093] Comparative Example 1
[0094] The difference between this comparative example and Example 1 is that the chemical formula of the phosphor provided in this comparative example is: CaSrLu4O8:0.01Bi 3+ The rest are the same as in Example 1.
[0095] The phosphor provided in Example 1 is mixed with (Ba, Sr) 10 (PO4)6Cl2:Eu 2+ (Central emission wavelength is 450nm), Lu3Al5O 12 :Ce 3+ (central emission wavelength is 520nm) and CaAlSiN3:Eu 2+ The phosphor composition is composed of a phosphor composition (with a central emission wavelength of 635nm), and the phosphor composition is combined with a light-emitting device to form an LED light-emitting device, wherein the light-emitting device is a 410nm near-ultraviolet chip, the color rendering index of the light-emitting device can reach 96.9, and the correlated color temperature is 4960K.
[0096] The emission bands of the phosphors obtained in Examples 1-6 and Comparative Example 1 were tested by using FLS1000 to test the emission spectrum and excitation spectrum of the phosphors obtained. The emission peak and excitation peak of the phosphors obtained by the test are shown in Table 1
[0097] Table 1
[0098]
[0099]
[0100] The test results show that:
[0101] (1) It can be seen from Examples 1 to 6 that the emission peaks of the phosphors provided in Examples 1-6 after being excited by ultraviolet light are 451 to 478 nm, and the excitation peaks are 400 to 408 nm. It can be seen that the phosphors of the present invention emit blue-cyan light under near-ultraviolet light excitation, thereby providing a blue-cyan phosphor for white light LEDs, which fills the deficiency of cyan emission in the spectrum of near-ultraviolet excited white light LED technology in the prior art, and can be used for full-spectrum lighting. In addition, the phosphors provided by the present invention can also be well adapted to LED chips with a wavelength of about 410 nm. Among them, the phosphors obtained in Example 1 are coated on a 410 nm near-ultraviolet chip with blue, green and red phosphors, and the electroluminescence spectrum is shown in the figure below. Figure 8 Said by Figure 8 It can be seen that there is a continuous spectrum between 400 and 750 nm, which fills the cyan gap of 470 to 510 nm to a certain extent and realizes full-spectrum lighting.
[0102] (2) It can be seen from Example 1 and Comparative Example 1 that if Ce ions are replaced by Bi ions in the present invention, no light will be emitted.
[0103] In summary, the present invention dopes Ce element into A2B4O8. 3+ The ions undergo a 4f→5d transition under near-ultraviolet light excitation, emitting blue-cyan light, thereby providing a blue-cyan phosphor for white light LEDs, which fills the deficiency of cyan emission in the spectrum of near-ultraviolet excited white light LED technology in the prior art. In addition, the phosphor provided by the present invention can also be well adapted to LED chips with a wavelength of about 410nm.
[0104] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A fluorescent powder, It is characterized in that The chemical formula of the phosphor is: A 2 B 4 O 8 :xCe 3+ ; where 0 < x ≤ 0.1, A includes alkaline earth metal elements, and B includes rare earth elements.
2. The phosphor according to claim 1, It is characterized in that The alkaline earth metal element includes any one or a combination of at least two of Be, Mg, Ca, Sr, Ba or Ra; Preferably, the rare earth element includes any one of La, Nd, Sm, Gd, Eu, Dy, Ho, Y, Er, Tm, Yb, Sc or Lu, or a combination of at least two thereof.
3. The phosphor according to claim 1 or 2, It is characterized in that The phosphor is of orthorhombic system; Preferably, the space group of the phosphor is Pnma; Preferably, the structure of the phosphor is a spinel structure, wherein A is filled in tetrahedral voids and B is filled in octahedral voids.
4. The phosphor according to any one of claims 1 to 3, It is characterized in that The wavelength at which the phosphor is effectively excited by near-ultraviolet light is 400-420 nm; Preferably, the strongest emission peak of the phosphor is 450-480 nm.
5. A method for preparing the phosphor according to any one of claims 1 to 4, It is characterized in that The preparation method comprises: Mixing raw material A, raw material B and raw material Ce to obtain a mixture; The mixture is sintered to obtain the phosphor.
6. The preparation method according to claim 5, It is characterized in that The A raw material includes any one of A oxide, A hydroxide or A salt, or a combination of at least two thereof; Preferably, the B raw material includes any one of B oxide, B hydroxide or B salt, or a combination of at least two thereof; Preferably, the Ce raw material includes any one of Ce oxide, Ce hydroxide or Ce salt, or a combination of at least two thereof; Preferably, the A salt, B salt or Ce salt independently includes any one of carbonate, halide salt, sulfate, chlorate, acetate or nitrate, or a combination of at least two thereof.
7. The preparation method according to claim 5 or 6, It is characterized in that The mixing method includes grinding; Preferably, the sintering temperature is 1200-1600°C; Preferably, the sintering time is 1 to 10 hours; Preferably, the sintering atmosphere comprises a reducing atmosphere; Preferably, the reducing atmosphere comprises a reducing gas; Preferably, the reducing gas comprises a mixed gas of nitrogen and hydrogen; Preferably, the reducing gas comprises carbon monoxide gas; Preferably, the sintering process further includes grinding the sintered product.
8. An LED light-emitting device, It is characterized in that The LED light-emitting device comprises a light-emitting device and a phosphor composition located in the light-emitting device, wherein the phosphor composition comprises the phosphor according to any one of claims 1 to 4.
9. The LED lighting device according to claim 8, It is characterized in that Among the light-emitting devices, at least one light-emitting device is capable of emitting light in the near-ultraviolet wavelength region; Preferably, the phosphor composition further comprises any one or a combination of at least two of a blue phosphor, a green phosphor, a yellow phosphor or a red phosphor that can be effectively excited by near-ultraviolet light; Preferably, the central emission wavelength of the blue phosphor is 440-470 nm; Preferably, the central emission wavelength of the green phosphor is 500-540 nm; Preferably, the central emission wavelength of the yellow phosphor is 550-590 nm; Preferably, the central emission wavelength of the red phosphor is 620-650 nm.
10. The LED lighting device according to claim 8 or 9, It is characterized in that The LED light emitting device has a correlated color temperature of 2500-7000K and has an uninterrupted continuous spectrum within a wavelength range of 400-750nm.
Citation Information
Patent Citations
Blue luminescent phosphor suitable for near ultraviolet excitation and preparation method and application thereof
CN107541211A
Fluophor and light emitting device using the same
JP2016176017A
Phosphor emitting green light, method for manufacturing the same and light emitting device package using the same
KR1020170054804A
Cited By
Broadband yellow fluorescent material excited by blue light as well as preparation method and application thereof
CN120158301A
Purple light excited cyan light emitting fluorescent material as well as preparation method and application thereof
CN120966478A