Method for selectively precipitating and separating zinc and magnesium

Through the combination method of citric acid precipitant and concentrated sulfuric acid, the selective separation of zinc and magnesium is achieved by taking advantage of the solubility difference in acidic environment, solving the problem of zinc and magnesium separation in wet zinc smelting, and achieving high efficiency and low cost. separation effect.

CN118726757APending Publication Date: 2024-10-01CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410971749.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing technology is difficult to efficiently and selectively separate zinc and magnesium in the zinc hydrometallurgy process. Traditional methods have problems such as large zinc losses, high costs, and equipment hazards, and lack economically feasible separation technologies.

Method used

Use a citric acid precipitant to adjust the pH value to precipitate zinc ions. After calcination, add a magnesium removing reagent and concentrated sulfuric acid to achieve selective separation of zinc and magnesium. The separation is carried out through the difference in solubility of zinc citrate and magnesium citrate in an acidic environment.

Benefits of technology

It achieves high-efficiency and high-quality separation of zinc and magnesium, with high zinc recovery rate (about 95%), low magnesium inclusion rate, green and environmentally friendly process, simplified production process and reduced costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726757A_ABST
    Figure CN118726757A_ABST
Patent Text Reader

Abstract

The invention discloses a method for selectively precipitating and separating zinc and magnesium, which comprises the following steps: firstly, adding a citric acid precipitant into a solution containing zinc and magnesium, then adjusting the pH value, and carrying out solid-liquid separation after precipitation to obtain a zinc citrate solid and a magnesium-containing filtrate; adding a magnesium removal reagent into the magnesium-containing filtrate, carrying out solid-liquid separation, and supplementing concentrated sulfuric acid into the filtrate; and finally, calcining zinc citrate to obtain zinc oxide, adding the zinc oxide into the filtrate supplemented with the concentrated sulfuric acid, and carrying out acid leaching to obtain a zinc sulfate solution, thereby realizing selective separation of zinc and magnesium in the zinc-magnesium mixed solution. According to the invention, selective high-efficiency high-quality separation of zinc and magnesium is realized through different pH values during precipitation of zinc citrate and magnesium citrate; the method is green, environmentally friendly and simple in process, the zinc and magnesium separation method in the zinc hydrometallurgy process is provided, and good application prospects are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of zinc hydrometallurgy, and in particular to a method for selectively precipitating and separating zinc and magnesium. Background Art

[0002] Separating zinc and magnesium from zinc-magnesium solutions is mainly used in the field of hydrometallurgical zinc smelting technology. Zinc sulfate is an important raw material in the hydrometallurgical smelting of zinc. Hydrometallurgical zinc smelting is the main technology for dissolving zinc in zinc roasted sand in aqueous solution to extract metallic zinc from it. In the zinc smelting process, the roasted zinc concentrate is acid-leached, and the generated zinc sulfate, as the source of zinc element, enters the electrolytic cell for electrolysis, thereby reducing the zinc dissolved in the solution. The electrolysis process is the core step of hydrometallurgical zinc smelting, and high-purity metallic zinc can be obtained through this step. During the acid leaching process, magnesium ions will enter the solution together with the dissolution of zinc, which has a great impact on the yield and equipment of zinc. Therefore, separating magnesium ions from zinc-containing solutions has become the key to producing high-purity zinc products. However, zinc and magnesium both belong to the main group IⅠ elements and have similar chemical properties. It is difficult for traditional methods to selectively separate zinc and magnesium from zinc-magnesium solutions, which has become a technical bottleneck for the production of high-purity zinc products.

[0003] In the hydrometallurgical zinc smelting process, sphalerite can be leached with sulfuric acid before smelting, and the leaching rate of magnesium can reach 77.8%. Similarly, sulfur dioxide gas and water vapor are introduced into the zinc concentrate before calcination to convert magnesium into magnesium sulfite. Since zinc sulfide can stably exist in low-concentration sulfuric acid, this method can achieve a certain separation of zinc and magnesium. However, some zinc will exist in the zinc concentrate in the form of zinc oxide, which will be lost with pickling. This method causes a large loss of zinc. In production, limestone can also be added to the leachate to form basic zinc sulfate precipitation to achieve the effect of zinc and magnesium separation. However, when the amount of lime is large, a large amount of calcium sulfate will be generated, which requires additional processes to remove.

[0004] Chinese patent CN 1935705 A relates to a method of passing a zinc-magnesium solution through a negative membrane dialyzer and then neutralizing and precipitating zinc with lime milk. However, this method requires regular membrane replacement and is costly. In addition, when lime is used in large amounts, calcium sulfate will be generated, which requires additional processes to remove. Chinese patent CN 118221180 A relates to a method of adding fluoride salts to generate magnesium fluoride precipitation. However, this method introduces a large amount of fluoride ions, which is harmful to production equipment. Chinese patent CN 118206142 A relates to a method for preparing basic magnesium carbonate to remove magnesium. However, the alkaline conditions of this method are not suitable for the solution environment of wet zinc smelting. Similarly, Chen Jinlong et al. used a carbonization precipitation method to separate and recover zinc and magnesium, but the solution environment also did not meet the requirements. Chinese patent CN 220664996 U relates to a method for removing magnesium with sodium phosphate. However, the phosphate introduced by this method also causes zinc precipitation and is not selective. Chinese patent CN 116623002 A relates to a method for removing magnesium ions in the process of wet zinc smelting by crystallization. However, this method has high energy consumption and high operating costs. Chinese patent CN 113528818 A relates to a method for removing magnesium using a specific ion exchange resin, but this method has a low efficiency in removing magnesium, is complex to operate, and has a high cost. Obviously, there is an urgent need to develop an economically feasible and easy-to-practice zinc-magnesium separation technology in the field of hydrometallurgy. Summary of the invention

[0005] The invention aims to overcome the disadvantages of the prior art and provide a method for selectively precipitating and separating zinc and magnesium. The method comprises the following steps: firstly, adding a citric acid precipitant to a solution containing zinc and magnesium, adjusting the pH value, and performing solid-liquid separation after precipitation to obtain zinc citrate solid and a magnesium-containing filtrate; then, adding a magnesium removal agent to the magnesium-containing filtrate, performing solid-liquid separation, and adding concentrated sulfuric acid to the filtrate; finally, calcining the zinc citrate to obtain zinc oxide, and then adding the zinc oxide to the filtrate added with concentrated sulfuric acid for acid leaching to obtain a zinc sulfate solution, thereby realizing selective separation of zinc and magnesium in a zinc-magnesium mixed solution; the invention realizes selective, efficient and high-quality separation of zinc and magnesium by virtue of different pH values ​​when zinc citrate and magnesium citrate are precipitated; the invention is green and environmentally friendly, has a simple process, provides a method for separating zinc and magnesium in a zinc hydrometallurgical process, and has good application prospects.

[0006] In order to achieve the above technical effects, the following technical solutions are adopted: A method for selectively precipitating and separating zinc and magnesium comprises the following steps: Step S1: adding a citric acid precipitant to a mixed solution containing zinc and magnesium, adjusting the pH value, and performing solid-liquid separation after sufficient precipitation to obtain a zinc precipitate and a magnesium-containing filtrate; Step S2: calcining the zinc precipitate obtained in step S1 to obtain zinc oxide; Step S3: adding a magnesium removal agent to the magnesium-containing filtrate obtained in step S1, and performing solid-liquid separation after sufficient precipitation to obtain a magnesium precipitate and a pure filtrate, and adding concentrated sulfuric acid to the pure filtrate; Step S4: adding the zinc oxide obtained in step S2 to the pure filtrate supplemented with concentrated sulfuric acid obtained in step S3; obtaining a zinc sulfate solution through acid leaching to complete the selective zinc-magnesium separation of the zinc-magnesium mixed solution.

[0007] Furthermore, the solution containing zinc and magnesium in step S1 has a zinc content of 130-150 g / L and a magnesium content of 10-15 g / L.

[0008] Furthermore, the citric acid precipitant in step S1 includes at least one of citric acid, sodium citrate and potassium citrate.

[0009] Furthermore, in step S1, the ratio of the amount of the zinc ion substance to the amount of the citric acid precipitant substance is 1-1.5:1.

[0010] Furthermore, in step S1, a sodium hydroxide solution is used to adjust the pH value.

[0011] Furthermore, in step S1, the pH value is adjusted to 2.0-4.0.

[0012] Furthermore, the reaction conditions in step S1 are 500-600 rpm, 60-80° C., and heating in a water bath for 1-2 h.

[0013] Furthermore, the calcination gas environment in step S2 is air, the calcination temperature is greater than 400° C., and the time is 1-2 hours.

[0014] Furthermore, the magnesium removal reagent in step S3 comprises at least one of conventional magnesium removal agents such as sodium hydroxide and sodium phosphate; the concentration of concentrated sulfuric acid is 18 mol / L, and the sulfuric acid concentration in the pure filtrate solution after adding concentrated sulfuric acid is 2-3 mol / L.

[0015] Furthermore, the acid leaching liquid in step S4 is sulfuric acid, with a liquid-to-solid ratio of 4-6 mL:1 g, and the end point pH value of the solution is controlled to be 2.0-3.0; the acid leaching conditions are 500-600 rpm, and heating in a water bath at 60-80° C. for 1-2 h.

[0016] Controlling the liquid-to-solid ratio, leaching temperature and leaching time in the acid leaching process within a reasonable range can improve the leaching efficiency and help obtain a high-purity zinc sulfate solution. Too low liquid-to-solid ratio, too low leaching temperature or too short leaching time will relatively reduce the zinc leaching rate; while too high liquid-to-solid ratio will lead to too low zinc concentration in the leaching solution, which is not conducive to subsequent reactions; too high leaching temperature or too long time will increase leaching energy consumption.

[0017] The principle of the technical solution of the present invention is: The structure of the citric acid molecule (C6H8O7) contains three carboxyl groups, which will combine with metal ions to form citrate. Among them, zinc citrate is a substance with good stability and is not easily soluble in an acidic environment, while magnesium citrate is usually soluble in an acidic environment. The leaching solution and electrolyte of hydrometallurgical zinc smelting are usually acidic. The difference in solubility between the two in an acidic environment can be used to separate zinc and magnesium. The reaction to form citrate is as follows:

[0018]

[0019] For example, when the reaction conditions are 500 rpm, 60°C water bath heating for 1 hour, and pH is in the range of 2.0-4.0, zinc citrate precipitates more completely, and magnesium citrate hardly precipitates, completing the selective separation of zinc and magnesium. Zinc citrate decomposes into zinc oxide after calcination at 400°C for 1 hour, and the reaction is as follows:

[0020] Since the filtrate mainly contains residual magnesium ions, it can be removed by conventional magnesium removal methods such as pH adjustment and phosphate precipitation.

[0021] Zinc oxide is leached with sulfuric acid to generate zinc sulfate, which enters the subsequent production. The acid leaching reaction is as follows:

[0022] This allows the separation of zinc and magnesium during the hydrometallurgical smelting of zinc.

[0023] The beneficial effects of the present invention are: 1. Good zinc-magnesium separation effect: The present invention converts zinc into zinc citrate, and after calcination (converting into zinc oxide is beneficial to subsequent zinc recovery) and acid leaching, the zinc ions and magnesium ions are efficiently separated in the original solution system without generating any waste water or solid waste. Only materials are added to the system without generating waste externally. The zinc recovery rate is high (about 95%), the magnesium inclusion rate is low (3-5%), and the zinc-magnesium separation effect is good; 2. High adaptability to the production environment: The present invention realizes the separation of zinc and magnesium in an acidic solution by using different pH values ​​when zinc citrate and magnesium citrate are precipitated, wherein zinc citrate is not easily soluble in an acidic environment, while magnesium citrate is usually soluble in an acidic environment; 3. Green and environmentally friendly: The citric acid reagent used in the present invention is an organic weak acid, green and non-toxic; natural citric acid is widely distributed in nature, has the advantages of being green and environmentally friendly, low cost, and has excellent application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. The drawings in the following description are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0025] Figure 1 It is a schematic diagram of the process of selective precipitation of zinc and magnesium by citric acid provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0028] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations and / or combinations thereof.

[0029] Embodiment 1: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 150 g / L and 13.8 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, after adding citric acid at a molar ratio of zinc to citric acid of 1.5:1, the pH of the solution was controlled to 3.0 with sodium hydroxide at a concentration of 10 mol / L, and the solution was kept warm for 1 hour; after the insulation was completed, the beaker was taken out, cooled to room temperature, and the solid and liquid were separated; then, the zinc citrate solid was calcined at 400°C for 1 hour to obtain zinc oxide; then, a magnesium removal reagent (theoretical amount of sodium phosphate) was added to the magnesium-containing filtrate, and the solution was kept warm in a water bath stirring pot at 60°C and a speed of 500 rpm for 1 hour to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the addition of concentrated sulfuric acid, the sulfuric acid concentration in the solution was 2 mol / L) was added to the filtrate, and the solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc oxide to obtain a zinc sulfate solution (liquid-to-solid ratio of 6 mL:1 g, and the end point pH of the solution was controlled to be 2.0). The results showed that the zinc precipitation rate was 98.3%, the magnesium inclusion rate was 3.8%, and the zinc recovery rate was 96.2%.

[0030] Embodiment 2: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Different from Example 1, the pH of the solution was controlled to 2.0 using sodium hydroxide having a concentration of 10 mol / L.

[0031] Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 130 g / L and 15 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, after adding citric acid at a molar ratio of zinc to citric acid of 1.5:1, the pH of the solution was controlled to 2.0 with sodium hydroxide at a concentration of 10 mol / L, and the solution was kept warm for 1 hour; after the insulation was completed, the beaker was taken out, cooled to room temperature, and the solid and liquid were separated; then, the zinc citrate solid was calcined at 400°C for 1 hour to obtain zinc oxide; then, a magnesium removal agent (theoretical amount of sodium phosphate) was added to the magnesium-containing filtrate, and the solution was kept warm in a water bath stirring pot at 60°C and a speed of 500 rpm for 1 hour to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the addition of concentrated sulfuric acid, the sulfuric acid concentration in the solution was 3 mol / L) was added to the filtrate, and the solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc oxide to obtain a zinc sulfate solution (liquid-to-solid ratio of 4 mL:1 g, and the end point pH of the solution was controlled to be 3.0). The results showed that the zinc precipitation rate was 97.2%, the magnesium inclusion rate was 3.5%, and the zinc recovery rate was 95.7%.

[0032] Embodiment 3: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Different from Example 1, the pH of the solution is controlled to be 4.0 using sodium hydroxide having a concentration of 10 mol / L, and sodium hydroxide is selected as the magnesium removal agent.

[0033] Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 150 g / L and 10 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, after adding citric acid at a molar ratio of zinc to citric acid of 1.5:1, the pH of the solution was controlled to 4.0 with sodium hydroxide at a concentration of 10 mol / L, and the solution was kept warm for 1 hour; after the insulation was completed, the beaker was taken out, cooled to room temperature, and the solid and liquid were separated; then, the zinc citrate solid was calcined at 400°C for 1 hour to obtain zinc oxide; then, a magnesium removal reagent (theoretical amount of sodium hydroxide) was added to the magnesium-containing filtrate, and the solution was kept warm in a water bath stirring pot at 60°C and a speed of 500 rpm for 1 hour to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the concentrated sulfuric acid was added, the sulfuric acid concentration in the solution was 2 mol / L) was added to the filtrate, and the solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc oxide to obtain a zinc sulfate solution (liquid-to-solid ratio of 6 mL:1 g, and the end point pH of the solution was controlled to be 2.0). The results showed that the zinc precipitation rate was 97.6%, the magnesium inclusion rate was 4.3%, and the zinc recovery rate was 95.9%.

[0034] Embodiment 4: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Different from Example 1, the molar ratio of zinc to citric acid is 1.2:1.

[0035] Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 150 g / L and 13.8 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, after adding citric acid at a molar ratio of zinc to citric acid of 1.2:1, the pH of the solution was controlled to 3.0 with sodium hydroxide at a concentration of 10 mol / L, and the solution was kept warm for 1 hour; after the insulation was completed, the beaker was taken out, cooled to room temperature, and the solid and liquid were separated; then, the zinc citrate solid was calcined at 400°C for 1 hour to obtain zinc oxide; then, a magnesium removal reagent (theoretical amount of sodium phosphate) was added to the magnesium-containing filtrate, and the solution was kept warm in a water bath stirring pot at 60°C and a speed of 500 rpm for 1 hour to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the addition of concentrated sulfuric acid, the sulfuric acid concentration in the solution was 2 mol / L) was added to the filtrate, and the solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc oxide to obtain a zinc sulfate solution (liquid-to-solid ratio of 6 mL:1 g, and the end point pH of the solution was controlled to be 2.0). The results showed that the zinc precipitation rate was 98.4%, the magnesium inclusion rate was 4.5%, and the zinc recovery rate was 96.4%.

[0036] Embodiment 5: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Different from Example 1, the molar ratio of zinc to citric acid is 1:1, and sodium hydroxide is used as the magnesium removal agent.

[0037] Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 150 g / L and 13.8 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, after adding citric acid at a molar ratio of zinc to citric acid of 1:1, the pH of the solution was controlled to 3.0 with sodium hydroxide at a concentration of 10 mol / L, and the solution was kept warm for 1 hour; after the insulation was completed, the beaker was taken out, cooled to room temperature, and the solid and liquid were separated; then, the zinc citrate solid was calcined at 400°C for 1 hour to obtain zinc oxide; then, a magnesium removal reagent (theoretical amount of sodium hydroxide) was added to the magnesium-containing filtrate, and the solution was kept warm in a water bath stirring pot at 60°C and a speed of 500 rpm for 1 hour to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the addition of concentrated sulfuric acid, the sulfuric acid concentration in the solution was 2 mol / L) was added to the filtrate, and the solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc oxide to obtain a zinc sulfate solution (liquid-to-solid ratio of 6 mL:1 g, and the end point pH of the solution was controlled to be 2.0). The results showed that the zinc precipitation rate was 99.5%, the magnesium inclusion rate was 4.9%, and the zinc recovery rate was 97.2%.

[0038] Embodiment 6: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Different from Example 1, sodium citrate was used as a precipitant.

[0039] Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 150 g / L and 13.8 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, sodium citrate was added at a molar ratio of zinc to sodium citrate of 1.5:1, and then the pH of the solution was controlled to 3.0 with sulfuric acid at a concentration of 1 mol / L, and the solution was kept warm for 1 hour. After the insulation was completed, the beaker was taken out, cooled to room temperature, and the solid and liquid were separated. Then, the zinc citrate solid was calcined at 400°C for 1 hour to obtain zinc oxide. Next, a magnesium removal agent (theoretical amount of sodium phosphate) was added to the magnesium-containing filtrate, and the solution was kept warm in a water bath stirring pot at 60°C and a speed of 500 rpm for 1 hour to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the addition of concentrated sulfuric acid, the sulfuric acid concentration in the solution was 2 mol / L) was added to the filtrate, and the solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc oxide to obtain a zinc sulfate solution (liquid-to-solid ratio of 6 mL:1 g, and the end point pH of the solution was controlled to be 2.0). The results showed that the zinc precipitation rate was 96.3%, the magnesium inclusion rate was 4.0%, and the zinc recovery rate was 95.2%.

[0040] Embodiment 7: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Different from Example 1, the calcination temperature was 300°C.

[0041] Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 150 g / L and 13.8 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, after adding citric acid at a molar ratio of zinc to citric acid of 1.5:1, the pH of the solution was controlled to 3.0 with sodium hydroxide at a concentration of 10 mol / L, and the solution was kept warm for 1 hour; after the insulation was completed, the beaker was taken out, cooled to room temperature, and the solid and liquid were separated; then, the zinc citrate solid was calcined at 300°C for 1 hour to obtain zinc oxide; then, a magnesium removal agent (theoretical amount of sodium phosphate) was added to the magnesium-containing filtrate, and the solution was kept warm in a water bath stirring pot at 60°C and a speed of 500 rpm for 1 hour to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the addition of concentrated sulfuric acid, the sulfuric acid concentration in the solution was 2 mol / L) was added to the filtrate, and the solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc oxide to obtain a zinc sulfate solution (liquid-to-solid ratio of 6 mL:1 g, and the end point pH of the solution was controlled to be 2.0). The results showed that the zinc precipitation rate was 98.0%, the magnesium inclusion rate was 3.8%, and the zinc recovery rate was 81.6%. Due to insufficient calcination temperature, zinc citrate was not completely converted into zinc oxide, so the zinc recovery rate was low.

[0042] Embodiment 8: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Different from Example 1, no sodium hydroxide was added to adjust the pH.

[0043] Selective separation of zinc and magnesium in a simulated mixed solution of zinc and magnesium, the zinc concentration and magnesium concentration in the simulated solution were set to 150 g / L and 13.8 g / L, respectively. 30 mL of the simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, citric acid was added at a molar ratio of zinc to citric acid of 1.5:1, and the mixture was kept warm for 1 hour; since no precipitation was produced at this pH value (about 0.5), it was impossible to selectively separate zinc and magnesium.

[0044] Embodiment 9: according to Figure 1 As shown, the zinc and magnesium separation operation is performed: Different from Example 1, humic acid is used as the precipitant.

[0045] Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the zinc concentration and magnesium concentration in the simulated solution were set to 150 g / L and 13.8 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, after adding humic acid at a molar ratio of zinc to humic acid of 1.5:1, the pH of the solution was adjusted with sodium hydroxide at a concentration of 10 mol / L, and no precipitation was produced, so zinc and magnesium could not be selectively separated.

[0046] Comparative Example 1: Example 1 is used as a benchmark: Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 150 g / L and 13.8 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, the pH of the solution was controlled to 6.5 with sodium hydroxide at a concentration of 10 mol / L, and the solution was kept warm for 1 hour. After the insulation, the beaker was taken out and cooled to room temperature to separate the solid and liquid. Then, the solid was calcined at 400°C for 1 hour. Then, a magnesium remover (theoretical amount of sodium phosphate) was added to the magnesium-containing filtrate, and the solution was kept warm in a water bath stirring pot at 60°C and a speed of 500 rpm for 1 hour to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the addition of concentrated sulfuric acid, the sulfuric acid concentration in the solution was 2 mol / L) was added to the filtrate. The solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc oxide to obtain a zinc sulfate solution (liquid-solid ratio of 6 mL: 1 g, and the end point pH of the solution was controlled to be 2.0). The results showed that the precipitation rate of zinc was 78.4%, the inclusion rate of magnesium was 34.5%, and the recovery rate of zinc was 70.6%. The precipitation rate and recovery rate of zinc were low, and the inclusion rate of magnesium was high.

[0047] Comparative Example 2: Using Example 1 as a benchmark: Selective separation of zinc and magnesium in simulated mixed solution of zinc and magnesium, the concentration of zinc and magnesium in the simulated solution was set to 150 g / L and 13.8 g / L respectively. 30 mL of simulated mixed solution of zinc and magnesium was added to a 100 mL beaker and stirred in a water bath stirring pot at 60°C and 500 rpm. First, after adding citric acid at a molar ratio of zinc to citric acid of 1.5:1, the pH of the solution was controlled to 3.0 with sodium hydroxide at a concentration of 10 mol / L, and the solution was kept warm for 1 hour; after the insulation was completed, the beaker was taken out, cooled to room temperature, and the solid and liquid were separated; then, a magnesium removal reagent (theoretical amount of sodium phosphate) was added to the magnesium-containing filtrate, and the solution was kept warm for 1 hour in a water bath stirring pot at 60°C and a speed of 500 rpm to separate the solid and liquid to obtain a magnesium precipitate, and concentrated sulfuric acid (concentration of 18 mol / L, after the addition of concentrated sulfuric acid, the sulfuric acid concentration in the solution was 2 mol / L) was added to the filtrate, and the solution was heated in a water bath at 500 rpm and 60°C for 1 hour to leach zinc citrate to obtain a zinc sulfate solution (liquid-solid ratio of 6 mL: 1 g, and the end point pH of the solution was controlled to be 2.0). The results showed that the precipitation rate of zinc was 98.3%, the inclusion rate of magnesium was 4.8%, and the recovery rate of zinc was 50.3%, and the recovery rate of zinc was low.

[0048] The experimental results of Examples 1-7 and Comparative Examples 1-2 are summarized in Table 1: Table 1 Changes in zinc precipitation rate, recovery rate and magnesium inclusion rate in simulated solution under different schemes Group Precipitant Molar ratio pH Calcination temperature (℃) Zinc precipitation rate (%) Magnesium inclusion rate (%) Zinc recovery rate (%) Example 1 Citric Acid 1.5:1 3.0 400 98.3 3.8 96.2 Example 2 Citric Acid 1.5:1 2.0 400 97.2 3.5 95.7 Example 3 Citric Acid 1.5:1 4.0 400 97.6 4.3 95.9 Example 4 Citric Acid 1.2:1 3.0 400 98.4 4.5 96.4 Example 5 Citric Acid 1:1 3.0 400 99.5 4.9 97.2 Example 6 Sodium Citrate 1.5:1 3.0 400 96.3 4.0 95.2 Example 7 Citric Acid 1.5:1 3.0 300 98.0 3.8 81.6 Comparative Example 1 Sodium hydroxide 1:1 6.5 400 78.4 34.5 70.6 Comparative Example 2 Citric Acid 1.5:1 3.0 Not calcined 98.3 4.8 50.3 The method of the present invention first precipitates zinc ions with a citric acid precipitant and then precipitates magnesium ions to achieve selective separation of zinc and magnesium; directly adds concentrated sulfuric acid to the filtrate (about 30 ml) after the precipitation of zinc and magnesium (the purpose is not to significantly increase the volume of the filtrate), dissolves the zinc oxide obtained after calcining zinc citrate, ensures the recovery rate of zinc ions, and obtains 35-40 mL of zinc sulfate solution (the concentration and purity of the zinc sulfate solution can be guaranteed). The filtrate of the original mixed system is fully utilized, the overall process does not generate any waste liquid and solid waste to the outside, the overall solution volume does not increase significantly, and a large amount of volume loading is not required. A relatively pure magnesium precipitate and a zinc sulfate solution with a high concentration and excellent purity are obtained, and no additional treatment of other products is required, and the added value is extremely high.

[0049] Therefore, when the precipitant is citric acid, the molar ratio is 1-1.5:1, the pH is 2.0-4.0, and the calcination temperature is above 400°C, the zinc precipitation rate and recovery rate are high, and the magnesium inclusion rate is low.

[0050] In summary, the present invention discloses a method for selectively precipitating and separating zinc and magnesium, comprising the following steps: first, adding a citric acid precipitant to a solution containing zinc and magnesium and adjusting the pH, and then performing solid-liquid separation to obtain zinc citrate solid and a magnesium-containing filtrate; then, adding a magnesium removal agent to the magnesium-containing filtrate and performing solid-liquid separation, and adding concentrated sulfuric acid to the filtrate; finally, calcining the zinc citrate to obtain zinc oxide, and then adding the zinc oxide to the filtrate supplemented with concentrated sulfuric acid to obtain a zinc sulfate solution by acid leaching. The present invention achieves the separation of zinc and magnesium by different pH values ​​when zinc citrate and magnesium citrate are precipitated. The present invention is green and environmentally friendly, has a simple process, is conducive to the separation of zinc and magnesium in a hydrometallurgical zinc smelting system, and has a good application prospect.

[0051] At this point, those skilled in the art recognize that, although the embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the contents disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all such other variations or modifications.

Claims

1. A method for selectively precipitating and separating zinc and magnesium, characterized in that: The method comprises the following steps: Step S1: adding a citric acid precipitant to a mixed solution containing zinc and magnesium, adjusting the pH value, and performing solid-liquid separation after sufficient precipitation to obtain a zinc precipitate and a magnesium-containing filtrate; Step S2: calcining the zinc precipitate obtained in step S1 to obtain zinc oxide; Step S3: adding a magnesium removal agent to the magnesium-containing filtrate obtained in step S1, and performing solid-liquid separation after sufficient precipitation to obtain a magnesium precipitate and a pure filtrate, and adding concentrated sulfuric acid to the pure filtrate; Step S4: adding the zinc oxide obtained in step S2 to the pure filtrate supplemented with concentrated sulfuric acid obtained in step S3; obtaining a zinc sulfate solution through acid leaching to complete the selective zinc-magnesium separation of the zinc-magnesium mixed solution.

2. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: The solution containing zinc and magnesium in step S1 has a zinc content of 130-150 g / L and a magnesium content of 10-15 g / L.

3. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: The citric acid precipitant in step S1 includes at least one of citric acid, sodium citrate and potassium citrate.

4. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: In step S1, the ratio of the amount of the zinc ion substance to the amount of the citric acid precipitant substance is 1-1.5:

1.

5. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: In step S1, a sodium hydroxide solution is used to adjust the pH value.

6. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: In the step S1, the pH value is adjusted to 2.0-4.

0.

7. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: The reaction conditions in step S1 are 500-600 rpm, 60-80° C., and heating in a water bath for 1-2 h.

8. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: The calcination gas environment in step S2 is air, the calcination temperature is greater than 400° C., and the time is 1-2 hours.

9. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: The magnesium removal reagent in step S3 comprises at least one of conventional magnesium removal agents such as sodium hydroxide and sodium phosphate; the concentration of concentrated sulfuric acid is 18 mol / L, and the concentration of sulfuric acid in the pure filtrate solution after adding concentrated sulfuric acid is 2-3 mol / L.

10. A method for selectively precipitating and separating zinc and magnesium as claimed in claim 1, characterized in that: The acid leaching liquid in step S4 is sulfuric acid, with a liquid-to-solid ratio of 4-6 mL:1 g, and the end point pH value of the solution is controlled to be 2.0-3.0; the acid leaching conditions are 500-600 rpm, and heating in a water bath at 60-80° C. for 1-2 h.