A conductive-electricity storage microbial composite material, preparation method and method for strengthening anaerobic fermentation

By modifying the conductive-electric storage materials that combine biochar with electron mediators by metal oxides, the problem of hydrogen accumulation in anaerobic digestion inhibits methane production and improves methane production and microbial metabolic efficiency.

CN118726338BActive Publication Date: 2024-11-19INSTITUTE OF ENVIRONMENT AND SUSTAINABLE DEVELOPMENT IN AGRICULTURE CAAS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411230217.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-19
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

During the anaerobic digestion, large amounts of hydrogen and electrons are generated due to rapid oxidation of the substrate, which leads to the accumulation of hydrogen, inhibits the activity of methane-producing microorganisms, and reduces methane production. The electron transfer capacity of existing conductive materials such as biochar is limited and the excessive electrons cannot be effectively utilized.

Method used

The biochar modified with metal oxide is combined with an electron mediator to form a conductive-electric storage material. The microbial composite material is prepared through covalent binding and copolymerization to improve conductivity and store and release excessive electrons, promote hydrogen transfer between microorganisms, and enhance Anaerobic fermentation efficiency.

Benefits of technology

It significantly improves methane production, and by improving the conductivity and capacitance capacity of conductive-electric storage materials, it alleviates hydrogen accumulation problems, maintains metabolic balance, and promotes methane generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726338B_ABST
    Figure CN118726338B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of resource utilization of agricultural waste, and specifically relates to a conductive-electricity storage microbial composite material, a preparation method and a method for strengthening anaerobic fermentation. The present invention provides a conductive-electricity storage microbial composite material, the microbial composite material includes a conductive-electricity storage material and microorganisms colonized in the conductive-electricity storage material; the microorganisms include acid-producing bacteria and / or methanogenic archaea; the conductive-electricity storage material is formed by combining biochar modified with metal oxides and an electron mediator. Biochar induces the nucleation and growth of metal oxide particles, resulting in the formation of an ultra-thin metal oxide nanostructure with uniform dispersion and controlled morphology on its surface, which has the ability to quickly transmit ions and electrons. The biochar modified with metal oxides can increase the capacitance and electrical adsorption capacity of the composite material, adsorb and transmit electrons, promote interspecies hydrogen transfer between the symbiotic bacterial communities of acid-producing bacteria and methanogenic archaea in anaerobic fermentation, and increase the methane production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of agricultural waste resource utilization, and specifically relates to a conductive-electricity storage microbial composite material, a preparation method and a method for strengthening anaerobic fermentation. Background Art

[0002] Anaerobic digestion technology has been widely used to treat agricultural organic waste, but the anaerobic digestion process is accompanied by the coordinated metabolism of multiple bacterial species, the orderly transfer of multiple substances, and the transformation of multiple energy forms, making it a complex process. In the anaerobic digestion process, there is a problem of accumulation of intermediate metabolites and inhibition of microbial activity due to the imbalance between substrate nutrients and microbial metabolism. Therefore, the metabolic balance between acid-producing bacteria and methanogenic archaea is crucial to the stable operation of the anaerobic digestion process.

[0003] Studies have shown that interspecies electron transfer between symbiotic bacterial communities is a key factor affecting the efficiency and stability of anaerobic digestion. In the process of microbial cooperative fermentation, improving interspecies electron transfer of microorganisms can significantly improve the metabolic efficiency of microorganisms, thereby accelerating the degradation of substrates and increasing methane production. In the process of interspecies electron transfer, interspecies hydrogen transfer is a common way for microorganisms to transfer electrons. However, the rapid oxidation of substrates produces a large amount of hydrogen and electrons, and methanogenic archaea are usually unable to consume excess hydrogen and electrons in time, resulting in hydrogen accumulation in the system. Due to the slow diffusion rate of hydrogen and electrons in the anaerobic digestion system, the synergistic effect between acidogenic bacteria and methanogenic archaea is limited. When the hydrogen partial pressure in the system is too high, it will lead to the accumulation of volatile fatty acids, resulting in a further decrease in the activity of methanogenic microorganisms, and the methanogenic process of methanogenic archaea is inhibited, reducing the methane production.

[0004] Adding conductive materials to increase the electron transfer rate has become a research hotspot in this field. Biochar has reversible redox-active functional groups, which form electron transfer pathways in a series of redox reactions and mediate electron transfer between microbial species by accepting / releasing electrons. The redox-active functional groups on the surface of biochar are key factors affecting the conductive properties of biochar. However, due to the different raw materials and pyrolysis processes of biochar, the content of redox-active functional groups on the surface of biochar usually cannot reach a certain abundance. Therefore, the electron transfer capacity of biochar is limited. In addition, a large amount of electrons and hydrogen produced by the hydrolysis and acidification of organic matter are still in the anaerobic system and are not used in time, which also reduces the methane production to a certain extent. Summary of the invention

[0005] In view of this, the present invention provides a conductive-electricity storage microbial composite material, a preparation method and a method for strengthening anaerobic fermentation. The conductive-electricity storage material in the microbial composite material has strong conductivity, stores and releases excess electrons during the co-production of methane, improves the conductivity of the microbial composite material, and ultimately increases methane production.

[0006] In order to solve the above problems, the present invention provides the following technical solutions:

[0007] The present invention provides a conductive-electricity storage microbial composite material, comprising a conductive-electricity storage material and microorganisms colonized in the conductive-electricity storage material; the microorganisms include acid-producing bacteria and / or methanogenic archaea; the conductive-electricity storage material is formed by combining biochar modified with metal oxides and an electron mediator.

[0008] Preferably, the bonding method includes covalent bonding and / or copolymerization.

[0009] Preferably, the electron mediator includes one or more of an endogenous electron mediator, an exogenous electron mediator of a humus mixture and an exogenous quinone-containing mediator, wherein the endogenous electron mediator includes riboflavin and / or flavin; the exogenous quinone-containing mediator includes one or more of benzoquinone, naphthoquinone, phenanthrenequinone and anthraquinone.

[0010] The present invention provides a method for preparing the microbial composite material described in the above technical solution, comprising the following steps:

[0011] The metal acetate and biochar are first mixed and hydrothermally modified to obtain biochar modified with metal oxides;

[0012] When the electron mediator is an endogenous electron mediator and / or an exogenous electron mediator of a humus mixture,

[0013] Dispersing the metal oxide-modified biochar, acrylamide and electron mediator to obtain a dispersion;

[0014] The dispersion is mixed with a cross-linking agent, an initiator and an accelerator for a second time to perform a hydrothermal reaction to obtain a hydrothermal product;

[0015] The hydrothermal product is dried and then subjected to a freezing and thawing cycle operation to obtain a conductive-electricity storage material;

[0016] The conductive-electricity storage material and the microorganism are mixed for the fourth time to obtain a conductive-electricity storage microbial composite material;

[0017] Alternatively, when the electron mediator is an exogenous quinone-containing mediator,

[0018] performing a third mixing of the metal oxide-modified biochar and the electron mediator to obtain a mixture;

[0019] The mixture is subjected to a freezing and thawing cycle operation to obtain a conductive-electricity storage material;

[0020] The conductive-electricity storage material and the microorganism are mixed for the fourth time to obtain a conductive-electricity storage microbial composite material.

[0021] Preferably, the metal acetate includes one or more of zinc acetate, magnesium acetate and ferric acetate;

[0022] The mass ratio of the metal oxide-modified biochar to acrylamide is 1:1-10;

[0023] The mass ratio of the biochar to the acetate metal salt is 10-20:1;

[0024] The first mixing method includes ultrasound, the power of the ultrasound is 480W, the temperature of the ultrasound is 60-90°C, and the time of the ultrasound is 0.5h;

[0025] The temperature of the hydrothermal modification is 110-150° C., and the time of the hydrothermal modification is 6-12 hours.

[0026] Preferably, the mass ratio of the acrylamide to the cross-linking agent is 1-10:0.1-1; the cross-linking agent comprises N,N-methylenebisacrylamide;

[0027] The mass ratio of acrylamide to initiator is 1-10:0.01-0.1; the initiator comprises persulfate;

[0028] The accelerator includes N,N,N′,N′-tetramethylethylenediamine;

[0029] The temperature of the hydrothermal reaction is 80-100° C.; the time of the hydrothermal reaction is 3-6 hours.

[0030] Preferably, the drying includes a first drying, the temperature of the first drying is 60° C., and the time of the first drying is 6 to 12 hours.

[0031] Preferably, after the freezing and thawing cycle operation, a second drying is further performed, wherein the temperature of the second drying is -80 to -50°C; the time of the second drying is 12 to 36 hours, and the vacuum degree of the second drying is 0.05 to 0.1 mBar.

[0032] Preferably, after the mixture is subjected to a freeze and thaw cycle operation, a third drying process is further performed, wherein the temperature of the third drying process is -80 to -50°C; the time of the third drying process is 12 to 36 hours, and the vacuum degree of the third drying process is 0.05 to 0.1 mBar.

[0033] The present invention provides a method for strengthening anaerobic fermentation using a composite material, comprising:

[0034] The microbial composite material described in the above technical solution or the microbial composite material prepared by the preparation method described in the above technical solution is added to an anaerobic fermentation reactor to promote anaerobic fermentation.

[0035] Beneficial effects of the present invention: The present invention provides a conductive-electricity storage microbial composite material, comprising a conductive-electricity storage material and microorganisms colonized in the conductive-electricity storage material; the microorganisms include acid-producing bacteria and / or methanogenic archaea; the conductive-electricity storage material is formed by combining biochar modified with metal oxides and an electron mediator.

[0036] Biochar is usually used as an auxiliary material to induce the nucleation and growth of metal oxide particles, resulting in the formation of ultra-thin metal oxide nanostructures with uniform dispersion and controlled morphology on the surface of biochar. The resulting nanostructures exhibit excellent ion storage capacity, and the ability of the conductive-storage material to quickly transport ions and electrons is also improved through the nanostructure conductive network. Biochar modified with metal oxides can also increase the surface area and Faraday capacitance of the metal oxide, as well as the double-layer capacitance of the biochar material, thereby increasing the capacitance and electrical adsorption capacity of the conductive-storage material, and ultimately increasing the conductivity and capacitance of the conductive-storage material, and absorbing more electrons generated by the transition from the hydrolysis acidification stage to the methanogenesis stage in the anaerobic digestion system.

[0037] Conductive-energy storage materials have strong conductive properties and can conduct electrons. The biochar modified with metal oxides in the conductive-energy storage materials stores excess electrons. When the anaerobic digestion system switches from the hydrolysis and acidification stage to the methanogenesis stage, the biochar modified with metal oxides slowly transfers electrons to microorganisms, promoting interspecies hydrogen transfer between acidogenic bacteria and methanogenic archaea in anaerobic fermentation, accelerating the rate of electron transfer, and effectively alleviating the accumulation of intermediate metabolites caused by rapid hydrolysis and acidification of substrates, thereby improving the metabolic level of microorganisms, maintaining metabolic balance, and thereby increasing methane production.

[0038] Compared with biochar, the microbial composite material of the present invention has an increased specific surface area. A larger specific surface area means more pores and more functional groups exposed on the outside. The increased specific surface area also provides more active sites for ion storage, which can increase the electron storage capacity of the microbial composite material.

[0039] In summary, the microbial composite material provided by the present invention can promote the efficient synthesis of methane and increase methane production. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the embodiments are briefly introduced below.

[0041] Figure 1 Fourier transform infrared spectra (FTIR) of the modified biochar and the original biochar prepared in Example 2;

[0042] Figure 2 This is a graph showing daily methane production when the microbial composite material prepared in Example 2 is used for mesophilic anaerobic digestion;

[0043] Figure 3 This is a graph showing the cumulative methane production of the microbial composite material prepared in Example 2 when used for mesophilic anaerobic digestion. DETAILED DESCRIPTION

[0044] The present invention provides a microbial composite material, comprising a conductive-electricity storage material and microorganisms colonized in the conductive-electricity storage material; the microorganisms include acid-producing bacteria and / or methanogenic archaea; the conductive-electricity storage material is formed by combining biochar modified with metal oxides and an electron mediator.

[0045] In the present invention, the bonding method preferably includes covalent bonding and / or copolymerization; the copolymerization method preferably includes graft copolymerization; as an optional embodiment, the grafting is preferably cross-linking grafting.

[0046] In the present invention, the electron mediator preferably includes one or more of an endogenous electron mediator, an exogenous electron mediator of a humus mixture, and an exogenous quinone-containing mediator. The endogenous electron mediator of the present invention preferably includes riboflavin and / or flavin, and more preferably riboflavin or flavin. In the present invention, the riboflavin or flavin is mixed with water to obtain an endogenous electron mediator solution, and the molar concentration of flavin in the endogenous electron mediator solution is preferably 1-5 mmol / L; more preferably 4 mmol / L. The molar concentration of riboflavin in the endogenous electron mediator solution of the present invention is preferably 1-5 mmol / L, and more preferably 4 mmol / L. The exogenous quinone-containing mediator of the present invention preferably includes one or more of benzoquinone, naphthoquinone, phenanthrenequinone and anthraquinone.

[0047] In the present invention, the preparation method of the humus mixture exogenous electron mediator preferably includes: mixing humic acid and acetone solution, shaking in a water bath and centrifuging to obtain a supernatant. The supernatant of the present invention is the humus mixture exogenous electron mediator. The mass volume ratio of humic acid and acetone solution of the present invention is preferably 1~5g:50~100mL, more preferably 3~5g:80~100mL, more preferably 5g:100mL; the molar concentration of the acetone solution is preferably 0.5~2mol / L; the temperature of the water bath shaking is preferably 60~90℃, the rotation speed of the shaking is preferably 120~180r / min, and the shaking time is preferably 12~24h; the centrifugal time is preferably 15~25min, and the centrifugal speed is preferably 8000~12000r / min.

[0048] The endogenous electron mediator, the humus mixture exogenous electron mediator and the exogenous quinone-containing mediator described in the present invention can all accept electrons and provide electrons. Compared with the electron mediators in the prior art that can only provide electrons, the electron mediator of the present invention can conduct electrons through redox active functional groups and store electrons when there are more functional groups containing carbon-oxygen double bonds.

[0049] In the present invention, the microorganisms include acidogenic bacteria and / or methanogenic archaea, and the acidogenic bacteria preferably include acetogenic proteinophilic bacteria ( Proteiniphilum ) and / or Ruminofilibacter, More preferably, it is acetogenic proteinophilic bacteria ( Proteiniphilum The methanogenic archaea preferably include Methanobacterium ( Methanobacterium The acetogenic proteophilic bacteria convert sugars, starch and other substances in the fermentation raw materials into a large amount of organic acids and carbon dioxide, and the methanogenic archaea generate methane by utilizing metabolites such as hydrogen, acetic acid, carbon dioxide and the like.

[0050] The present invention provides a method for preparing the conductive-electricity storage microbial composite material described in the above technical solution, comprising the following steps:

[0051] The metal acetate and biochar are first mixed and hydrothermally modified to obtain biochar modified with metal oxides;

[0052] When the electron mediator is an endogenous electron mediator and / or an exogenous electron mediator of a humus mixture,

[0053] Dispersing the metal oxide-modified biochar, acrylamide and electron mediator to obtain a dispersion;

[0054] The dispersion is secondly mixed with a cross-linking agent, an initiator and an accelerator to undergo a hydrothermal reaction to obtain a hydrothermal product;

[0055] The hydrothermal product is dried and then subjected to a freezing and thawing cycle operation to obtain a conductive-electricity storage material;

[0056] The conductive-electricity storage material and the microorganism are mixed for the fourth time to obtain a conductive-electricity storage microbial composite material;

[0057] Alternatively, when the electron mediator is an exogenous quinone-containing mediator,

[0058] Stirring the metal oxide-modified biochar and the electron mediator to obtain a mixture;

[0059] The mixture is subjected to a freezing and thawing cycle operation to obtain a conductive-electricity storage material;

[0060] The conductive-electricity storage material and the microorganism are mixed for the fourth time to obtain a conductive-electricity storage microbial composite material.

[0061] In the present invention, the metal acetate preferably includes one or more of zinc acetate, magnesium acetate and iron acetate, and more preferably zinc acetate. The metal acetate serves to improve the electrical conductivity of biochar.

[0062] In the present invention, the biochar is preferably prepared by pyrolysis of lignocellulosic waste; the pyrolysis temperature is preferably 550-850°C, more preferably 650-750°C; the pyrolysis time is preferably maintained for 2 hours after reaching the pyrolysis temperature to obtain the biochar.

[0063] The present invention preferably first mixes the biochar and the acetate metal salt, and performs hydrothermal modification to obtain biochar modified with metal oxides. Before the first mixing, the biochar is preferably dispersed, washed, dried and ball-milled to obtain ball-milled biochar. The solvent used for the dispersion preferably includes alcohol, and the mass volume ratio of the biochar and the alcohol is preferably 1-5 g: 25-100 mL; the dispersion is preferably completed by stirring; the stirring time is preferably 3-6 h, and more preferably 3.5 h. The washing is preferably completed by deionized water filtration and washing; the number of deionized water filtration and washing is preferably 2-3 times. The drying temperature is preferably 60°C; the mass ratio of the material in the ball mill to the grinding body of the ball mill is preferably (50-150): 1, and more preferably 100: 1. The rotation speed of the ball mill is preferably 495 r / min; the ball milling time is preferably 12-24 h, and more preferably 12 h.

[0064] To obtain ball-milled biochar, the present invention preferably mixes the ball-milled biochar with deionized water for a first ultrasound, and then mixes it with a metal acetate for a first time, and performs hydrothermal modification to obtain metal oxide-modified biochar. The mass volume ratio of the ball-milled biochar and deionized water is preferably 5g:100mL; the first ultrasound is preferably performed under the condition of first stirring, and the time of the first ultrasound is preferably 0.5~1h, more preferably 0.5h; the speed of the first stirring is preferably 120r / min; the first ultrasound result is preferably first mixed with a metal acetate, and the mass ratio of the biochar to the metal acetate is preferably 10~20:1, more preferably 10:1; the first mixing method preferably includes a second ultrasound, and the second ultrasound is preferably completed under the condition of a second stirring, the time of the second ultrasound is preferably 0.5h, the power of the second ultrasound is preferably 480W, and the temperature of the second ultrasound is preferably 60~90°C, more preferably 90°C; the first mixed result is preferably hydrothermally modified in a high-pressure hydrothermal reactor. The temperature of the hydrothermal modification is preferably 110-150°C, and the time of the hydrothermal modification is preferably 6-12 hours; the hydrothermal modification product is preferably washed and then dried to obtain biochar modified with metal oxides. The washing is preferably completed with deionized water, and the number of washings is preferably 2-3 times. The drying temperature is preferably 60°C, and the drying time is preferably

[0065] The time period is selected to be 6 to 12 hours; after drying, the metal oxide-modified biochar is obtained, and the metal oxide-modified biochar has higher pseudocapacitive properties.

[0066] The metal oxide modified biochar is obtained. When the electron mediator is an endogenous electron mediator and / or an exogenous electron mediator of a humus mixture, the present invention disperses the metal oxide modified biochar, acrylamide and electron mediator to obtain a dispersion. The mass ratio of the metal oxide modified biochar and acrylamide is preferably 1:1 to 10, more preferably 1:1 to 5, and more preferably 1:2. The endogenous electron mediator of the present invention is mixed with water and prepared into a solution for use; the present invention has no special limitation on the mass volume ratio of the endogenous electron mediator solution, the metal oxide modified biochar, and the acrylamide dispersion, as long as the endogenous electron mediator in the endogenous electron mediator solution meets the above-mentioned molar concentration.

[0067] The volume mass ratio of the humus mixture exogenous electron mediator, metal oxide modified biochar and acrylamide dispersion of the present invention is preferably 50mL:1g:2g. The dispersion method is preferably ultrasonic dispersion; the ultrasonic dispersion time is preferably 20min; after ultrasonic dispersion, the dispersion liquid is preferably purged with nitrogen; the nitrogen purge time is preferably 15min.

[0068] A dispersion is obtained, and the present invention mixes the dispersion with a crosslinker, an initiator, and an accelerator for a second time, performs a hydrothermal reaction, and obtains a hydrothermal product; more preferably, the dispersion is stirred with a crosslinker to obtain a stirrer; the stirrer is stirred with an initiator for a third time to obtain a third stirrer; the third stirrer is hydrothermally reacted with an accelerator to obtain a hydrothermal product. The mass ratio of acrylamide and a crosslinker in the present invention is preferably (1-10): (0.1-1), further preferably (1-5): (0.1-0.5), and more preferably 4:0.5; the crosslinker preferably includes N,N-methylenebisacrylamide, and when the monomer acrylamide is polymerized to a certain extent, N,N-methylenebisacrylamide and acrylamide polymer are crosslinked to obtain an insoluble crosslinked polymer; the stirring time is preferably 10-20 minutes, and the stirring method is preferably slow stirring; the speed of the slow stirring is preferably 60-90r / min.

[0069] A stirrer is obtained, and the present invention performs a third stirring of the stirrer and the initiator to obtain a third stirrer; the mass ratio of acrylamide to initiator is preferably (1-10): (0.01-0.1), further preferably (1-5): (0.05-0.1), and more preferably 4:0.1; the time of the third stirring is preferably 5-10 minutes, and the temperature of the third stirring is preferably 50-80°C. The initiator of the present invention preferably includes persulfate, which can be used to initiate free radical polymerization and copolymerization of olefin and diene monomers, and can also be used for cross-linking and curing of unsaturated polyesters and polymer cross-linking reactions. The persulfate preferably includes one or more of potassium persulfate, sodium persulfate and ammonium persulfate, and more preferably ammonium persulfate.

[0070] A third agitator is obtained. The present invention performs a hydrothermal reaction on the third agitator and a promoter to obtain a hydrothermal product. More preferably, the third agitator and a promoter are mixed to obtain a mixed solution, and the mixed solution is subjected to a hydrothermal reaction to obtain a hydrothermal product. The promoter preferably includes N,N,N′,N′-tetramethylethylenediamine. The volume ratio of the third agitator to the promoter is preferably (1-2): (0.01-0.02), and more preferably 1:0.01. The temperature of the hydrothermal reaction is preferably 80-100° C., and more preferably 90° C.; the time is preferably 3-6 hours, and more preferably 4-5 hours.

[0071] The hydrothermal product is dried and then subjected to a freezing and thawing cycle to obtain a conductive-electricity storage material; washing is preferably performed before drying, and the washing is preferably performed using deionized water, and the number of washings is preferably 2 to 3 times; the drying preferably includes a first drying and a second drying, the temperature of the first drying is preferably 60°C, the drying time is preferably 6 to 12 hours, more preferably 8 to 12 hours, and more preferably 12 hours; the number of freezing and thawing cycles is preferably 5 to 10 times, more preferably 8 to 10 times, and more preferably 10 times; the freezing temperature is preferably -24°C, and the freezing time is preferably 12 hours; the thawing temperature is preferably room temperature temperature, and the thawing time is preferably 5h; the present invention preferably subjects the product obtained by the freezing and thawing cycle operation to a second drying to obtain a conductive-electricity storage material; the second drying method preferably includes vacuum freeze drying; the vacuum freeze drying temperature is preferably -80~-50°C, further preferably -65~-50°C, and more preferably -50°C; the vacuum degree of the vacuum freeze drying is preferably 0.05~0.1mBar, further preferably 0.05~0.07mBar, and more preferably 0.05mBar; the vacuum freeze drying time is preferably 12~36h, further preferably 12~24h, and more preferably 12h; the conductive-electricity storage material is obtained after vacuum freeze drying.

[0072] The present invention performs a fourth mixing of the conductive-electricity storage material and the microorganism to obtain a conductive-electricity storage microbial composite material; the microorganism comprises acid-producing bacteria and / or methanogenic archaea, and the acid-producing bacteria preferably comprises acetogenic proteinophilic bacteria ( Proteiniphilum ) and / or Ruminofilibacter, More preferably, it is acetogenic proteinophilic bacteria ( Proteiniphilum ) 。 The methanogenic archaea preferably include Methanobacterium ( Methanobacterium The acetogenic proteophilic bacteria convert sugars, starch and other substances in the fermentation raw materials into a large amount of organic acids and carbon dioxide, and the methanogenic archaea generate methane by utilizing metabolites such as hydrogen, acetic acid, carbon dioxide and the like.

[0073] The present invention preferably cultured the acid-producing bacteria in a liquid culture medium to obtain an acid-producing bacteria liquid; the viable count of the acid-producing bacteria liquid is preferably ≥100 CFU / mL; the present invention preferably cultured the methanogenic archaea in a liquid culture medium to obtain a methanogenic archaea liquid; the viable count of the methanogenic archaea liquid is preferably ≥100 CFU / mL. The present invention preferably mixes the acid-producing bacteria liquid and the methanogenic archaea liquid in a mass ratio of 1:1 to 1.25 to obtain a strain suspension, more preferably 1:1.

[0074] A bacterial suspension is obtained. The present invention preferably mixes the bacterial suspension, the conductive-electricity storage material and the growth factor solution and then adsorbs to obtain an adsorption liquid. The volume mass ratio of the bacterial suspension and the conductive-electricity storage material in the present invention is preferably 10~50mL:1g; the adsorption temperature is preferably 30~35℃, the adsorption speed is preferably 80~120 r / min, and the adsorption time is preferably 6~12h; the number of viable bacteria in the adsorption liquid is preferably ≥100CFU / mL, more preferably 1000CFU / mL; the growth factor solution preferably includes a glucose solution; the glucose solution is preferably a commercially available glucose solution; the addition amount of the growth factor solution is preferably 0.5~2mL per milliliter of bacterial suspension; the function of the growth factor solution is to promote the growth and reproduction of acid-producing bacteria and methanogenic archaea.

[0075] The present invention preferably centrifuges the adsorption liquid to obtain a precipitate; and rinses the precipitate with physiological saline to obtain a microbial composite material. The centrifugal speed is preferably 500-800 r / min, more preferably 600-700 r / min, and more preferably 650 r / min; the centrifugal time is preferably 10-30 min, more preferably 15-25 min, and more preferably 20 min. The mass concentration of the physiological saline is preferably 0.9% by mass for the final rinse.

[0076] When the electron mediator is an exogenous quinone-containing mediator, the present invention performs a third mixing of the metal oxide-modified biochar and the electron mediator to obtain a mixture, more preferably, performs a third mixing of the metal oxide-modified biochar and the solution containing the electron mediator to obtain a mixture; the mass volume ratio of the biochar and the solution containing the electron mediator is preferably 1-5 g:50-100 mL, more preferably 1 g:50 mL; the molar concentration of quinone in the solution containing the electron mediator is preferably 0.5-2 mmol / L, more preferably 1 mmol / L; the third mixing method is preferably stirring, the stirring speed is preferably 120 r / min, and the stirring time is preferably 6-12 h, more preferably 10-12 h; after the stirring, the obtained product is preferably subjected to water bath shaking culture to obtain a mixture; the temperature of the water bath is preferably 60-90°C, more preferably 60-70°C, the shaking speed is preferably 120-150 r / min, more preferably 120-130 r / min; the culture time is preferably 24-36 h, more preferably 24-28 h.

[0077] A mixture is obtained, and the present invention subjects the mixture to a freeze and thaw cycle operation to obtain a conductive-electricity storage material. The number of freeze and thaw cycles is preferably 5 to 10 times, and more preferably 5 to 7 times; the freezing temperature is preferably -24°C, and the freezing time is preferably 12 hours; the thawing temperature is preferably room temperature, and the thawing time is preferably 5 hours; after the freeze and thaw cycle operation, the present invention preferably subjects the obtained product to a third drying; the third drying method preferably includes freeze drying; the freeze drying method preferably includes vacuum freeze drying; the vacuum freeze drying temperature is preferably -80 to -50°C, and more preferably -60 to -50°C; the vacuum degree of the vacuum freeze drying is preferably 0.05 to 0.1 mBar, and more preferably 0.06 to 0.07 mBar; the vacuum freeze drying time is preferably 12 to 36 hours, and more preferably 12 to 18 hours; after vacuum freeze drying, a conductive-electricity storage material is obtained.

[0078] The present invention performs a fourth mixing of the conductive-electricity storage material and the microorganism to obtain a conductive-electricity storage microbial composite material; the technical features of the microorganism and the fourth mixing have been described above and will not be repeated here.

[0079] The present invention provides a method for strengthening anaerobic fermentation using the microbial composite material described in the above technical solution, comprising:

[0080] The microbial composite material is added into an anaerobic fermentation reactor to promote anaerobic fermentation.

[0081] In the present invention, the anaerobic fermentation is preferably continuous anaerobic digestion. Before the continuous anaerobic digestion described in the present invention is carried out, the inoculum is preferably subjected to anaerobically digestion. The anaerobic digestion of the inoculum preferably includes: placing the inoculum in a fermentation tank for anaerobic digestion. The inoculum described in the present invention preferably includes anaerobic sludge, and the amount of the inoculum added is preferably 75% to 85% of the total volume of the fermentation tank, and more preferably 80%. The anaerobic sludge is preferably taken from an anaerobic fermentation tank, and the anaerobic sludge preferably includes bacteria and methanogenic archaea; the bacteria preferably include Prevotella ( Prevotella )、Bacteroides( Bacteroides ), acetogenic proteinophilic bacteria ( Proteiniphilum ) or more than one of the following; the methanogenic archaea preferably include the archaeon Methanobacterium ( Methanobacterium ) and / or Methanobacterium ( Methanosaeta ). In the embodiment of the present invention, the anaerobic sludge is taken from the anaerobic fermentation tank of the laboratory of the Institute of Agricultural Environment and Sustainable Development of the Chinese Academy of Agricultural Sciences. The temperature of the anaerobic digestion of the inoculum of the present invention is preferably 35-38°C, and the method of anaerobic digestion of the inoculum is preferably water bath constant temperature fermentation. The anaerobic digestion of the inoculum of the present invention is carried out until the inoculum no longer produces gas.

[0082] After the inoculum no longer produces gas, the present invention preferably adds fermentation raw materials, composite materials and water to the inoculum for continuous anaerobic digestion.

[0083] The continuous anaerobic digestion of the present invention preferably adds fermentation material and discharges daily; the composition of the added fermentation material preferably includes fermentation raw materials, microbial composite materials and water. The fermentation raw materials of the present invention preferably include one or more of straw, livestock and poultry manure, and kitchen waste. In an embodiment of the present invention, the fermentation raw material is preferably corn stalks, which are single lignocellulose fermentation raw materials. The microbial composite material of the present invention is preferably crushed before adding, and the diameter of the composite material particles after crushing is preferably 1~2mm; the addition amount of the microbial composite material is preferably 3%~12% of the mass of the fermentation raw material, and more preferably 5%.

[0084] The continuous anaerobic digestion of the present invention preferably calculates the amount of fermentation material added and the amount of discharge per day based on the organic load and hydraulic retention time, and the amount of fermentation material added and the amount of discharge are preferably the same. The hydraulic retention time (HRT) of the continuous anaerobic digestion of the present invention is preferably 20-30 days, more preferably 20 days, and the organic load (OLR) of the continuous anaerobic digestion is preferably 1-2.5 g / d / L, more preferably 1 g / d / L; in an embodiment of the present invention, the daily feed and discharge amounts are both 0.12 L. The temperature of the continuous anaerobic digestion of the present invention is preferably 35-38°C, and the method of the continuous anaerobic digestion is preferably water bath constant temperature fermentation.

[0085] The present invention prepares high pseudocapacitive carbon materials by modifying biochar with metal oxides, and simultaneously couples redox electron mediators to prepare a composite material of conductive-electricity storage microorganisms (i.e., a "binary" conductive / electricity storage composite material). On the basis of the conductive-electricity storage material (composite precursor, i.e., monomer self-polymerization), the redox electron mediator is grafted on the side chain to make the polymer skeleton of the composite precursor have strong conductive properties, and a mutually penetrating interpenetrating conductive network is formed through a co-hydrothermal synthesis method, thereby significantly improving the conductivity of the composite material.

[0086] The microbial composite material prepared by the present invention conducts electrons through side chain redox, and the high pseudocapacitive biochar stores the electron surplus. When the anaerobic digestion system turns from the hydrolysis and acidification stage to the methanogenesis stage, the electrons are slowly transmitted to the microorganisms. The composite material effectively alleviates the accumulation of intermediate metabolites caused by rapid hydrolysis and acidification of the substrate, improves the metabolic level of the microorganisms, and maintains metabolic balance. The composite material prepared by the present invention can be used in the anaerobic digestion process to increase the methane production.

[0087] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0088] In the following embodiments and application examples, the inoculum is anaerobic sludge taken from an anaerobic fermentation tank in the laboratory of the Institute of Agricultural Environment and Sustainable Development of the Chinese Academy of Agricultural Sciences.

[0089] Example 1

[0090] 1. Using corn stalks as raw materials, corn stalks, inoculants and water were mixed to obtain a fermentation system for medium-temperature anaerobic digestion, and the total solid content of the fermentation system was 8%. The container for anaerobic digestion was a 500mL serum bottle, the effective volume of the serum bottle was 400mL, and the inoculant ratio was 30% (v / v) of the effective volume of the serum bottle. The inoculant was anaerobic sludge.

[0091] During the mesophilic anaerobic digestion process, the fermentation liquid was sampled and frozen every day. After the experiment was over, the overall gas production was observed to determine the peak period of gas production. 4g of frozen samples collected during the peak period of gas production were taken for metagenomic sequencing, and the screening strains were determined based on species abundance. Based on functional gene prediction, acetic acid-producing protein-loving bacteria ( Proteiniphilum )、 Ruminofilibacter and the archaea Methanobacterium genus that is beneficial for methanogenesis under this system ( Methanobacterium ).

[0092] 2. Corn stalks were used as raw materials, inoculants and water were added to obtain a fermentation system; the total solid content in the fermentation system was 10%, and the inoculant was anaerobic sludge. The container for anaerobic digestion was a 500 mL serum bottle, the effective volume of the serum bottle was 400 mL, and the inoculant ratio was 40% (v / v) of the effective volume.

[0093] During the mesophilic anaerobic digestion process, the fermentation liquid was sampled and frozen every day. After the experiment was over, the overall gas production was observed to determine the peak gas production period. 4 g of samples that had been sampled and frozen during the peak gas production period were taken for metagenomic sequencing.

[0094] The strains were screened according to species abundance, and acetic acid-producing protein-loving bacteria that were beneficial for lignin degradation were selected ( Proteiniphilum ), which is conducive to the methanogenic archaea Methanobacterium genus ( Methanobacterium ) growth.

[0095] 3. Cow dung was used as raw material, inoculum and water were added to obtain a fermentation system; the total solid content in the fermentation system was 10%, and the inoculum was anaerobic sludge. The container for anaerobic digestion was a 500mL serum bottle, the effective volume of the serum bottle was 400mL, and the inoculum ratio was 40% (v / v) of the effective volume.

[0096] During the mesophilic anaerobic digestion process, samples were collected and frozen every day. After the experiment was over, the overall gas production was observed to determine the peak period of gas production. 4 g of samples that had been collected and frozen during the peak period of gas production were taken for metagenomic sequencing, and the selected strains were determined based on species abundance.

[0097] Based on the prediction of functional genes, acetogenic proteinophilic bacteria that are beneficial to lignin degradation were screened out ( Proteiniphilum )、 Ruminofilibacter and the archaea Methanobacterium genus that is beneficial for methanogenesis under this system ( Methanobacterium ).

[0098] 4. According to the above three experiments, the most abundant bacteria in the corn straw fermentation process are acetogenic proteinophilic bacteria ( Proteiniphilum ), the archaea belong to the genus Methanobacterium ( Methanobacterium ). It can be seen that acetic acid protein-loving bacteria and Methanobacterium can promote anaerobic fermentation. Therefore, these two strains were used to prepare microbial composite materials.

[0099] In order to achieve pure culture of acetic acid proteinophilic bacteria and Methanobacterium, acetic acid proteinophilic bacteria ( Proteiniphilum ) were purchased from China General Microbiological Culture Collection Center, strain number CGMCC 1.5024; Methanobacterium spp. ( Methanobacterium ) was purchased from China General Microbiological Culture Collection, No. CGMCC 1.5011.

[0100] The acetic acid protein-loving bacteria CGMCC 1.5024 was cultured in a DSM liquid culture medium at 37° C. for 6 hours until the liquid became turbid, thereby obtaining an acetic acid protein-loving bacteria suspension; the viable cell count of the acetic acid protein-loving bacteria suspension was 100 CFU / mL.

[0101] Methanobacterium CGMCC 1.5011 was cultured in DSM liquid culture medium at 37° C. for 6 hours until the liquid became turbid, thereby obtaining a Methanobacterium bacterial suspension; the number of viable bacteria in the Methanobacterium bacterial suspension was 100 CFU / mL.

[0102] The acetic acid protein-loving bacteria suspension and the methanobacterium bacteria suspension were mixed in a mass ratio of 1:1.25 to obtain a bacterial suspension.

[0103] The bacterial suspension was used in the following experiments.

[0104] Example 2

[0105] 1. Preparation of conductive-storage materials (i.e. composite precursors)

[0106] Biochar was prepared using corn cobs as raw materials. The pyrolysis temperature was 550°C. The temperature was raised to 550°C and maintained for 2 hours to obtain biochar. 2 g of biochar was dispersed in alcohol, and then stirred with a magnetic stirrer at 120 r / min for 3.5 hours. After stirring, it was filtered and washed with deionized water for 3 times, and dried in an oven at 60°C to obtain dry biochar, which can also be called raw biochar.

[0107] The dried biochar was ball-milled with a ball-to-powder ratio of 100:1, where the ball-to-powder ratio is the ratio of the mass of the material in the ball mill to the mass of the grinding body. The speed was adjusted to 495 r / min during ball milling, and the time was 24 h.

[0108] The ball-milled biochar was dispersed in 80 mL of deionized water and ultrasonically stirred for 0.5 h at an ultrasonic power of 480 W; 0.2 g of zinc acetate was then added, ultrasonically stirred for 0.5 h at an ultrasonic power of 480 W, and the temperature was set at 60 ° C for preheating. The preheated mixed solution was transferred to a 100 mL high-pressure hydrothermal reactor with a polytetrafluoroethylene liner, and then the reactor was reacted at 120 ° C for 6 h. The obtained product was washed with deionized water and vacuum dried at 60 ° C for 12 h to obtain biochar modified with zinc oxide, which was recorded as zinc oxide-biochar.

[0109] 2 g of zinc oxide-biochar and 4 g of acrylamide were dissolved in a 4 mmol / L riboflavin aqueous solution. The resulting mixture was ultrasonically dispersed for 20 min, and the dispersion was purged with nitrogen for 15 min. Then 0.5 g of N,N-methylenebisacrylamide was added and slowly stirred for 20 min at a speed of 90 r / min. Subsequently, 0.1 g of ammonium persulfate was added, and the whole was placed in a water bath for preheating to 50-80 °C with stirring during the preheating process for 10 min. After the stirring was completed, 25 μL of N,N,N′,N′-tetramethylethylenediamine was added. Afterwards, the obtained mixed solution was transferred to a hydrothermal reactor with a 100mL polytetrafluoroethylene liner, reacted at 90°C for 4h, the obtained product was washed with deionized water and dried at 60°C for 12h, and the dried mixture was poured into a Teflon mold for a total of 10 freeze and thaw cycles, wherein the freezing was at -24°C for 12h and the thawing was at room temperature for 5h; the obtained sample was then placed in a freeze dryer and freeze-dried at -50°C and 0.05mBar vacuum conditions for 12h, and the obtained product (i.e., the composite precursor, also known as conductive-electricity storage material) was stored in a drying oven.

[0110] The pseudocapacitance of the composite precursor was 1.27 F / g by cyclic voltammetry, and the pseudocapacitance of the original biochar was 0.55 F / g; the conductivity of the composite precursor was 13.49 μS / cm by four-probe method, and the conductivity of the original biochar was 6.56 μS / cm. The obtained composite precursor is the modified biochar.

[0111] 2 Preparation of composite materials

[0112] 50 mL of the bacterial suspension prepared in Example 1 and 5 g of the composite precursor were mixed, 25 mL of commercially available glucose solution was added, and the mixture was adsorbed for 6 h at 35 ° C and 120 r / min to ensure that the bacterial density in the obtained bacterial solution was greater than 1000 CFU / mL. The obtained bacterial solution was centrifuged at 500 r / min for 30 min to obtain a precipitate. Finally, the precipitate was washed with 0.9% mass fraction of physiological saline, and the precipitate was the obtained microbial composite material.

[0113] Figure 1 FTIR images of the original biochar in Example 2 and the modified biochar prepared in Example 2 show that the surface functional group distributions of the two materials are basically similar before and after modification, but the oxygen-containing functional groups of the biochar after a series of modifications have obvious fluctuations, CO fluctuations are significantly enhanced, and Zn-O is observed in the modified biochar to show a stronger peak vibration, which is not found in the original biochar, indicating that zinc oxide exists in the modified biochar, which is beneficial to improve the pseudocapacitance of the modified biochar and further improve its conductivity. Figure 1 The horizontal axis is the wave number (cm -1 ).

[0114] Example 3

[0115] 1. Preparation of conductive-storage materials (i.e. composite precursors)

[0116] Biochar was prepared from corn stalks at a pyrolysis temperature of 500°C and maintained at 500°C for 1.5 hours to obtain biochar. 4 g of the prepared biochar was dispersed in alcohol using a magnetic stirrer, which was stirred at 120 r / min for 6 hours. After stirring, it was filtered and washed three times with deionized water, and the obtained product was dried in an oven at 60°C.

[0117] The dried biochar was ball-milled with a ball-to-powder ratio of 150:1; the ball-milling speed was 495r / min and the time was 24h. The ball-milled biochar was dispersed in 80mL deionized water and ultrasonically stirred for 0.5h, and then 0.2g ferric acetate was added and ultrasonically stirred for 0.5h. The ultrasonic power was 480W, and the temperature was set to 60℃ for preheating. The preheated mixed solution was transferred to a 100mL high-pressure hydrothermal reactor with a polytetrafluoroethylene liner. The reactor was reacted at 130℃ for 6h. The obtained product was washed with deionized water and dried at 60℃ for 12h to obtain biochar modified with iron oxide, which was recorded as iron oxide-biochar.

[0118] Dissolve 5 g of humic acid in 100 mL of acetone solution with a molar concentration of 0.5 mol / L. After sufficient stirring, shake the mixture in a 90°C water bath shaker at 180 r / min for 12 h, then centrifuge at 10,000 r / min for 25 min, and perform membrane separation to obtain a supernatant and a precipitate.

[0119] Take 50mL of the supernatant, dissolve 1g of iron oxide-biochar and 2g of acrylamide in the supernatant, disperse the mixture by ultrasonication for 20min, purge the dispersion with nitrogen for 15min, add 0.4g of N,N-methylenebisacrylamide and stir slowly for 20min, then add 0.1g of ammonium persulfate, place the whole in a water bath and preheat to 50℃, stir during heating, stir for 10min, add 20μL of N,N,N′,N′-tetramethylethylenediamine after stirring. Transfer the preheated mixed solution to a 100mL hydrothermal reactor with a polytetrafluoroethylene liner, and react at 90℃ for 4h. The obtained product was washed with deionized water and dried at 60°C for 12 hours, then poured into a Teflon mold and subjected to 10 freeze and thaw cycles, wherein the freezing condition was -24°C for 12 hours and the thawing condition was room temperature for 5 hours. The sample obtained from the freeze and thaw cycle was placed in a freeze dryer and freeze-dried at -50°C and 0.05 mBar vacuum conditions for 12 hours. The obtained product (i.e., composite precursor, conductive-electricity storage material) was stored in a drying oven.

[0120] The pseudocapacitance of the composite precursor was measured by cyclic voltammetry to be 1.23 F / g, and the pseudocapacitance of the original unmodified biochar was measured to be 0.45 F / g; the conductivity of the composite precursor was measured by the four-probe method to be 15.71 μS / cm, and the conductivity of the original unmodified biochar was measured to be 7.41 μS / cm.

[0121] 2 Preparation of composite materials

[0122] Take 50 mL of the bacterial suspension prepared in Example 1 and 5 g of the composite precursor, add 25 mL of commercially available glucose solution, mix well, and adsorb for 6 hours at 35°C and 80 r / min to ensure that the bacterial density in the obtained bacterial solution is greater than 1000 CFU / mL. The obtained bacterial solution is centrifuged at 500 r / min for 30 minutes to obtain a precipitate. Finally, the precipitate is rinsed with 0.9% mass fraction of physiological saline, and the precipitate is the obtained microbial composite material. The microbial composite material is the composite mediator.

[0123] Example 4

[0124] 1. Preparation of conductive-storage materials (i.e. composite precursors)

[0125] Biochar was prepared using fruit tree prunings as raw materials. The pyrolysis temperature was 600°C, and the temperature was increased to 600°C and maintained for 2 hours to obtain biochar. 5 g of the prepared biochar was dispersed in alcohol. The dispersion was completed using a magnetic stirrer. The magnetic stirrer was stirred at 120 r / min for 6 hours. After stirring, it was filtered and washed with deionized water for 3 times, and dried in an oven at 60°C to obtain dry biochar.

[0126] The dried biochar was ball-milled with a ball-to-powder ratio of 150:1, a ball-milling speed of 495r / min, and a time of 24h. The ball-milled biochar was dispersed in 80mL of deionized water and ultrasonically stirred for 0.5h at an ultrasonic power of 480W. Then 0.5g of zinc acetate was added, ultrasonically stirred for 0.5h at an ultrasonic power of 480W, and the ultrasonic temperature was set to 60°C for preheating. The preheated mixed solution was transferred to a 100mL high-pressure hydrothermal reactor with a polytetrafluoroethylene liner. The reactor was reacted at 100°C for 12h. The obtained product was washed with deionized water and dried at 60°C for 12h to obtain biochar modified with zinc oxide, i.e., zinc oxide-biochar.

[0127] 1 g of zinc oxide-biochar was immersed in 50 mL of 1 mmol / L p-benzoquinone solution, the solvent of which was ethanol. The mixture was first stirred at 120 r / min for 12 h, and then shaken at 120 r / min in a 60°C water bath shaker for 24 h. The resulting mixture was poured into a Teflon mold and subjected to a total of 5 freeze and thaw cycles, wherein the freezing condition was -24°C freezing for 12 h, and the thawing condition was room temperature thawing for 5 h. The sample obtained by freezing and thawing was then placed in a freeze dryer and freeze-dried at -50°C and 0.05 mBar vacuum conditions for 12 h. The resulting product (i.e., composite precursor, conductive-electricity storage material) was stored in a drying oven.

[0128] The pseudocapacitance of the composite precursor was measured by cyclic voltammetry to be 1.07 F / g, and the pseudocapacitance of the original biochar was measured to be 0.68 F / g; the conductivity of the composite precursor was measured by four-probe method to be 12.72 μS / cm, and the conductivity of the original biochar was measured to be 4.69 μS / cm.

[0129] 2 Preparation of composite materials

[0130] Take 50 mL of the bacterial suspension prepared in Example 1 and 5 g of the composite precursor, add 25 mL of commercially available glucose solution, mix well, and adsorb for 6 hours at 35°C and 80 r / min to ensure that the bacterial density in the obtained bacterial solution is greater than 1000 CFU / mL. The obtained bacterial solution is centrifuged at 500 r / min for 30 minutes to obtain a precipitate. Finally, the precipitate is washed with 0.9% mass fraction physiological saline, and the precipitate is the obtained microbial composite material.

[0131] Application Example 1

[0132] Experimental group (also recorded as the composite mediator addition group, i.e., composite material addition group): The composite material prepared in Example 1 was applied to medium temperature (37±1°C) corn stalks for continuous anaerobic digestion. The total volume of the fermenter used for continuous anaerobic digestion is 3L. The inoculum anaerobic sludge was first placed in the fermenter, and the amount of anaerobic sludge added was 80% of the total volume of the fermenter, i.e., 2.4L. The anaerobic sludge was first anaerobically digested until the fermenter no longer produced gas. The temperature of anaerobic digestion was 35~38°C, and the anaerobic digestion method was water bath constant temperature fermentation.

[0133] After that, the fermentation tank began to add fermentation raw materials, composite materials and water daily for continuous anaerobic digestion. The fermentation system of continuous anaerobic digestion consisted of inoculum, fermentation raw materials, composite materials and water. The organic load of the continuous anaerobic digestion system was set to 1g / d / L, the hydraulic retention time (HRT) was 20d, and the fermentation material and discharge were added to the fermentation tank every day: the added fermentation material was a mixture of 2.85g corn stalks, 0.1425g composite materials and 0.12L of water, wherein the composite material addition ratio was 5% of the mass of corn stalks, and the composite material was crushed into 1~2mm diameter particles by a pulverizer before addition. The discharge was: 0.12L of fermentation liquid was discharged from the fermentation tank. Discharge was performed before adding the fermentation material, and the above-mentioned discharge and addition of fermentation material steps were repeated every day. The time of continuous anaerobic digestion was 30d. The temperature of continuous anaerobic digestion was 35~38℃, and the continuous anaerobic digestion method was water bath constant temperature fermentation.

[0134] Blank control group: Same as the experimental group, except that the composite material prepared in Example 1 was not added, and the fermentation material added was a mixture of 2.85 g corn stalks and 0.12 L of water, and the output was: 0.12 L of fermentation liquid was discharged from the fermentation tank.

[0135] The daily methane production and cumulative methane production within 30 days of continuous anaerobic digestion in the experimental group and the control group were measured. Figure 2 Table 1 and Table 2 are graphs of daily methane production from anaerobic digestion using the composite material prepared in Example 2 and a blank control group. It can be clearly observed that the daily methane production in the experimental group after adding the composite material was significantly enhanced. Within 30 days, the daily methane production per unit VS of the experimental group was always higher than that of the anaerobic digestion of the control group without adding any material.

[0136] Table 1 Daily methane production in the experimental group and the control group (unit: mL / gVS)

[0137]

[0138] Figure 3Table 2 shows the cumulative methane production within 30 days of anaerobic digestion using the composite material prepared in Example 2 and the blank control group. The cumulative methane production of the experimental group with the composite material added and the control group without the composite material added were 24310 mL / gVS and 20855 mL / gVS, respectively. The cumulative methane production of the experimental group increased by 16.57%.

[0139] Table 2 Cumulative methane production in the experimental group and the control group (unit: mL / gVS)

[0140]

[0141] In summary, applying the composite material prepared by the present invention to the anaerobic digestion process can increase the unit VS daily methane production and cumulative methane production of anaerobic fermentation.

[0142] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A conductive-electricity storage microbial composite material, characterized in that: It comprises a conductive-electricity storage material and microorganisms colonized in the conductive-electricity storage material; the microorganisms comprise acidogenic bacteria and / or methanogenic archaea; the conductive-electricity storage material is formed by combining biochar modified with metal oxides and an electron mediator.

2. The microbial composite material according to claim 1, characterized in that: The bonding method includes covalent bonding and / or copolymerization.

3. The microbial composite material according to claim 1, characterized in that: The electron mediator includes one or more of an endogenous electron mediator, an exogenous electron mediator of a humus mixture and an exogenous quinone-containing mediator. The endogenous electron mediator includes riboflavin and / or flavin; the exogenous quinone-containing mediator includes one or more of benzoquinone, naphthoquinone, phenanthrenequinone and anthraquinone.

4. The method for preparing the microbial composite material according to any one of claims 1 to 3, characterized in that: The following steps are involved: The metal acetate and biochar are first mixed and hydrothermally modified to obtain biochar modified with metal oxides; When the electron mediator is an endogenous electron mediator and / or an exogenous electron mediator of a humus mixture, Dispersing the metal oxide-modified biochar, acrylamide and electron mediator to obtain a dispersion; The dispersion is mixed with a cross-linking agent, an initiator and an accelerator for a second time to perform a hydrothermal reaction to obtain a hydrothermal product; The hydrothermal product is dried and then subjected to a freezing and thawing cycle operation to obtain a conductive-electricity storage material; The conductive-electricity storage material and the microorganism are mixed for the fourth time to obtain a conductive-electricity storage microbial composite material; Alternatively, when the electron mediator is an exogenous quinone-containing mediator, performing a third mixing of the metal oxide-modified biochar and the electron mediator to obtain a mixture; The mixture is subjected to a freezing and thawing cycle operation to obtain a conductive-electricity storage material; The conductive-electricity storage material and the microorganism are mixed for the fourth time to obtain a conductive-electricity storage microbial composite material.

5. The preparation method according to claim 4, characterized in that: The metal acetate includes one or more of zinc acetate, magnesium acetate and ferric acetate; The mass ratio of the metal oxide-modified biochar to acrylamide is 1:1-10; The mass ratio of the biochar to the acetate metal salt is 10-20:1; The first mixing method includes ultrasound, the power of the ultrasound is 480W, the temperature of the ultrasound is 60-90°C, and the time of the ultrasound is 0.5h; The temperature of the hydrothermal modification is 110-150° C., and the time of the hydrothermal modification is 6-12 hours.

6. The preparation method according to claim 4, characterized in that: The mass ratio of acrylamide to cross-linking agent is 1-10:0.1-1; the cross-linking agent includes N,N-methylenebisacrylamide; The mass ratio of acrylamide to initiator is 1-10:0.01-0.1; the initiator comprises persulfate; The accelerator includes N,N,N′,N′-tetramethylethylenediamine; The temperature of the hydrothermal reaction is 80-100° C.; the time of the hydrothermal reaction is 3-6 hours.

7. The preparation method according to claim 4, characterized in that: The drying includes a first drying process, wherein the temperature of the first drying process is 60° C. and the time of the first drying process is 6 to 12 hours.

8. The preparation method according to claim 4, characterized in that: After the freezing and thawing cycle operation, a second drying is also performed, the temperature of the second drying is -80~-50°C; the time of the second drying is 12~36h, and the vacuum degree of the second drying is 0.05~0.1mBar.

9. The preparation method according to claim 4, characterized in that: After the mixture is subjected to a freezing and thawing cycle operation, a third drying process is further performed, wherein the temperature of the third drying process is -80 to -50°C; the time of the third drying process is 12 to 36 hours, and the vacuum degree of the third drying process is 0.05 to 0.1 mBar.

10. A method for strengthening anaerobic fermentation using composite materials, characterized in that: include: The microbial composite material according to claims 1 to 3 or the microbial composite material prepared by the preparation method according to claims 4 to 9 is added to an anaerobic fermentation reactor to promote anaerobic fermentation.