Steel for base plate of aluminum-coated plate strip for high-strength corrosion-resistant structure and production method of steel
By optimizing the chemical composition and organizational structure of the steel used for the base plate of aluminum-clad panels and strips, the problems of insufficient strength and bonding performance in the existing technology are solved, and the production of aluminum-clad panels and strips with high strength and good surface quality is achieved to meet the requirements of high-strength corrosion-resistant structures. need.
Patent Information
- Application Number
- CN202310328400.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-30
AI Technical Summary
The strength and steel-aluminum bonding properties of the steel used for existing aluminum-clad panels and strip substrates are insufficient, resulting in defects such as peeling and slag inclusions during the production process, which increases the difficulty of billet cleaning and production costs, and is difficult to meet the needs of high-strength, corrosion-resistant structures. .
By optimizing the chemical composition design, controlling the content of C, Si, Mn, P, S, Al, N, O and other elements, combined with the addition of Ti, Nb, Cu, Cr, Ca and other alloying elements, a uniform ferrite+ is formed. A small amount of bainite structure satisfies specific composition relationships to improve yield strength, tensile strength and steel-aluminum bonding properties.
It achieves yield strength ≥300MPa and tensile strength ≥360MPa, eliminates surface warping and slag inclusion defects, improves steel-aluminum bonding performance and surface quality, and is suitable for the production of aluminum-clad plates and strips with high-strength corrosion-resistant structures.
Smart Images

Figure CN118726831A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of low alloy steel manufacturing, and specifically relates to a steel for an aluminum-clad plate strip substrate for a high-strength corrosion-resistant structure and a production method thereof. Background Art
[0002] Aluminum-clad strip is a composite strip formed by rolling and deforming the aluminum layer on the surface of the strip at room temperature. It has both steel-aluminum structure and steel-aluminum-steel or aluminum-steel-aluminum structure. Aluminum-clad strip has the strength of steel and the characteristics of aluminum such as good heat dissipation, corrosion resistance, light weight and beautiful appearance. Compared with pure aluminum materials, it greatly reduces the cost, so it is widely used in radiators, corrosion-resistant pipes, home appliance panels and other fields, and gradually expanded to automobile engine protective covers, new energy vehicle parts, atmospheric corrosion resistance, cookers, construction and other fields.
[0003] In order to extend the service life, existing container plates mostly use weathering steel, and its composition system needs to add many corrosion-resistant alloy elements; at the same time, in order to achieve high strength and weight reduction, some strengthening elements such as Ti and Nb need to be added, which significantly increases the cost. At the same time, weathering steel is overall corrosion-resistant, and steel structure corrosion mainly occurs on the surface of the material. The many corrosion-resistant alloys added inside the steel plate cannot fully play their role, which is also a waste of resources.
[0004] Aluminum is not only light, beautiful, and has good heat dissipation, but also has excellent atmospheric corrosion resistance in atmospheric environments. Aluminum is an active metal that easily reacts chemically with oxygen in the air to form aluminum oxide, forming a dense film of micron thickness on the surface to prevent corrosion from deepening. In industrial atmospheric environments, the corrosion rate of aluminum is about 1μm / a, and its corrosion resistance is about 10 times that of conventional atmospheric corrosion-resistant steel. In addition, the surface is beautiful, so the surface of aluminum does not need to be painted, reducing the painting process, which not only reduces costs, but is also more energy-saving and environmentally friendly.
[0005] With the development and application of aluminum-clad steel strips, numerous patents for composite plates and strips and steel for their base plates have been developed.
[0006] Chinese patent CN102019727 discloses "aluminum-clad steel strip for cooler, preparation method thereof, and steel strip and aluminum alloy strip used therein". The patent introduces a method for producing composite strips. Although the substrate used is mentioned, it is mainly used to produce aluminum-clad strips with a thickness of about 1.5 mm, and its yield strength is relatively low.
[0007] The steel used in the production of aluminum-clad strips deforms together with the aluminum layer during the production process, so it is required to have strength and plasticity comparable to aluminum, especially excellent plasticity, and good steel-aluminum bonding performance, and has specific requirements on composition. Therefore, existing conventional low-strength steel is difficult to use in the production of aluminum-clad strips.
[0008] Japanese patent JP2005281806 discloses "Low yield point steel with excellent toughness and its production method". The steel disclosed belongs to low alloy structural steel with low yield strength and high elongation, and the yield strength is generally around 200MPa. The resulting product is generally a thick plate product. In terms of composition design, one or more components of alloys such as chromium (Cr), molybdenum (Mo), nickel (Ni), copper (Cu), and boron (B) are added based on low carbon (C)-silicon (Si)-manganese (Mn). The strength of the resulting steel is low, and there is no mention of aluminum coating performance. It is mainly used for the production of seismic dampers.
[0009] The Chinese patent CN111349869A discloses "a kind of high-strength steel for aluminum-clad substrate and its production method", and the obtained steel has a yield strength of 210-290MPa, a tensile strength of ≥320MPa, and an elongation of ≥40%, which is lower than the strength of the present invention. By adding a higher content of P element, the diffusion of Al is inhibited, thereby improving the steel-aluminum bonding performance, but the steel involved is used for the production of aluminum-clad materials, and there is still an iron-aluminum compound layer with a thickness of no more than 5μm at the steel-aluminum interface, and the excessively high P content is prone to cold brittleness problems, which is not conducive to the forming and welding performance of the steel plate. However, the steel composition contains a higher O (oxygen), which will lead to more defects such as pores and slag inclusions inside and on the surface of the ingot, increase the difficulty of cleaning the ingot, make the strip surface prone to warping defects, and reduce the yield rate.
[0010] The "high-strength aluminum-clad strip and its manufacturing method" disclosed in Chinese patent CN107881426A ensures the steel-aluminum bonding performance through N, O and controlled Si, Al, and has a yield strength of 280-400MPa, and is mainly used in the production of radiators, home appliance panels, etc. However, the steel composition contains a high O (oxygen), which will lead to more defects such as pores and slag inclusions inside and on the surface of the ingot, increase the difficulty of cleaning the ingot, make the strip surface prone to warping defects, and reduce the yield rate.
[0011] Chinese patent CN114250411A discloses "a steel with aluminum-clad plate for kitchenware and its production method". Although the steel plate involves nitriding process, its yield and tensile strengths do not exceed 280MPa and 380MPa respectively. At the same time, the patent requires that the carbon content be controlled below 0.005%, and the P and S contents are limited to no more than 0.012% and 0.006% respectively, which increases the difficulty of steelmaking and production costs. The patent mainly improves the strength during nitriding through the precipitation strengthening of V and Mo. In terms of function, the steel is limited to the processing of aluminum-clad materials for frying pans, and is not suitable for the production of other aluminum-clad materials with high strength requirements.
[0012] From the comparison with the existing patents, it can be found that the steel used for the existing aluminum-clad plate substrate is either low in strength, or has poor steel-aluminum bonding performance, or has poor surface quality of the ingot, which increases the difficulty of cleaning the ingot. Summary of the invention
[0013] The purpose of the present invention is to provide a steel for a substrate of an aluminum-clad plate with high strength and corrosion resistance, and a production method thereof, wherein the steel has a yield strength ≥300MPa, a tensile strength ≥360MPa, and an elongation ≥30%, and has excellent plasticity, aluminum-clad performance, high strength, and high surface quality, and eliminates defects such as surface warping and slag inclusions. The aluminum-clad plate produced by the steel has excellent surface quality and high strength, and is mainly used for the production of aluminum-clad plates with high strength and corrosion resistance.
[0014] To achieve the above object, the technical solution of the present invention is:
[0015] A steel for a high-strength corrosion-resistant structure aluminum-clad plate strip substrate, the chemical composition weight percentage of which is: C: 0.04-0.09%, 0 < Si ≤ 0.005%, Mn: 0.4-0.8%, P: 0.008-0.020%, S ≤ 0.008%, 0 < Al ≤ 0.005%, N: 0.012-0.030%, 0 < O ≤ 0.01%, B: 0.0005-0.002%, and one or more of Ti: 0.01-0.06%, Nb: 0.01-0.03%, Cu: 0.01-0.15%, Cr: 0.03-0.60%, Ca: 0.001-0.004% are selectively added, and the balance contains Fe and other unavoidable impurities; and at the same time,
[0016] 0.5C+3.83N+O-0.89Al-1.15Si≥0.08;
[0017] 150(C-0.01)+60P+300N+5Mn≥13.0.
[0018] Furthermore, the balance is Fe and other inevitable impurities.
[0019] The microstructure of the steel for the aluminum-clad plate strip substrate of the present invention is a uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%.
[0020] The steel used for the aluminum-clad plate strip substrate of the present invention has a yield strength of ≥300MPa, a tensile strength of ≥360MPa, and an elongation of ≥30%.
[0021] The steel for the aluminum-clad plate strip substrate for high-strength corrosion-resistant structure of the present invention requires a yield strength and a tensile strength of respectively over 300 MPa and 360 MPa, an elongation of over 30%, and good steel-aluminum bonding performance, excellent plasticity, aluminum-cladding performance and high strength, good surface quality, and elimination of surface warping, slag inclusion and other defects. For this reason, the content of specific alloy elements must be limited as much as possible.
[0022] In the chemical composition design of the steel for the aluminum-clad plate strip substrate of the present invention:
[0023] C improves yield strength through solid solution strengthening and phase transformation strengthening, while inhibiting the diffusion of Al in steel and the formation of iron-aluminum compounds. Too high C content is not good for the subsequent processing properties of the material such as stamping and drawing; however, higher C is easy to be concentrated at defective positions such as dislocations, which is not good for surface quality. According to the actual steelmaking process, the present invention controls the C content to 0.04-0.09%.
[0024] Si is a deoxidizing element and also a solid solution strengthening element, which increases the yield strength and reduces the elongation. Although an appropriate amount of Si is beneficial to improving the steel-aluminum interface bonding performance, it will also weaken the inhibitory effect of O (oxygen) on the formation of a brittle compound layer at the steel-aluminum interface. Therefore, the present invention controls 0<Si≤0.005%.
[0025] Mn is also a common strengthening element in steel. It increases yield strength and reduces elongation through solid solution strengthening. An appropriate amount of Mn can combine with S in steel to form MnS, reducing the hot brittleness of steel. However, excessive Mn solid solution hinders the recovery of the structure and inhibits the growth of recrystallized grains, reducing the γ texture (ND∥ <111> ) strength, which is very unfavorable for the stamping forming of steel plates and will also increase costs, so the present invention controls its content to 0.40-0.80%.
[0026] P is generally controlled as an impurity element in steel, and is only allowed to be added in a few special-purpose steels. For example, adding no more than 0.15% P to sulfur-containing free-cutting steel makes it solid-dissolved in ferrite, causing strengthening and embrittlement to improve its cutting performance. In addition, P is the main corrosion-resistant element in traditional atmospheric corrosion-resistant steel. P in steel can accelerate the uniform dissolution of steel and Fe 2+ The oxidation rate is high, which helps to form a uniform FeOOH rust layer on the steel surface and promotes the formation of amorphous iron oxyhydroxide FeO x (OH) 3-2xDense protective film effectively improves the atmospheric corrosion resistance of steel. Generally, the corrosion resistance is best when the P content is 0.08% to 0.15%, so P was added as a corrosion-resistant element in some early atmospheric corrosion-resistant steels. However, too much P causes "cold brittleness" of steel, reduces plasticity and impact toughness, and deteriorates the welding performance and cold bending performance of steel, so the amount of addition is clearly limited for steel types with requirements for low-temperature impact toughness or high forming performance. In recent years, some atmospheric corrosion-resistant steels have also reduced the P content and selected other alternative corrosion-resistant elements to ensure corrosion resistance, and even controlled it as an impurity element, requiring the content to be ≤0.015%, but controlling the P content at such a low level will increase the difficulty of steelmaking and increase manufacturing costs. The present invention considers that P improves the strength of steel for aluminum-clad plates and strips by solid solution strengthening, phase transformation strengthening, etc., and uses it to improve the steel-aluminum bonding performance. Therefore, 0.008 to 0.020% of P is added in the present invention.
[0027] S is detrimental to the performance of steel, and can easily cause "hot brittleness" of steel, reduce the low-temperature toughness of steel, and deteriorate the steel-aluminum interface bonding performance. The addition of Mn can form MnS with S, and increasing the Mn / S ratio can improve hot ductility. It is required to control its content at a minimum level. Considering that too low a controlled content increases the difficulty of steelmaking and production costs, the present invention requires that the S content be controlled below 0.008%.
[0028] Al is an important deoxidizing element in steel, but a higher Al content is easy to diffuse to the steel-aluminum bonding interface, deteriorating the interface bonding strength. Therefore, its content must be controlled within a certain range, so the present invention controls 0<Al≤0.005%.
[0029] B is a very active element in steel, and it is easy to form compounds with C and N. At the same time, B is easy to segregate at austenite grain boundaries and dislocations, thereby suppressing the segregation of other interstitial atoms there. Moreover, the segregation of B does not hinder the movement of dislocations, making the strain uniform, improving the plasticity of the material, and being beneficial to improving the rolling performance of aluminum cladding; B significantly improves the hardenability, and a trace amount of B can effectively improve the strength of steel. However, too high a content of B is likely to promote the improvement of hardenability, resulting in excessive strength and reduced stamping performance, so the present invention controls its content to 0.0005-0.002%.
[0030] N can form AlN particles with Al in steel, thereby binding Al and limiting the diffusion of Al in steel. At the same time, N, like C, is easy to aggregate at dislocations to form Coriolis gas clusters, resulting in strain concentration, causing strain unevenness in the aluminum-clad material during processing, affecting the surface quality, and too high N also deteriorates impact toughness, so the present invention controls its content to 0.012-0.030%.
[0031] Oxygen (O) can inhibit the adverse effect of Al in steel on aluminum coating performance, so it is required to add a certain amount of O. However, too much oxygen will produce subcutaneous bubbles, looseness and other defects, and aggravate the thermal brittleness of sulfur, making it easy for the strip surface to have defects such as warping and slag inclusion. During the solidification process of steel, oxygen will precipitate in large quantities in the form of oxides, reducing the plasticity and impact toughness of the steel. Therefore, the O content is controlled to be ≤0.01% and less than 0.01%.
[0032] In addition to the above elements, the present invention also requires the addition of one or more of Ti: 0.01-0.06%, Nb: 0.01-0.03%, Cu: 0.01-0.15%, Cr: 0.03-0.60%, Ca: 0.001-0.004%, so as to further improve the room temperature strength and the strength after heat treatment. Among them:
[0033] Cr forms a continuous solid solution with Fe in steel, which has a solid solution strengthening effect, and forms various types of carbides with C, such as M3C, M7C3 and M 23 C6, etc., produce a secondary strengthening effect. At the same time, the addition of Cr is beneficial to inhibit the diffusion of Al and improve the steel-aluminum bonding performance. Higher Cr is not good for toughness and increases the difficulty of welding. Cr is a precious alloy element, so the present invention controls its content to 0.03-0.6%.
[0034] Cu has solid solution and precipitation strengthening effects. When the content is high, tempering at an appropriate temperature has a secondary hardening effect, thereby improving the strength. At the same time, the addition of Cu is also beneficial to improving the steel-aluminum bonding performance. Too much Cu causes cracks in the steel billet during heating and hot rolling, deteriorating the surface properties, so the present invention controls the Cu content to 0.01-0.15%.
[0035] Nb is a strong nitrogen carbide-forming element. During the cooling process after rolling, it can combine with carbon and nitrogen in steel to form intermediate phases such as NbC, Nb(CN) and NbN. The fine carbide particles formed can refine the structure, produce fine grain strengthening and precipitation strengthening, and significantly improve the strength of the steel. In addition, Nb can inhibit the expansion of the austenite interface, increase the recrystallization temperature of the steel, and achieve non-recrystallization zone rolling at a higher temperature. Therefore, adding an appropriate amount of Nb to the steel is beneficial to improving the strength, but the effect of improving the strength will no longer increase after exceeding 0.06%. When the Nb content is high, coarse carbonitride particles are formed at the grain boundary, which deteriorates the impact toughness. It can be added selectively, and its content needs to be controlled to be 0.01-0.03%.
[0036] Ti has high chemical activity and is easy to form compounds with C, N, O, S, etc. and precipitate during rolling and cooling to increase strength; at the same time, fine precipitates can pin the grain boundaries, thereby refining the austenite grains and preventing the grain growth in the welding heat affected zone, improving the welding performance of the steel. The composite addition of Ti and B can significantly reduce the temper brittleness. When the Ti content is too high, the titanium nitride particles are easy to grow and agglomerate at high temperatures, which damages the plasticity and toughness of the steel. Therefore, it needs to be controlled at 0.01-0.06%.
[0037] Ca added to steel can change the shape of sulfides, inhibit the hot brittleness of S, and improve toughness. Moreover, when there is excessive Ti in the steel, it can form titanium sulfide or titanium carbosulfide with sulfides. The effect is not obvious when the Ca content is too low. When the content exceeds 0.005%, the size of Ca(O,S) formed is too large, and the brittleness is also increased, which can become the starting point of fracture cracks. At the same time, the purity of steel is reduced and the toughness of the welding heat affected zone is deteriorated. Therefore, the present invention limits its content to 0.001-0.004%.
[0038] The aluminum-clad plate strip substrate steel of the present invention is required to have high surface quality, high strength and good steel-aluminum bonding performance to meet the use requirements of more application fields, and its yield strength is required to be controlled to be ≥300MPa and tensile strength ≥360MPa. In order to meet the above performance requirements, the present invention strictly designs the composition according to the influence of different alloy elements on the above performance, and achieves the performance requirements through the comprehensive effect of multiple elements. Among them, the addition of C has solid solution strengthening and phase transformation strengthening effects. The existing aluminum-clad steel (such as Chinese patent CN114250411A) generally controls C≤0.005% to ensure plasticity, which greatly increases the difficulty of steelmaking. In order to ensure high strength after nitriding treatment, the present invention requires the yield strength of the substrate steel to be above 300MPa, so 0.04-0.09% C is used. On the one hand, it plays a role of solid solution strengthening, and at the same time, in the steel production process, by controlling rolling and controlling post-rolling cooling, a ferrite + a small amount of bainite structure is formed in the steel, which plays a phase transformation strengthening role and improves strength.
[0039] Since the aluminum-clad strip undergoes annealing heat treatment during production, conventional fine grain strengthening means have little effect after heat treatment, while solid solution strengthening is not limited by heat treatment, so the higher the steel strength, the higher the strength of the finished aluminum-clad material. For this reason, the present invention adds 0.4-0.8% Mn to ensure steel strength through solid solution strengthening of Mn.
[0040] In the present invention, the P content is controlled at 0.008-0.020%. P is usually controlled as an impurity element in steel, so it is hoped that its content is as low as possible, and is generally required to be controlled below 0.015% or even lower. However, the lower the P content, the higher the steelmaking cost and the greater the difficulty. Since P is an element of the same family as N, appropriate P is beneficial to the steel-aluminum bonding performance, but the research of the present invention has found that its improvement effect on the steel-aluminum bonding performance is not linear. When the P content exceeds 0.020%, the steel-aluminum bonding performance begins to deteriorate. Therefore, considering the difficulty, cost and performance requirements of steelmaking, the upper limit of P control is relaxed to 0.020%, which ensures the steel-aluminum bonding performance on the one hand, while improving the strength and reducing the steelmaking cost.
[0041] In addition to solid solution strengthening, Cr in the steel of the present invention also has a secondary strengthening effect. Cu also has a solid solution strengthening effect in the steel and can precipitate strengthening to improve strength during heat treatment. Nb, V and Ti precipitate fine carbonitrides during rolling and cooling to strengthen the matrix.
[0042] According to the strengthening effect of the above elements on steel, it is required to control the contents of C, P, N and Mn in the steel to satisfy the relationship 1: 150(C-0.01)+60P+300N+5Mn≥13.0. If the value of the relationship is lower than 13.0, the problem of low strength is likely to occur.
[0043] The key to the steel-aluminum bonding performance is to control the formation of brittle iron-aluminum compounds at the steel-aluminum interface in the aluminum-clad material. The formation of iron-aluminum compounds is closely related to the diffusion of Al in steel. Controlling the diffusion of Al can inhibit the formation of iron-aluminum compounds within a certain temperature range. The research of the present invention shows that the steel-aluminum bonding performance is further improved through the synergistic effect of C, Cu, O, N and other elements, while O (oxygen) and N can inhibit the diffusion of Al and reduce the formation of brittle iron-aluminum compounds, thereby improving the steel-aluminum bonding performance. However, too high O will cause defects such as subcutaneous bubbles and looseness in the ingot, and aggravate the hot brittleness of sulfur, making it easy for defects such as warping and slag inclusion to appear on the steel surface. Therefore, the O content is limited to ≤0.01% in the present invention, and 0.012-0.03% N is used to ensure the steel-aluminum bonding performance. Si and Al, as deoxidizing elements, hinder the improvement of O on the steel-aluminum bonding performance, so their content should be limited.
[0044] Therefore, the present invention obtains good steel-aluminum bonding performance through the synergistic effect of multiple elements such as C, Mn, Si, Al, O, and N. According to the strength of the effect of C, N, O and Al, Si on the steel-aluminum bonding performance, their contents are required to satisfy the relationship 2: 0.5C+3.83N+O-0.89Al-1.15Si≥0.08, so as to ensure that the steel has excellent steel-aluminum bonding performance. If the relationship value is lower than 0.08, steel-aluminum stratification is likely to occur.
[0045] In general, the present invention adopts the above-designed component system, comprehensively considering the requirements of surface quality, steel-aluminum bonding performance and high strength, and through the joint action of various elements, an invented steel type that meets the performance requirements can be obtained.
[0046] The production method of the steel for the aluminum-clad plate strip substrate for high-strength corrosion-resistant structure of the present invention comprises the following steps:
[0047] 1) Smelting
[0048] According to the above composition, the molten iron is pretreated, blown in a converter, refined outside the furnace, and cast into a slab;
[0049] 2) Reheating and controlled rolling
[0050] The thickness of the steel strip after rolling is greater than 2.5mm, the heating temperature is ≥1230℃, the rough rolling end temperature is above 1050℃; the finishing rolling start temperature is above 980℃, and the finishing rolling end temperature is 860~900℃;
[0051] The thickness of the steel strip after rolling is ≤2.5mm, the heating temperature is ≥1100℃, the rough rolling end temperature is above 900℃, and the cumulative deformation in the rough rolling stage is ≥80%; the finishing rolling start temperature is 790~850℃, and the finishing rolling end temperature is 710~750℃;
[0052] 3) Control cooling, cooling rate above 20℃ / s;
[0053] 4) Coiling: coiling temperature 550~610℃.
[0054] Preferably, the slab obtained in step 1) is machine cleaned.
[0055] Preferably, in step 2) controlled rolling, the side pressure in the rough rolling stage is controlled within 50 mm.
[0056] In the production method of the present invention:
[0057] Pretreatment of molten iron to remove P and S to ensure low P and S content in steel; top and bottom composite blowing in converter to control C content.
[0058] The function of machine cleaning after continuous casting is to eliminate surface defects of the ingot, reduce slag inclusions, warping, pits, scars and other defects on the strip surface, improve the surface quality of the strip, and reduce surface defects of the finished aluminum-clad materials.
[0059] The present invention formulates a rolling process according to the phase change temperature curve of the steel grade and combines the target performance to determine the temperature control parameters of the steel rolling process. The present invention relates to a steel grade with a low alloy content and a continuous cooling curve such as Figure 1As shown in the figure, it can be seen that the starting temperature of the ferrite phase transformation of the steel is 852℃, pearlite begins to form after the temperature drops to 698℃, and the starting temperature of the bainite phase transformation is 653℃. When the cooling rate is above 1℃ / s, only ferrite and bainite are formed.
[0060] According to different thickness specifications, the present invention designs two rolling processes for the steel. For steel strips with a thickness greater than 2.5 mm, a conventional austenite rolling process is used; and for steel strips with a thickness less than 2.5 mm, a ferrite rolling process is selected to obtain a good plate shape and higher strength.
[0061] According to the composition calculation of the steel grade of the present invention, the Ar3 temperature of the steel grade is 857°C, and the ferrite phase transformation starting temperature is 852°C. Therefore, during the austenite rolling process, it is required to control the finishing temperature above 860°C. If the finishing temperature is too high, a higher heating temperature is required, which increases energy consumption and oxidation of the steel strip. Therefore, the upper limit of the finishing temperature is set to not exceed 900°C. Correspondingly, the finishing entrance temperature is required to be 980°C, and the rough rolling end temperature is required to be above 1050°C. In order to ensure the rough rolling end temperature, and considering the dissolution behavior of micro-alloying element carbonitride in austenite and the growth behavior of austenite grains during heating, it is required to control the heating temperature above 1230°C.
[0062] When the thickness of the steel strip is below 2.5mm, the deformation resistance of the steel strip in the high-temperature austenite zone of 860-900℃ is low, and the strip is prone to breakage, local stretching and lateral bending at the outlet of the finishing mill. For this reason, the present invention adopts the ferrite rolling process for production. On the one hand, the strength of the steel strip is higher at a lower temperature, and the steel strip is not easy to deform under the same coiling tension, thereby reducing the occurrence of narrowing and rolling breakage. At the same time, higher strength also allows higher coiling tension, thereby improving the plate shape and reducing the occurrence of lateral bending. Ferrite rolling requires that the entire finishing deformation is carried out in the ferrite zone, so the starting temperature of the finishing rolling is controlled not to be higher than 850℃, and the ending temperature is controlled not to be lower than 710℃. If the starting temperature of the finishing rolling is too low, the thermal deformation resistance is high, the rolling load of the final stand is increased, and the energy consumption is increased; if it is too high, it is easy to enter the austenite and ferrite two-phase zone, and mixed crystals are easily formed in the matrix, causing rolling force fluctuations, which is not conducive to the thickness control and plate shape of the steel strip. Therefore, the start temperature of finishing rolling is set at 790-850℃ and the end temperature of finishing rolling is set at 710-750℃ during the ferrite rolling process. According to the start temperature of finishing rolling, considering the temperature drop of the intermediate billet on the roller, the end temperature of rough rolling is required to be above 900℃, and the corresponding billet heating temperature is controlled above 1100℃. In addition, in order to ensure the effect of recrystallization and grain refinement, the cumulative deformation in the rough rolling stage is required to be ≥80%.
[0063] In order to obtain high strength, the steel of the present invention selectively adds one or more of Cu, Cr, Nb, V and Ti. The solid solubility of copper in steel is limited and decreases rapidly with the decrease of temperature. At high temperature, Cu dissolved in austenite precipitates in the form of fine ε-Cu and disperses in the matrix. Its twin structure and pinning effect on dislocations improve the strength of the steel. Studies have shown that Cu precipitates are formed at 650°C, and the lower the temperature, the smaller the size of the precipitates; the best precipitation strengthening effect is achieved at 500°C, so the lower limit of the coiling temperature cannot be lower than 500°C. Figure 2 From the TTT curve, 581℃ is the fastest temperature for bainite transformation. The structure of the steel of the present invention is mainly equiaxed ferrite. In order to obtain higher strength, it is hoped that there is a certain amount of bainite structure in the matrix, so the coiling temperature is controlled at about 580℃. The carbonitrides of Nb, V and Ti selected for addition also have a good precipitation strengthening effect near this temperature, so the coiling temperature is set to 550~610℃ by comprehensively considering the precipitation strengthening and phase transformation strengthening effects.
[0064] In order to obtain the target performance, the steel matrix structure is controlled to be a uniform equiaxed ferrite structure, and a small amount of bainite structure is allowed to form. Figure 1 It can be seen that the ferrite + a small amount of bainite structure can be obtained when the cooling rate is above 1°C / s; considering that rapid cooling can refine the structure and increase the phase transformation rate, the post-rolling cooling rate of the steel type involved in the present invention is controlled to be above 20°C / s.
[0065] In order to obtain good surface quality, the side pressure in the rough rolling stage is controlled within 50mm. At the same time, it is required that there should be no defects such as pores and scars at the corners of the billet.
[0066] In order to suppress the abnormal growth of ferrite grains in the steel after final rolling and ensure that the steel structure is a uniform equiaxed ferrite + bainite structure, the post-rolling cooling is required to adopt a front cooling method. That is, the steel is immediately intensively cooled after leaving the hot rolling unit. The process of the present invention can obtain a uniform ferrite + a small amount of bainite structure, and the specific requirement is that the bainite content is ≤20%. Too high a bainite content will lead to insufficient plasticity and increase the difficulty of aluminum cladding rolling.
[0067] The present invention has the following advantages:
[0068] 1. The present invention improves the strength of steel by solid solution strengthening and phase transformation strengthening, adopts a simple C-Mn design in the composition design, and controls the contents of C, P, N and Mn to satisfy the relationship: 150(C-0.01)+60P+300N+5Mn≥13.0, thereby obtaining higher strength. Its yield strength is ≥300MPa and tensile strength is ≥360MPa, and it is mainly used for the production of high-strength corrosion-resistant structural aluminum-clad plates and strips.
[0069] 2. In order to obtain higher steel-aluminum bonding performance, the present invention requires that the contents of C, Mn, Si, Al, O, and N satisfy the relationship: 0.5C+3.83N+O-0.89Al-1.15Si≥0.08 according to the effects of C, Mn, Si, Al, O, and N on the steel-aluminum bonding performance in the composition design, so as to inhibit the formation of brittle iron-aluminum compounds at the steel-aluminum interface, thereby ensuring that the steel plate obtains good steel-aluminum bonding performance.
[0070] 3. The present invention adopts a low-oxygen and high-nitrogen composition design, limiting the O content to ≤0.01%, and using 0.012-0.030% N to compensate for the steel-aluminum bonding performance, thereby solving the subcutaneous bubbles, looseness and other defects of the high-oxygen composition ingot, reducing the occurrence of defects such as steel surface, warping, slag inclusions, and improving the surface quality.
[0071] 4. The present invention controls the P content to 0.008-0.020%, utilizes the solid solution strengthening effect of P and its influence on the steel-aluminum bonding performance, further improves the steel-aluminum bonding performance, and at the same time reduces the difficulty and cost of steelmaking, and has higher production efficiency.
[0072] 5. In terms of process control, the present invention adopts austenite rolling and ferrite rolling processes respectively for different ingot thicknesses obtained after rolling, so that the steel plate can obtain high strength while significantly improving the shape of thin-gauge steel strips, reducing the occurrence of problems such as strip narrowing, strip breaking and side bending during rolling. The production process is simple, the cost is low, and it is suitable for large-scale production of enterprises.
[0073] 6. The process of the present invention adopts different controlled rolling processes, combined with a coiling temperature of 550-610°C and a cooling rate after rolling ≥20°C / s, so that the obtained steel plate structure is uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%. The obtained steel plate has good deformation ability and can meet the deformation requirements of more than 80% of aluminum cladding rolling, as well as the stamping and drawing deformation in the subsequent processing process. No annealing is required in the middle, which reduces the production process and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] Figure 1 It is a schematic diagram of the static CCT curve (calculation) of the steel grade of the present invention.
[0075] Figure 2 It is a schematic diagram of the static TTT curve (calculation) of the steel grade of the present invention.
[0076] Figure 3 This is a typical matrix structure photo of the steel in Example 1 of the present invention. DETAILED DESCRIPTION
[0077] The present invention will be further described below in conjunction with the embodiments and drawings.
[0078] The embodiment of the present invention adopts steelmaking in a 500kg vacuum induction furnace. The chemical composition of the embodiment steel is shown in Table 1, the specific process parameters are shown in Table 2, and the mechanical properties of the embodiment steel are shown in Table 3.
[0079] Depend on Figure 3 It can be seen that the microstructure of the steel plate obtained by using the composition and process of the present invention is a uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%.
[0080] The composition, production process and performance of similar steel grades were compared.
[0081] Comparative steel 1 is Chinese patent CN101514426A "Low yield point steel for earthquake resistance of buildings with yield strength of 100 MPa and its production method", which has high Si and Al contents and does not contain O.
[0082] Comparative steel 2 is Chinese patent CN101525720 "A new type of special substrate for preparing aluminum-clad steel strip", and the alloy composition is too high.
[0083] Comparative steel 3 is Chinese patent CN111349869A "A high-strength aluminum-clad substrate steel and its production method", with 0.018-0.03% P added to the composition. An iron-aluminum compound layer with a thickness of no more than 5μm appeared at the steel-aluminum interface, and the steel-aluminum bonding performance was reduced. At the same time, the strength was low, and its composition contained a high oxygen content, which was detrimental to the surface quality of the ingot and strip steel, increased the production difficulty, and affected the yield rate.
[0084] Comparative steel 4 is Chinese patent CN107881426A "A high-strength aluminum-clad strip and its manufacturing method", and its higher oxygen content is not good for the surface quality of the ingot and strip, increases the difficulty of production, and affects the yield rate.
[0085] The steel of the present invention has obvious differences in composition from the four comparative steels. In order to ensure good steel-aluminum bonding performance, high strength and good surface quality, the steel of the present invention has a specially designed composition system.
[0086] Among the above four comparison steels, comparison steels 1 and 2 contain relatively high Al and extremely high P, S, N, etc., without considering the steel-aluminum bonding performance; comparison steel 3 explicitly adds P, which is unfavorable to the steel-aluminum bonding performance and has low strength; comparison steel 4 involves an aluminum-clad plate and strip, without considering the influence of O content on surface quality, so the comparison steel is significantly different from the steel of the present invention in composition.
[0087] From the performance point of view, comparison steels 1 and 2 are only required to have lower yield strength and higher elongation, while the steel of the present invention, in addition to the above requirements, also explicitly requires that the steel has good aluminum coating performance and is suitable for the production of aluminum-clad strip steel without the need for annealing in the middle, which is also not available in comparison steel 2.
[0088] Although the comparative steels 3 and 4 also require aluminum coating performance, they are mainly used for the production of aluminum-coated strips such as radiators and home appliance panels, and the thickness of the aluminum layer on the surface does not exceed 0.1 mm. The steel type involved in the present invention has a wider application field, mainly used for the production of aluminum-coated strips for containers and other structures with high strength and corrosion resistance requirements, so there are significant differences in performance between the present invention steel and the comparative steel.
[0089] As can be seen from Table 3, the steel of the present invention has a stable yield strength. Under different rolling processes, the yield and tensile strengths of steel plates of various specifications are respectively above 300 MPa and 360 MPa, and have very high elongation. It is superior to the comparative steel grades in composition design and function, thus meeting the production requirements of aluminum-clad plates and strips with high elongation, good aluminum-clad performance, high surface quality and strong deformation ability.
[0090] In addition, the embodiments are only for illustration, and the thickness of the steel type described in the present invention is not limited thereto, and thinner or thicker strip steel can be produced within the range allowed by the equipment.
[0091]
[0092]
[0093]
Claims
1. A steel for aluminum-clad strip substrate for high-strength corrosion-resistant structure, the chemical composition weight percentage of which is: C: 0.04-0.09%, 0<Si≤0.005%, Mn: 0.4-0.8%, P: 0.008-0.020%, S≤0.008%, 0<Al≤0.005%, N: 0.012-0.030%, 0<O≤0.01%, B: 0.0005-0.002%, and one or more of Ti: 0.01-0.06%, Nb: 0.01-0.03%, Cu: 0.01-0.15%, Cr: 0.03-0.60%, Ca: 0.001-0.004% are selectively added, and the balance contains Fe and other unavoidable impurities; and at the same time, 0.5C+3.83N+O-0.89Al-1.15Si≥0.08; 150(C-0.01)+60P+300N+5Mn≥13.
0.
2. The high-strength corrosion-resistant structural aluminum-clad plate strip substrate steel according to claim 1, characterized in that: The balance is Fe and other inevitable impurities.
3. The high-strength corrosion-resistant structural aluminum-clad plate strip substrate steel according to claim 1 or 2, characterized in that: The microstructure of the steel for the aluminum-clad plate strip substrate is uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%.
4. The high-strength corrosion-resistant structural aluminum-clad plate strip substrate steel according to claim 1, 2 or 3, characterized in that: The yield strength of the steel used for the aluminum-clad plate strip substrate is ≥300MPa, the tensile strength is ≥360MPa, and the elongation is ≥30%.
5. The method for producing steel for high-strength corrosion-resistant structural aluminum-clad plate strip substrate according to any one of claims 1 to 4, characterized in that: The steps include: 1) Smelting The composition according to claim 1 or 2 is subjected to molten iron pretreatment, converter blowing, external refining, and casting into slabs; 2) Reheating and controlled rolling The thickness of the steel strip after rolling is greater than 2.5mm, the heating temperature is ≥1230℃, the rough rolling end temperature is above 1050℃; the finishing rolling start temperature is above 980℃, and the finishing rolling end temperature is 860~900℃; The thickness of the steel strip after rolling is ≤2.5mm, the heating temperature is ≥1100℃, the rough rolling end temperature is above 900℃, and the cumulative deformation in the rough rolling stage is ≥80%; the finishing rolling start temperature is 790~850℃, and the finishing rolling end temperature is 710~750℃; 3) Control cooling, the cooling rate is above 20℃ / s; 4) Coiling: coiling temperature 550~610℃.
6. The production method according to claim 5, characterized in that: The slab obtained in step 1) is machine cleaned.
7. The production method according to claim 5, characterized in that: Step 2) During the controlled rolling, the side pressure in the rough rolling stage is controlled within 50 mm.
8. The production method according to claim 5, characterized in that: The microstructure of the steel for the aluminum-clad plate strip substrate is uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%.
9. The production method according to claim 5 or 8, characterized in that: The yield strength of the steel used for the aluminum-clad plate strip substrate is ≥300MPa, the tensile strength is ≥360MPa, and the elongation is ≥30%.
Citation Information
Patent Citations
Novel special base metal strip for preparing feran
CN101525720A
Steel-aluminum composite board and preparation method thereof
CN102734625A
High-strength steel for aluminum-coated base plate and production method thereof
CN107881425A
High-strength aluminum-coated plate strip and production method thereof
CN107881426A
Method and device for preparing steel / aluminum laminated composite plate by hot continuous rolling with small rolling reduction
CN111014294A