Decarburization annealing process and manufacturing method of oriented electrical steel plate, and oriented electrical steel plate

By controlling the water/hydrogen partial pressure ratio and adding ammonia gas in the annealing furnace, combined with the use of ferrous oxide powder in the isolation agent, the problem of unstable quality of the bottom layer of the magnesium silicate glass film in the existing technology is solved, and high efficiency and stability are achieved. decarburization, nitriding and improvement of surface quality.

CN118726720APending Publication Date: 2024-10-01BAOSHAN IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310320491.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing decarburization annealing technology for oriented silicon steel, it is difficult to accurately control the water/hydrogen partial pressure gradient of the furnace atmosphere, resulting in fluctuations in the quality of the bottom layer of the magnesium silicate glass film and prone to defects such as dew crystals and gold deposits.

Method used

By controlling the water/hydrogen partial pressure ratio in the annealing furnace to 0.1 to 0.15, using an N2+H2 mixed atmosphere for decarburization annealing, and adding ammonia gas in the nitriding section to maintain the same p(H2O)/p(H2), Add ferrous oxide powder to the release agent to ensure that the inner oxide layer reacts with the ferrous oxide powder to form a stable and dense bottom layer of glass film.

Benefits of technology

It achieves an electrical steel plate with good surface quality after high-temperature annealing, reduces the need for equipment and high instrumentation, improves the efficiency and stability of decarburization and nitriding, and forms a dense and uniform bottom layer of magnesium silicate glass film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004151493640000061
    Figure BDA0004151493640000061
  • Figure BDA0004151493640000071
    Figure BDA0004151493640000071
  • Figure BDA0004151493640000072
    Figure BDA0004151493640000072
Patent Text Reader

Abstract

The invention discloses a decarburization annealing process of an oriented electrical steel plate, which comprises the following steps: carrying out decarburization annealing in an N2 + H2 mixed atmosphere in an annealing furnace, and controlling p (H2O) / p (H2) in the decarburization annealing process to be 0.1-0.15; ammonia gas is added into the N2 + H2 mixed atmosphere at the tail of the heat preservation section of the annealing furnace for nitriding, and p (H2O) / p (H2) in the nitriding process is kept consistent with p (H2O) / p (H2) in the decarburization annealing process; and a separant is applied, the separant is a suspension containing mixed powder, and the mixed powder comprises magnesium oxide powder and ferrous oxide powder. Correspondingly, the invention also discloses a manufacturing method of the oriented electrical steel plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a type of steel and a manufacturing method thereof, and in particular to an oriented silicon steel and a manufacturing method thereof. Background Art

[0002] Grain-oriented electrical steel sheets contain about 3% silicon and have a crystal texture with a grain orientation of (110)

[001] and excellent magnetic properties along the rolling direction, so they can be used as core materials for transformers, motors, generators and other electronic equipment.

[0003] The conventional production process of oriented electrical steel sheets is: ironmaking → steelmaking → hot rolling → pickling and normalizing → cold rolling → decarburization annealing → nitriding → isolation coating → high temperature annealing → insulation coating → final annealing → finished product shearing → packaging.

[0004] The oxide layer on the surface of the steel plate after decarburization annealing needs to control the total oxygen content and the ratio of silicon (silicon dioxide) to iron (ferrous oxide) to ensure that a dense and uniform magnesium silicate glass film bottom layer is formed during the high-temperature annealing process. The steel plate after decarburization annealing is coated with an isolation agent, the main component of which is magnesium oxide, and generally an appropriate amount of titanium dioxide, boride, Sb element, Bi element and alkali metal compounds and other additives are added. The mixed isolation agent coating is mixed and stirred with water in a certain proportion to form a suspension, which is then coated on the surface of the strip by a coating machine and a coating roller and then dried and coiled.

[0005] The current decarburization annealing technology for oriented silicon steel generally adopts the method of introducing nitrogen-hydrogen mixed gas from the middle section of the heating furnace and humidifying for decarburization. During the decarburization process, a certain amount of SiO2 inner oxide layer is generated, and a certain amount of Fe2SiO4 or FeO is generated in the outer layer. During the secondary recrystallization annealing process, a solid-state diffusion reaction occurs with the magnesium oxide coated on the surface of the steel plate: 2MgO+SiO2→Mg2SiO4, forming a magnesium silicate glass film bottom layer.

[0006] For example, the Chinese patent document with publication number CN113249554A and publication date August 13, 2021, entitled “A decarburization annealing process for high magnetic induction oriented silicon steel”, which simultaneously performs decarburization and nitriding treatment, requires an ammonia flow rate of 6-20m / s introduced into the annealing furnace. 3 / h, humidification tank temperature 30-70℃, decarbonization temperature 780-880℃, unit speed 45-75m / min, hydrogen ratio 20-60% and nitrogen ratio 40%-80% in the atmosphere.

[0007] For example, the Chinese patent document with publication number CN113832322A, publication date December 24, 2021, and titled "High-efficiency decarburization annealing process for high magnetic induction oriented silicon steel", uses a nitriding atmosphere as a wet atmosphere with a partial pressure ratio of p(H2O) / p(H2) controlled between 0.1 and 0.3, and the nitriding time is controlled to be ≤10s.

[0008] The disadvantage of the prior art is that the key links such as decarburization, internal and external oxide layer formation, and nitriding must be completed within the limited length of the annealing furnace and the plate-passing time. The annealing furnace needs to control the gradient change of the furnace atmosphere from the entrance to the end of the decarburization annealing, with the water / hydrogen partial pressure ratio gradually increasing. However, due to the circulation of the atmosphere in the furnace, the total amount and proportion of components such as SiO2 / FeO / Fe2SiO4 in the generated oxide layer are difficult to accurately control, resulting in the quality of the magnesium silicate bottom layer produced after high-temperature annealing being prone to fluctuations, which in turn leads to defects such as crystal dew and gold spotting.

[0009] Based on this, it is desired to provide a decarburization annealing process and a manufacturing method for an oriented electrical steel sheet to overcome the defects of the prior art. Summary of the invention

[0010] One of the purposes of the present invention is to provide a decarburization annealing process for oriented electrical steel sheets, which controls the water / hydrogen partial pressure ratio in a decarburization annealing furnace to form a dense inner oxide layer mainly composed of silicon dioxide on the surface of the steel strip, and then nitriding is performed in a nitriding section. After annealing, ferrous oxide powder is added to the separator coating to control the oxide layer structure and the total oxygen content on the surface of the steel strip. Accordingly, in the subsequent high-temperature annealing process, the inner oxide layer reacts with the added ferrous oxide powder to finally form a stable and dense glass film bottom layer, so as to manufacture electrical steel sheets with good surface quality.

[0011] In order to achieve the above object, the present invention proposes a decarburization annealing process for oriented electrical steel sheets, which comprises the following steps:

[0012] Decarburization annealing is performed in a N2+H2 mixed atmosphere in an annealing furnace, and p(H2O) / p(H2) during the decarburization annealing is controlled to be 0.1 to 0.15;

[0013] Adding ammonia to the N2+H2 mixed atmosphere at the end of the annealing furnace insulation section to perform nitriding, and keeping the p(H2O) / p(H2) in the nitriding process consistent with the p(H2O) / p(H2) in the decarburization annealing process;

[0014] Applying a release agent, wherein the release agent is a suspension containing mixed powders, wherein the mixed powders include magnesium oxide powder and ferrous oxide powder.

[0015] The present invention controls the water / hydrogen partial pressure ratio during the decarburization annealing process to be 0.1-0.15, so that only a dense SiO2 inner oxide layer is generated on the surface of the steel plate after the decarburization annealing. If p(H2O) / p(H2) is too small, decarburization will be difficult, and if it is too large, ferrous oxide will be generated, affecting the total amount and uniformity of SiO2 in the oxide layer.

[0016] The range of p(H2O) / p(H2) in the nitriding section of the present invention is to ensure the nitriding efficiency and the oxide layer composition. If it is too small, it may cause low nitriding efficiency, and if it is too large, ferrous oxide will be generated, affecting the total amount and uniformity of SiO2 in the oxide layer.

[0017] The decarburization annealing and nitriding sections of the present invention adopt the same p(H2O) / p(H2), and only a certain amount of ammonia needs to be introduced into the nitriding section, i.e., the rear section of the annealing furnace insulation section. Compared with the traditional control mode in which the p(H2O) / p(H2) of the decarburization section is high and the p(H2O) / p(H2) of the nitriding section is low, the device and high instrument used for isolating the atmosphere can be reduced, and the length of the annealing furnace can be reduced, thereby realizing efficient and stable decarburization and nitriding.

[0018] In addition, the present invention adds ferrous oxide (FeO) powder to the separator coating after decarburization annealing. After a reaction in a high-temperature annealing process, SiO2 in the inner oxide layer, the added FeO powder and residual moisture in the coating react to generate Fe2SiO4, and further generate a magnesium silicate base layer, so as to obtain a oriented electrical steel sheet with good surface quality.

[0019] Furthermore, in the decarburization annealing process described in the present invention, the volume ratio of hydrogen in the N2+H2 mixed atmosphere is 30-85%.

[0020] Furthermore, in the decarburization annealing process of the present invention, the decarburization annealing and carburizing temperatures are 800-900°C.

[0021] Furthermore, in the decarburization annealing process described in the present invention, the mass ratio of the ferrous oxide powder to the magnesium oxide powder is (0.1-1):100.

[0022] Furthermore, in the decarburization annealing process described in the present invention, the particle size of the ferrous oxide powder is 100 to 400 nm.

[0023] This particle size can further ensure that the added FeO powder can participate in the production of the inner oxide layer, fully react with the SiO2 inner oxide layer to generate Fe2SiO4, and better generate the magnesium silicate bottom layer.

[0024] Furthermore, the decarburization annealing process of the present invention is characterized in that the nitrogen content in the steel plate after nitriding treatment is 150-250 ppm.

[0025] Furthermore, in the decarburization annealing process of the present invention, the carbon content after decarburization annealing is ≤30 ppm, and the oxygen content is 500-800 ppm.

[0026] Furthermore, in the decarburization annealing process described in the present invention, in the suspension, the mass ratio of the mixed powder to water is 1:6 to 1:10.

[0027] Furthermore, in the decarburization annealing process described in the present invention, the temperature of the isolation agent is 5-8°C, the stirring speed when preparing the isolation agent is above 500r / min, and the isolation agent is applied to the steel plate and dried within 6 hours after preparation.

[0028] The present invention further achieves high-precision control of the total amount of oxides and the SiO2 / FeO ratio of the strip steel surface oxide layer by controlling the coating time, the isolation agent configuration temperature and the stirring speed.

[0029] Furthermore, in the decarburization annealing process of the present invention, the coating thickness of the isolation agent is 10 to 15 g / m 2 .

[0030] Another object of the present invention is to provide a method for manufacturing a oriented electrical steel sheet, by which a oriented electrical steel sheet with good surface quality can be manufactured.

[0031] Based on the above object, the present invention provides a method for manufacturing a oriented electrical steel sheet, which comprises the steps of:

[0032] Producing a cold-rolled steel sheet;

[0033] The cold rolled steel sheet is subjected to decarburization annealing, nitriding and coating with a release agent by using the decarburization annealing process as described above;

[0034] High temperature annealing, insulation coating and flat annealing.

[0035] Furthermore, in the high temperature annealing step of the manufacturing method described in the present invention, heating is performed at a temperature of above 1100°C in a mixed atmosphere of nitrogen and hydrogen, and after completing the secondary recrystallization, heating is performed at a temperature of above 1150°C in the mixed atmosphere of nitrogen and hydrogen for at least 20 hours, and the volume content of hydrogen in the mixed atmosphere is higher than 50%.

[0036] Another object of the present invention is to provide a grain-oriented electrical steel sheet, which is manufactured by the manufacturing method as described above.

[0037] Furthermore, the oriented electrical steel sheet of the present invention, in addition to Fe and other inevitable impurity elements, further contains the following chemical elements in percentage by mass:

[0038] Si: 2.50-4.5%;

[0039] C: 0.015~0.12%;

[0040] Mn: 0.05-0.45%;

[0041] S: 0.002~0.012%;

[0042] Als: 0.015~0.04%;

[0043] N: 0.001~0.01%.

[0044] In this implementation, the design principles of each element are as follows:

[0045] Si increases the electrical resistance of the steel sheet and is very effective in reducing eddy current losses. If the Si content is lower than 2.0wt%, the eddy current losses of the finished product cannot be effectively reduced, and if the Si content is higher than 4.5wt%, the rollability of the steel sheet deteriorates.

[0046] The C content needs to match the Si content to ensure that the reheated billet and steel plate obtain an appropriate proportion of austenite phase (γ phase). Increasing the γ phase ratio can use phase transformation rolling to obtain more fine hot rolled microstructures and reduce (100) <011> It is unfavorable to the strength of the texture and prevents the appearance of fine grains. Since the solid solubility of nitrogen in the γ phase is 10 times greater than that in the α phase, increasing the proportion of the γ phase can also ensure that a large amount of fine AlN is obtained when the hot-rolled steel plate is rapidly cooled after annealing, which is conducive to the small and uniform primary grains and promotes the development of secondary recrystallization.

[0047] The main purpose of Mn and S is to improve hot rolling productivity. Due to the grain boundary segregation of S, when the Mn / S ratio is too low, hot brittleness is prone to occur during hot rolling of the steel billet. In order to improve hot workability, the Mn / S ratio is controlled at 2.5-3.5. This is because Mn significantly reduces the solid solubility of S and forms compounds. In addition, Mn is easily oxidized in the decarburization annealing atmosphere, which affects the formation of the bottom layer. When the S content is high, linear crystals are prone to occur, and it is difficult to remove S during the final high-temperature annealing. In addition, Mn and S can also generate MnS, an inhibitor required for secondary recrystallization.

[0048] Als and N are the constituent elements of AlN, the main inhibitor in high magnetic induction oriented silicon steel. In order to obtain moderately strong inhibitory force, the present invention controls the range of Als and N in the steel to adjust the size and distribution of AlN, ensure that the well-oriented Gossian nuclei undergo perfect secondary recrystallization, and obtain excellent magnetic properties.

[0049] The decarburization annealing process and manufacturing method of the oriented electrical steel sheet of the present invention have the following advantages and beneficial effects:

[0050] The decarburization annealing and nitriding sections of the present invention adopt the same p(H2O) / p(H2), and only a certain amount of ammonia needs to be introduced into the nitriding section, i.e., the rear section of the annealing furnace insulation section. Compared with the traditional control mode in which the p(H2O) / p(H2) of the decarburization section is high and the p(H2O) / p(H2) of the nitriding section is low, the device and high instrument used for isolating the atmosphere can be reduced, and the length of the annealing furnace can be reduced, thereby realizing efficient and stable decarburization and nitriding.

[0051] After high-temperature annealing, the present invention can eventually form a stable and dense glass film bottom layer to obtain a oriented electrical steel sheet with good surface quality. DETAILED DESCRIPTION

[0052] The decarburization annealing process, manufacturing method and oriented electrical steel sheet of the present invention will be further explained and illustrated in conjunction with specific embodiments below. However, such explanation and illustration do not constitute an improper limitation on the technical solution of the present invention.

[0053] Examples 1-16 and Comparative Examples 1-18

[0054] The oriented electrical steel sheets of each embodiment and comparative example were manufactured according to the following steps:

[0055] (1) Steel billets were prepared. The composition ratios of the steel billets of the embodiments and comparative examples are shown in Table 1.

[0056] (2) The steel billet is reheated at a temperature below 1380°C and hot rolled to obtain a hot-rolled steel plate with a thickness of 2.0 to 3.0 mm.

[0057] (3) Then, the steel is hot-rolled and annealed at 1000-1150°C, pickled, and cold-rolled to obtain a cold-rolled steel sheet with a thickness of 0.15-0.35 mm.

[0058] (4) Decarburization annealing, nitriding treatment and coating of isolation agent:

[0059] Decarburization annealing is performed in a N2+H2 mixed atmosphere in an annealing furnace, wherein the volume ratio of hydrogen in the mixed atmosphere is 30-85%, p(H2O) / p(H2) during the decarburization annealing is controlled to be 0.1-0.15, and the carbon content after decarburization annealing is ≤30ppm, and the oxygen content is 500-800ppm;

[0060] Adding ammonia to the N2+H2 mixed atmosphere at the end of the annealing furnace insulation section to perform nitriding, keeping the p(H2O) / p(H2) in the nitriding process consistent with the p(H2O) / p(H2) in the decarburization annealing process, and the nitrogen content in the steel plate after nitriding is 150-250ppm; the decarburization annealing and carburizing temperatures are 800-900°C;

[0061] The isolation agent is prepared according to a mass ratio of mixed powder to water of 1:6 to 1:10, wherein the mixed powder includes magnesium oxide powder and ferrous oxide powder, the mass ratio of ferrous oxide powder to magnesium oxide powder is: (0.1 to 1):100, and the particle size of the ferrous oxide powder is 100 to 400 nm. During the liquid preparation process, the temperature of the isolation agent is controlled to be 5 to 8°C, and the stirring speed when preparing the isolation agent is above 500 r / min. The isolation agent is applied to a steel plate and dried within 6 hours after preparation, and the coating thickness of the isolation agent is 10 to 15 g / m2.

[0062] (5) High temperature annealing: heating at a temperature of 1100° C. or higher in a mixed atmosphere of nitrogen and hydrogen, and after completion of secondary recrystallization, heating at a temperature of 1150° C. or higher for at least 20 h in a mixed atmosphere of nitrogen and hydrogen, wherein the volume content of hydrogen in the mixed atmosphere is higher than 50%.

[0063] (6) Insulation coating and flat annealing: A conventional insulation coating containing phosphate and colloidal silica is applied and hot-stretched flat annealing is performed to obtain a oriented electrical steel sheet.

[0064] Table 1 lists the mass percentages of various chemical elements in the oriented electrical steel sheets of Examples 1-16 and the steel sheets of Comparative Examples 1-18.

[0065] Table 1. (wt%, the balance is Fe and other inevitable impurity elements)

[0066]

[0067]

[0068] Table 2 lists the decarburization annealing process parameters involved in Examples 1-16 and Comparative Examples 1-18.

[0069] Table 2.

[0070]

[0071]

[0072] Note: The p(H2O) / p(H2) standard in Table 2 is: the shielding gas is passed into the furnace after passing through the humidifier, and the water partial pressure p(H2O) is calculated by controlling the water content of saturated water vapor in the atmosphere by controlling the water temperature of the humidifier. The p(H2) is calculated by the proportion of hydrogen in the shielding gas, thus measuring p(H2O) / p(H2), that is, the water / hydrogen partial pressure ratio.

[0073] Table 3 lists the configuration and coating parameters of the release agents involved in Examples 1-16 and Comparative Examples 1-18.

[0074] Table 3.

[0075]

[0076]

[0077] Note: In Table 3, the average particle size of FeO powder was measured by laser particle size analyzer.

[0078] Table 4 lists the high temperature annealing process parameters of various embodiments and comparative examples.

[0079] Table 4.

[0080]

[0081]

[0082] In order to verify the effect of the present invention, the inventors sampled the oriented electrical steel sheets of each embodiment and comparative example, and tested and evaluated the coating quality, baking effect, bottom layer thickness, and bottom layer uniformity. In addition, the magnetic induction of each embodiment and comparative example was tested with a single-piece tester based on GB / T 13789-2008, and the results are listed in Table 5. In Table 5, coating quality "○" indicates uniform coating, and coating quality "×" indicates uneven coating. Baking effect "○" indicates that the coating is dried and the moisture content is less than 3%, and baking effect "×" indicates that the coating is not dried or the moisture content is greater than 3%. Bottom layer thickness "○" indicates that the magnesium silicate bottom layer is uniform and dense, and bottom layer thickness "×" indicates that the magnesium silicate bottom layer cannot cover the grains, and the substrate grains are visible to the naked eye. Bottom layer uniformity "○" indicates that the surface of the magnesium silicate bottom layer is uniform, and bottom layer uniformity "×" indicates that the surface of the magnesium silicate bottom layer is uneven, with obvious color difference or stripes. Magnetic performance "○" indicates that the magnetic induction intensity of the finished product is higher than 1.92T, magnetic performance "△" indicates that the magnetic induction intensity of the finished product is between 1.88-1.92T, and magnetic performance "×" indicates that the magnetic induction intensity of the finished product is lower than 1.88T.

[0083] Table 5.

[0084]

[0085] It can be seen that by adopting the technical solution of the present invention, a oriented electrical steel sheet with good surface quality and excellent magnetic properties can be manufactured.

[0086] It should be noted that the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.

[0087] It should also be noted that the above-listed embodiments are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therewith can be directly derived or easily associated with the contents disclosed by those skilled in the art from the present invention, and all should belong to the protection scope of the present invention.

Claims

1. A decarburization annealing process for oriented electrical steel sheets. It is characterized in that Includes steps: N in the annealing furnace 2 +H 2 Decarburization annealing is carried out in a mixed atmosphere to control the p(H 2 O) / p(H 2 ) is 0.1 to 0.15; At the end of the annealing furnace insulation section, 2 +H 2 Add ammonia to the mixed atmosphere for nitriding, and keep the pH (H 2 O) / p(H 2 ) and p(H 2 O) / p(H 2 ) are consistent; Applying a release agent, wherein the release agent is a suspension containing mixed powders, wherein the mixed powders include magnesium oxide powder and ferrous oxide powder.

2. The decarburization annealing process according to claim 1, It is characterized in that The N 2 +H 2 The volume ratio of hydrogen in the mixed atmosphere is 30 to 85%.

3. The decarburization annealing process according to claim 1, It is characterized in that The decarburization annealing and carburizing temperature is 800-900℃.

4. The decarburization annealing process according to claim 1, It is characterized in that The mass ratio of the ferrous oxide powder to the magnesium oxide powder is (0.1-1):

100.

5. The decarburization annealing process according to claim 1, It is characterized in that The particle size of the ferrous oxide powder is 100-400 nm.

6. The decarburization annealing process according to claim 1, It is characterized in that The nitrogen content in the steel sheet after the nitriding treatment is 150 to 250 ppm.

7. The decarburization annealing process according to claim 1, It is characterized in that The carbon content after decarburization annealing is ≤30ppm, and the oxygen content is 500-800ppm.

8. The decarburization annealing process according to claim 1, It is characterized in that In the suspension, the mass ratio of the mixed powder to water is 1:6 to 1:

10.

9. The decarburization annealing process according to claim 1, It is characterized in that The temperature of the isolation agent is 5-8°C, the stirring speed during the preparation of the isolation agent is above 500r / min, and the isolation agent is applied to the steel plate and dried within 6 hours after preparation.

10. The decarburization annealing process according to claim 1, It is characterized in that The coating thickness of the release agent is 10 to 15 g / m 2 .

11. A method for manufacturing a oriented electrical steel sheet, It is characterized in that It includes the steps of: Producing a cold-rolled steel sheet; Decarburization annealing, nitriding and coating of a release agent are performed on the cold-rolled steel sheet using the decarburization annealing process as described in any one of claims 1 to 10; High temperature annealing, insulation coating and flat annealing.

12. The manufacturing method according to claim 11, It is characterized in that In the high temperature annealing step, heating is performed at a temperature above 1100°C in a mixed atmosphere of nitrogen and hydrogen, and after completing secondary recrystallization, heating is performed at a temperature above 1150°C for at least 20 hours in the mixed atmosphere of nitrogen and hydrogen, wherein the volume content of hydrogen in the mixed atmosphere is higher than 50%.

13. A oriented electrical steel sheet, It is characterized in that The method is prepared by the manufacturing method according to any one of claims 1 to 12.

14. The oriented electrical steel sheet according to claim 13, It is characterized in that In addition to Fe and other unavoidable impurity elements, it also contains the following chemical elements in percentage by mass: Si: 2.50-4.5%; C:0.015~0.12%; Mn: 0.05-0.45%; S:0.002~0.012%; Als: 0.015~0.04%; N:0.001~0.01%。

Citation Information

Cited By

  • Annealing optimization method for high-magnetic-induction oriented silicon steel

    CN121874436A