Homogenizing heat treatment method capable of regulating and controlling second phase of aluminum alloy cast ingot

By setting different homogenization treatment systems according to the Cu content, the second phase of the 2324 aluminum alloy ingot is controlled, which solves the problem of alloy performance differences caused by differences in Cu content, realizes the homogenization heat treatment of the aluminum alloy ingot, and improves the quality of the finished plate. Strength and toughness, and save heat treatment costs.

CN118726869APending Publication Date: 2024-10-01BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410761230.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology fails to effectively control the homogenization heat treatment of the second phase of 2324 aluminum alloy ingots with different Cu contents, resulting in differences in alloy properties and difficulties in quality control of finished sheets.

Method used

According to different Cu contents, different homogenization treatment systems are set, including heating rate, temperature and holding time, and the type, quantity and size of the second phase in the ingot are controlled to ensure that the diffusion speed of Cu element is smaller than that of Mg element to achieve the second phase. The phase is fully redissolved.

Benefits of technology

It effectively regulates the second phase structure of the aluminum alloy ingot, ensures the smooth progress of subsequent deformation heat treatment, improves the strength and toughness of the finished plate, avoids over-burning and saves heat treatment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726869A_ABST
    Figure CN118726869A_ABST
Patent Text Reader

Abstract

The invention relates to a homogenizing heat treatment method capable of regulating and controlling a second phase of an aluminum alloy cast ingot, belongs to the technical field of aluminum alloy heat treatment, and particularly relates to a homogenizing heat treatment method for regulating and controlling the second phase of 2324 aluminum alloy cast ingots with different Cu contents, which can regulate and control the second phase of the 2324 alloy cast ingots with different Cu contents. Appropriate homogenization treatment systems including the heating rate, the homogenization treatment temperature and the homogenization treatment duration are set for 2324 alloy ingots with different Cu contents respectively, the type, the number and the size of second phases in microstructures of the homogenized ingots are regulated and controlled, and it is guaranteed that the subsequent deformation heat treatment process is conducted smoothly and the quality control of final finished plates is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aluminum alloy heat treatment, and in particular to a homogenizing heat treatment method capable of adjusting a second phase of an aluminum alloy ingot, and in particular to a homogenizing heat treatment method for a second phase of an aluminum alloy ingot with different Cu contents. Background Art

[0002] 2324 aluminum alloy has excellent properties such as high tensile strength, excellent fatigue crack growth resistance and fracture toughness, and is an important lightweight structural material in the aerospace field.

[0003] The second phase in 2324 aluminum alloy is a key factor affecting the alloy performance. Since Al2Cu, Al2CuMg, Al7Cu2Fe, and Mg2Si phases in the alloy's second phase are difficult to eliminate during the subsequent deformation process and heat treatment, in order to ensure that the final 2324 aluminum alloy finished plate has good mechanical properties, the composition must be strictly controlled during the casting stage to reduce the influence of impurity elements, and the type, quantity, and size of the second phase must be regulated during the homogenization heat treatment process of the ingot.

[0004] In the prior art, Chinese patent CN114737144B adopts a method of slowly heating at the melting temperature of the low-melting eutectic phase, that is, heating the aluminum alloy ingot to 494-495°C, then heating it to 498-500°C for 25-30h, and finally air cooling the aluminum alloy ingot to 20-25°C for homogenization heat treatment, to ensure that the low-melting eutectic phase is fully dissolved without overburning the ingot. Chinese patent application CN115976381A adopts an alloy composition with a higher Cu / Mg value and an aging process with an external tensile stress to promote the precipitation of the θ precipitate phase that is coherent or semi-coherent with the Al matrix, and inhibit the formation of the S phase and the precipitation phase that is incoherent with the matrix, thereby achieving the purpose of regulating the precipitate phase composition and improving the alloy performance; As can be seen from the above, the prior art does not consider the influence of different Cu contents on the second phase of the aluminum alloy, and does not provide a specific homogenization heat treatment system for different Cu contents. Summary of the invention

[0005] In view of the above problems, the present invention provides a homogenization heat treatment method for the second phase of an aluminum alloy ingot, which can adjust the second phase of a 2324 alloy ingot with different Cu contents, and sets appropriate homogenization treatment systems for the 2324 alloy ingots with different Cu contents, including heating rate, homogenization treatment temperature, and homogenization treatment time, to adjust the type, quantity, and size of the second phase in the microstructure of the ingot after homogenization, so as to ensure the smooth progress of the subsequent deformation heat treatment process and good quality control of the final finished plate.

[0006] The present invention provides a homogenization heat treatment method capable of regulating the second phase of an aluminum alloy ingot, comprising:

[0007] Step 1, obtaining an aluminum alloy ingot; the alloy composition of the aluminum alloy ingot is Si≤0.10wt%, Fe≤0.12wt%, Cu 3.8-4.4wt%, Mn 0.3-0.9wt%, Mg 1.2-1.8wt%, Cr≤0.10wt%, Zn≤0.25wt%, Ti 0.01-0.15wt%;

[0008] Step 2, setting a homogenization treatment system; the homogenization treatment system is that the mass fraction of Cu is 3.8%-4.4w%, the temperature is 490-495°C, and the insulation time is 20-30h;

[0009] The aluminum alloy ingot described in step 1 is placed in a container, and the aluminum alloy ingot is subjected to homogenization annealing based on the homogenization treatment system to obtain an updated aluminum alloy ingot; the updated aluminum alloy ingot is an aluminum alloy ingot after the second phase of the aluminum alloy ingot is regulated.

[0010] Preferably, the specific steps of obtaining the updated aluminum alloy ingot include:

[0011] Step 1, determining aluminum alloy raw materials; the aluminum alloy raw materials include alloy main raw materials and alloy additives;

[0012] Step 2, melting the aluminum alloy raw material to obtain an aluminum alloy melt, and casting to obtain an aluminum alloy ingot;

[0013] Step 3, placing the aluminum alloy ingot described in step 2 in a box furnace, and performing homogenization annealing on the aluminum alloy ingot based on a homogenization treatment system to obtain an updated aluminum alloy ingot; the updated aluminum alloy ingot is an aluminum alloy ingot after the second phase of the aluminum alloy ingot is regulated.

[0014] Furthermore, the aluminum alloy raw material in step 1 includes an alloy main body raw material and an alloy additive; the composition and weight percentage of the alloy additive are: Si≤0.10wt%, Fe≤0.12wt%, Cu3.8-4.4wt%, Mn0.3-0.9wt%, Mg1.2-1.8wt%, Cr≤0.10wt%, Zn≤0.25wt%, Ti0.01-0.15wt% and impurity elements;

[0015] The alloy main raw materials include aluminum ingots, magnesium ingots, aluminum-copper master alloy AlCu50, aluminum-manganese master alloy AlMn20 and aluminum-titanium master alloy AlTi10;

[0016] Furthermore, the total mass fraction of the impurity elements does not exceed 0.15%; wherein the mass fraction of a single impurity element does not exceed 0.05%;

[0017] The weight of the alloy main material is calculated based on the composition and weight percentage of the alloy additive;

[0018] Preferably, the specific steps of preparing the aluminum alloy ingot in step 2 include:

[0019] The aluminum ingot is melted to obtain a melt 1; an aluminum-manganese master alloy is added to the melt 1 and melted to obtain a melt 2;

[0020] Adding aluminum-copper master alloy and aluminum-titanium master alloy to melt 2 in sequence, and smelting to obtain melt 3;

[0021] Adding magnesium ingots to the melt three, smelting to obtain melt four; adding a refining agent to the melt four, standing it, performing slagging, stirring and slagging to obtain melt five; refining the melt five to obtain an aluminum alloy melt;

[0022] The aluminum alloy melt is cast into a preheated mold to obtain an aluminum alloy ingot.

[0023] Furthermore, the temperatures of melt one when the aluminum-manganese master alloy is added, melt two when the aluminum-copper master alloy and the aluminum-titanium master alloy are added, and melt three when the magnesium ingot is added are the same.

[0024] Furthermore, when the refining agent is added, the temperature of the melt 4 is less than or equal to 720°C.

[0025] Furthermore, the ratio of the mass of the refining agent to the mass of the melt is 0.2:100.

[0026] Furthermore, the refining time of the melt 5 is 3-5 minutes.

[0027] Furthermore, the temperature for refining the melt 5 is 690°C-750°C.

[0028] Furthermore, the smelting temperature of the aluminum ingot to obtain the melt 1 is 660-780°C.

[0029] Exemplarily, the specific steps of preparing the aluminum alloy ingot include:

[0030] The aluminum ingot is melted and slag is removed to obtain a melt 1; an aluminum-manganese master alloy is added to the melt 1, and after melting, the slag is removed, stirred, and slag is removed to obtain a melt 2;

[0031] Adding aluminum-copper master alloy and aluminum-titanium master alloy to melt 2 in sequence, and performing slag removal, stirring, and slag removal after melting to obtain melt 3;

[0032] Adding magnesium ingots to the melt three, and after melting, performing slag removal, stirring, and slag removal to obtain melt four; adding a refining agent to the melt four, and performing slag removal, stirring, and slag removal after standing to obtain melt five; refining the melt five, keeping it warm, standing, and slag removal to obtain an aluminum alloy melt;

[0033] The aluminum alloy melt is cast into a preheated cast iron mold to obtain an aluminum alloy ingot.

[0034] Furthermore, the tool used for melting is a melting furnace, which is preheated in advance when used; the preheating temperature is 200° C., and the preheating time is greater than 0.5 h;

[0035] Furthermore, the temperature of melting the aluminum ingot is 660-780°C;

[0036] Furthermore, the temperature ratio of melt 1 when adding the aluminum-manganese master alloy, melt 2 when adding the aluminum-copper master alloy and the aluminum-titanium master alloy, and melt 3 when adding the magnesium ingot is 1:1:1.

[0037] Furthermore, when the aluminum-manganese master alloy is added, the temperature of the melt 1 is 720°C-730°C;

[0038] When the aluminum-copper master alloy and the aluminum-titanium master alloy are added, the temperature of the melt 2 is 720°C-730°C; when the magnesium ingot is added, the temperature of the melt 3 is 720°C-730°C;

[0039] When the refining agent is added, the temperature of the melt 4 drops below 720°C;

[0040] Further, a graphite rod is used to press the magnesium ingot into the melt 3 to prevent the magnesium ingot from floating above the liquid surface and contacting the air;

[0041] Use a graphite rod to add the refining agent wrapped in aluminum foil into melt 4 to prevent the refining agent from floating above the liquid surface and contacting with air;

[0042] Exemplarily, the standing time is 10-20 min;

[0043] The refining gas is argon, and the insulation time is 10-20 minutes;

[0044] Specifically, the specific steps of preparing the aluminum alloy ingot in step 2 include:

[0045] The aluminum ingot is added into the preheated smelting furnace, and the slag is removed after the melting is completed to obtain the melt 1; when the temperature of the melt 1 is 720°C-730°C, the aluminum-manganese master alloy is added, and the slag is removed-stirred-slag removed after the aluminum-manganese master alloy is melted to obtain the melt 2;

[0046] When the temperature of the second melt is 720°C-730°C, aluminum-copper master alloy and aluminum-titanium master alloy are added in sequence, and after the aluminum-copper master alloy and the aluminum-titanium master alloy are melted, slag-stirring-slag-scraping are performed to obtain a third melt;

[0047] When the temperature of melt three is 720°C-730°C, a magnesium ingot is pressed into melt three with a graphite rod to prevent the magnesium ingot from floating above the liquid surface and contacting the air, and after the magnesium ingot is completely melted, slag-stirring-slag ...

[0048] Casting the aluminum alloy melt into a preheated cast iron mold to obtain an aluminum alloy ingot;

[0049] Exemplarily, the updated aluminum alloy ingot in step 3 is 2324 aluminum alloy.

[0050] Preferably, the homogenization treatment system includes: updating the mass fraction of Cu in the aluminum alloy ingot to 3.8%-4.4w%, the temperature to 490-495°C, the heating rate to 5-20°C / min, and the holding time to 20-30h;

[0051] Furthermore, the specific steps of uniform annealing in step 3 include:

[0052] When the mass fraction of Cu in the updated aluminum alloy ingot is 3.8%-4.0w%, the set temperature is 490-493℃, the heating rate is 5-20℃ / min, and the holding time is 20-25h;

[0053] Furthermore, the specific steps of uniform annealing in step 3 include:

[0054] When the mass fraction of Cu in the updated aluminum alloy ingot is 4.0%-4.2w%, the set temperature is 490-495℃, the heating rate is 5-20℃ / min, and the holding time is 20-25h;

[0055] Furthermore, the specific steps of uniform annealing in step 3 include:

[0056] When the mass fraction of Cu in the updated aluminum alloy ingot is 4.2%-4.4w%, the temperature is set at 490-495°C, the heating rate is 5-20°C / min, and the holding time is 25-30h.

[0057] The present invention sets the holding temperature and holding time of the homogenization heat treatment, and the heating time in the heating process is within 1 hour, and the annealing treatment is performed, which has a smaller impact than the holding time (about 20 hours), and controls the diffusion of the Cu element in the second phase of the 2324 aluminum alloy. The diffusion rate of Cu atoms in the aluminum matrix is ​​less than the diffusion rate of Mg atoms. When Cu is completely diffused, the homogenization is completed; with the change of the Cu content in the 2324 aluminum alloy ingot, the second phase (including Al 2 Cu、Al 2 CuMg、Al20Cu 2 Mn 3 The volume fraction and size of the alloy (such as aluminum alloy) will change. For 2324 aluminum alloys with different Cu content, the heat treatment temperature should be controlled between 490-495℃ and the time should be controlled between 20-30h. The temperature change has little effect within the above temperature range. For 2324 aluminum alloys with a Cu mass fraction of 3.8%-4.0w%, a lower heat treatment temperature is selected. For 2324 aluminum alloys with a Cu mass fraction of 4.2%-4.4w%, a longer holding time is selected to promote dissolution.

[0058] The present invention designs a homogenization heat treatment method for aluminum alloy ingots with different Cu contents, provides corresponding homogenization heat treatment systems for 2324 alloy ingots with different Cu contents, and systematically regulates the type, quantity and size of the second phase in the ingot structure; the mass fraction of the Cu element in the aluminum alloy is controlled to be below 4.2%, so that the second phase in the 2324 aluminum alloy after the homogenization heat treatment is fully dissolved back, and different homogenization treatment systems are adopted to ensure the completion of homogenization, so as to solve the differences in alloy phase composition, morphology and size caused by the difference in Cu content, and is beneficial to the subsequent deformation hot processing performance and the quality control of the final finished plate.

[0059] The second phase in the 2324 aluminum alloy ingot of the present invention is mainly Al 2 Cu、Al 2 CuMg, its morphology and size are closely related to the Cu content; when the Cu content is higher at 4.0wt%-4.4wt%, the second phase in the 2324 aluminum alloy ingot is larger in size and presents an interconnected long strip shape. When the Cu content is reduced to 3.8wt%-4.0wt%, the second phase can be transformed into a smaller short rod or granular shape, which is conducive to the dissolution of the second phase.

[0060] Compared with the prior art, the present invention has at least the following beneficial effects:

[0061] (1) The present invention sets different homogenization treatment temperatures and times for aluminum alloy ingots with different Cu contents, so that the second phase of the aluminum alloy ingot is fully dissolved back during the homogenization process, and a large amount of Al can be obtained in the subsequent aging treatment. 2The precipitation of Cu dispersed phase ensures that the finished plate has excellent strength and toughness;

[0062] (2) The present invention sets different homogenization treatment temperatures and times for 2324 aluminum alloys with different Cu contents, so as to more effectively control the morphology and size of the second phase in the alloy ingot structure. For the 2324 aluminum alloy with a higher Cu content, the homogenization treatment system is often too high in temperature or too long in time. For the 2324 aluminum alloy with a lower Cu content, a lower homogenization temperature is set, which can not only avoid overburning, but also save the cost of homogenization heat treatment and save heat treatment time. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] The drawings are only for the purpose of illustrating particular embodiments and are not to be construed as limiting the invention.

[0064] Figure 1 (a) is a schematic diagram of the as-cast structure of a 2324 alloy ingot with a Cu mass fraction of 3.8% prepared in Example 1 of the present invention;

[0065] Figure 1 (b) is a schematic diagram of the as-cast structure of the 2324 alloy ingot with a Cu mass fraction of 4.0% prepared in Example 2 of the present invention;

[0066] Figure 1 (c) is a schematic diagram of the as-cast structure of the 2324 alloy ingot with a Cu mass fraction of 4.2% prepared in Example 3 of the present invention;

[0067] Figure 1 (d) is a schematic diagram of the as-cast structure of the 2324 alloy ingot with a Cu mass fraction of 4.4% prepared in Example 4 of the present invention;

[0068] Figure 2 (a) is a schematic diagram of the as-cast structure of the 2324 alloy ingot with a Cu mass fraction of 3.8% prepared in Example 5 of the present invention after heat treatment;

[0069] Figure 2 (b) is a schematic diagram of the as-cast structure of the 2324 alloy ingot with a Cu mass fraction of 4.0% prepared in Example 6 of the present invention after heat treatment;

[0070] Figure 2 (c) is a schematic diagram of the as-cast structure of the 2324 alloy ingot with a Cu mass fraction of 4.2% prepared in Example 7 of the present invention after heat treatment;

[0071] Figure 2 (d) is a schematic diagram of the as-cast structure of the 2324 alloy ingot with a Cu mass fraction of 4.4% prepared in Example 8 of the present invention after heat treatment;

[0072] Figure 3 Schematic diagram of the as-cast structure of 2324 alloy ingots with Cu mass fractions of 3.8% and 4.2% respectively prepared in Comparative Examples 1 and 2 of the present invention after heat treatment. DETAILED DESCRIPTION

[0073] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. In addition, the present invention can also be implemented in other ways different from those described herein, and therefore, the protection scope of the present invention is not limited by the specific embodiments disclosed below.

[0074] A specific embodiment of the present invention, as Figure 1-3 , discloses a homogenization heat treatment method capable of regulating the second phase of an aluminum alloy ingot;

[0075] In order to illustrate the effectiveness of the method proposed in the present invention, the above technical solution of the present invention is described in detail below through a specific embodiment;

[0076] Embodiment 1

[0077] Step 1, Si mass fraction is less than 0.10%, Fe mass fraction is less than 0.12%, Cu mass fraction is 3.8%, Mn mass fraction is 0.55%, Mg mass fraction is 1.4%, Cr mass fraction is less than 0.10%, Zn mass fraction is less than 0.25%, Ti mass fraction is 0.01%-0.15%, and other impurity elements, single mass fraction does not exceed 0.05%, and the total does not exceed 0.15%;

[0078] According to the composition range of each alloy element in the above aluminum alloy ingot, and taking into account the burnout during the alloy smelting process and the alloy composition and content in the waste, the weight of the high-purity aluminum ingot (99.99%), the magnesium ingot, the aluminum-copper master alloy AlCu50, the aluminum-manganese master alloy AlMn20 and the aluminum-titanium master alloy AlTi10 are calculated, and various alloy raw materials are weighed according to the calculation results;

[0079] Step 2: Add the high-purity aluminum ingot prepared in step 1 into the preheated smelting furnace;

[0080] Put magnesium ingots, aluminum-copper master alloys, aluminum-manganese master alloys, aluminum-titanium master alloys, stirring and slagging tools, and casting molds into a box furnace for preheating;

[0081] After the aluminum ingot is melted, the slag is removed to obtain melt one. When the temperature of melt one is 720°C-730°C, an aluminum-manganese master alloy is added. After the aluminum-manganese master alloy is melted, the slag is removed-stirred-slag removed to obtain melt two.

[0082] When the temperature of melt 2 is 720°C-730°C, aluminum-copper master alloy and aluminum-titanium master alloy are added in sequence, and after melting, slag-stirring-slag-slag-scraping are performed to obtain melt 3;

[0083] When the temperature of melt 3 is 720℃-730℃, a graphite rod is used to press the magnesium ingot into melt 3 to prevent the magnesium ingot from floating above the liquid surface of melt 3 and contacting the air. After the magnesium ingot is completely melted, slag-stirring-slag-slag-scraping is performed to obtain melt 4.

[0084] When the temperature of melt 4 drops below 720°C, a graphite rod is used to press a refining agent of 0.2% of the total mass of melt 4 wrapped in aluminum foil into melt 4 to prevent the refining agent from floating above the liquid surface of melt 4 and contacting with air. After 10 minutes, slag-stirring-slag-scraping is performed to obtain melt 5.

[0085] The melt is refined using argon for 5 minutes, kept warm for 20 minutes, and then the furnace door is opened and allowed to stand for 10 minutes. After the standing time is completed, slag is removed to obtain an aluminum alloy melt;

[0086] The aluminum alloy melt is cast into a preheated mold to obtain an aluminum alloy ingot.

[0087] Step 3: Place the aluminum alloy ingot obtained in step 2 in a box furnace for homogenization annealing at a furnace temperature of 495°C, a heating rate of 5°C / min, and keep warm for 20 hours to obtain an updated aluminum alloy ingot.

[0088] Embodiment 2

[0089] In Example 1, "the mass fraction of Cu is changed to 4.0%", and the rest remain unchanged.

[0090] Embodiment 3

[0091] In Example 1, "the mass fraction of Cu is changed to 4.2%", and the rest remain unchanged.

[0092] Embodiment 4

[0093] In Example 1, "the mass fraction of Cu is changed to 4.4%", and the rest remain unchanged.

[0094] The aluminum alloy ingots of step 2 in embodiments 1 to 4 and the updated aluminum alloy ingots of step 3 were subjected to microstructural observation. The main second phase in the as-cast structure of the aluminum alloy ingots of embodiments 1 to 4 is Al 2 Cu phase and Al 2 CuMg phase, the existing ternary eutectic phase size is 5-10μm in width and 5-100μm in length. In addition, there is Al 2 The fine precipitate phase of CuMg has a size between 0.2 and 1 μm;

[0095] When the Cu content increases from 3.8wt.% to 4.4wt.%, the volume fraction of the second phase in the ingot structure gradually increases from 6.19% to 7.95%. In the microstructure of the updated aluminum alloy ingot obtained in step 3, there is still a residual second phase with a ternary eutectic morphology, and a large number of Al2O3 with a size of about 1-2μm are distributed in the crystal. 2 CuMg phase, when the Cu content increases from 3.8wt.% to 4.4wt.%, the volume fraction of the residual second phase in the ingot structure gradually increases from 0 to 0.69%. With the increase of Cu content, the second phase in the ingot structure gradually changes from a large interconnected long strip to a small short rod or granular shape, and the secondary dendrite spacing decreases slightly.

[0096] Embodiment 5

[0097] The furnace temperature in Example 1 is changed to 490° C., and other technical solutions remain unchanged.

[0098] Embodiment 6

[0099] The furnace temperature in Example 2 is changed to 493° C., and other technical solutions remain unchanged.

[0100] Embodiment 7

[0101] The furnace temperature in Example 3 is changed to 495° C., and other technical solutions remain unchanged.

[0102] Embodiment 8

[0103] The furnace temperature in Example 4 was changed to 495° C., the heating rate was 5° C. / min, and the temperature was kept for 25 h. Other technical solutions remained unchanged.

[0104] Microstructural observation of the updated aluminum alloy ingot obtained in step 3 of Examples 5 to 7 revealed that after different homogenization heat treatments, the second phase dissolution effects in the 2324 alloy ingots with Cu mass fractions of 3.8, 4.0, 4.2, and 4.4% were almost the same, and the residual second phase volume fractions were ≤0.01%, 0.18%, 0.43%, and 0.69%, respectively, which were basically all below 0.5%.

[0105] Comparative Example 1

[0106] (1) The 2324 alloy ingot with a Cu mass fraction of 3.8% prepared in Example 1 was subjected to homogenization heat treatment, with the furnace temperature set to 494° C., the heating rate set to 0.67° C. / min, the converter temperature set to 500° C., the conversion time set to 27 h, and air cooling to obtain the treated ingot;

[0107] (2) Microstructural observation of the ingot after the treatment revealed that after homogenization heat treatment, the residual second phase volume in the 2324 alloy ingot with a Cu mass fraction of 3.8% was 0.09%, which was higher than the second phase volume fraction of the ingot with the same Cu content after heat treatment in the embodiment.

[0108] Comparative Example 2

[0109] (1) The 2324 alloy ingot with a Cu mass fraction of 4.2% prepared in Example 1 was subjected to homogenization heat treatment, with the furnace temperature set to 494° C., the heating rate set to 0.67° C. / min, the converter temperature set to 500° C., the conversion time set to 27 h, and air cooling to obtain the treated ingot;

[0110] (2) Microstructural observation of the treated ingot revealed that after homogenization heat treatment, the residual second phase volume in the 2324 alloy ingot with a Cu mass fraction of 4.2% was 0.60%, which was higher than the second phase volume fraction of the ingot with the same Cu content after heat treatment in the embodiment.

[0111] The experimental results show that in order to ensure that the second phase in the 2324 aluminum alloy after homogenization heat treatment is fully dissolved, the mass fraction of the Cu element in the alloy should be controlled at 4.2% or below. For 2324 aluminum alloys with different Cu contents, designing different homogenization heat treatments can more effectively control the second phase.

[0112] Table 1

[0113]

[0114]

[0115] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A homogenization heat treatment method capable of regulating the second phase of an aluminum alloy ingot, It is characterized in that The specific steps include: Step 1, obtaining an aluminum alloy ingot; the alloy composition of the aluminum alloy ingot is Si≤0.10wt%, Fe≤0.12wt%, Cu 3.8-4.4wt%, Mn 0.3-0.9wt%, Mg 1.2-1.8wt%, Cr≤0.10wt%, Zn≤0.25wt%, Ti0.01-0.15wt%; Step 2, setting a homogenization treatment system; the homogenization treatment system includes a Cu mass fraction of 3.8%-4.4w%, a temperature of 490-495°C, and a holding time of 20-30h; The aluminum alloy ingot described in step 1 is placed in a container, and the aluminum alloy ingot is subjected to homogenization annealing according to the homogenization treatment system to obtain an updated aluminum alloy ingot; the updated aluminum alloy ingot is an aluminum alloy ingot after the second phase of the aluminum alloy ingot is regulated.

2. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 1, It is characterized in that The aluminum alloy ingot is a 2324 aluminum alloy ingot.

3. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 2, It is characterized in that The homogenization treatment system specifically includes: when the mass fraction of Cu in the updated aluminum alloy ingot is 3.8%-4.0w%, the temperature is set to 490-493°C, the heating rate is 5-20°C / min, and the temperature is kept for 20-25h; When the mass fraction of Cu in the updated aluminum alloy ingot is 4.0%-4.2w%, the set temperature is 490-495℃, the heating rate is 5-20℃ / min, and the temperature is kept for 20-25h; When the mass fraction of Cu in the updated aluminum alloy ingot is 4.2%-4.4w%, the set temperature is 490-495°C, the heating rate is 5-20°C / min, and the heat preservation is 25-30h.

4. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 3, It is characterized in that The specific steps of preparing the aluminum alloy ingot include: The aluminum ingot is melted to obtain a melt 1; an aluminum-manganese master alloy is added to the melt 1 and melted to obtain a melt 2; Adding aluminum-copper master alloy and aluminum-titanium master alloy to melt 2 in sequence, and smelting to obtain melt 3; Adding magnesium ingots to the melt three, smelting to obtain melt four; adding a refining agent to the melt four, standing it, performing slagging, stirring and slagging to obtain melt five; refining the melt five to obtain an aluminum alloy melt; The aluminum alloy melt is cast into a preheated mold to obtain an aluminum alloy ingot.

5. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 4, It is characterized in that The temperatures of melt 1 when the aluminum-manganese master alloy is added, melt 2 when the aluminum-copper master alloy and the aluminum-titanium master alloy are added, and melt 3 when the magnesium ingot is added are the same.

6. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 4, It is characterized in that When the refining agent is added, the temperature of the melt 4 is less than or equal to 720°C.

7. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 4, It is characterized in that The ratio of the mass of the refining agent to the mass of the melt is 0.2:

100.

8. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 4, It is characterized in that The time for refining the melt 5 is 3-5 minutes.

9. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 4, It is characterized in that The temperature for refining the melt 5 is 690°C-750°C.

10. The homogenization heat treatment method for the second phase of the adjustable aluminum alloy ingot according to claim 4, It is characterized in that The smelting temperature of the aluminum ingot to obtain the melt 1 is 660-780°C.