Homogenization treatment method for inner wall of copper alloy pipe with large length-diameter ratio

A highly corrosion-resistant film layer is formed through sandblasting, pickling and natural passivation, which solves the problem of insufficient corrosion resistance of small-diameter, large-aspect-ratio copper alloy pipes in seawater environments and achieves long-term stability of copper alloy pipes. use.

CN118726987APending Publication Date: 2024-10-01CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410903792.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult for the existing technology to effectively improve the corrosion resistance of small-diameter, large-aspect-ratio copper alloy pipes under seawater conditions for a long time. Especially in the high-sand environment of the East China Sea, defects in the inner wall of the pipe and non-uniform coating lead to frequent leakage and corrosion problems.

Method used

After removing defects on the inner wall of the pipe by sandblasting, a pre-passivation film is formed through pickling and pre-passivation, and then naturally passivated in flowing seawater to form a natural passivation film with high electrochemical impedance and low corrosion current density.

Benefits of technology

It significantly improves the corrosion resistance of copper alloy pipes, reduces the risk of leakage, and forms a uniform, continuous and complete film layer on the inner wall of the pipe. It is suitable for copper alloy pipes of different diameters and materials, and has strong applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726987A_ABST
    Figure CN118726987A_ABST
Patent Text Reader

Abstract

The invention discloses a homogenization treatment method for the inner wall of a copper alloy pipe with a large length-diameter ratio, which comprises the following steps of: removing defects in the pipe through a sand blasting method, performing acid washing to reduce the roughness in the pipe, preparing a layer of pre-passivation film in the pipe through a pre-passivation method, and preparing a layer of natural passivation film in the pipe through flushing of flowing seawater. The method specifically comprises the following steps that S1, sand blasting is conducted; s2, removing oil; s3, acid pickling; s4, pre-passivation is carried out; s5, detecting a formed film; s6, corrosion resistance detection; and S7, generating a natural passivation film. A complex film layer is prepared on the basis of removing inner wall defects through sand blasting, acid pickling and pre-passivation treatment methods, the corrosion resistance of the copper alloy pipe can be effectively improved in the initial stage of use, and formation of a passive film of the pipe can be promoted. The inner wall of the copper alloy pipe obtained through the method is uniform, continuous and complete, the copper alloy pipe can be used in a seawater environment for a long time, the corrosion resistance of the copper alloy pipe can be remarkably improved, and the leakage risk is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface treatment and relates to copper alloy surface treatment. Background Art

[0002] Seawater system is the main working system of ships, offshore oil and gas fields, coastal power plants, offshore firefighting, oil field water injection and other equipment. Early seawater systems were mostly built with carbon steel and cast iron. Although the initial investment cost was low, these materials had poor seawater corrosion resistance and low resistance to marine biofouling, which not only wasted a lot of manpower and material resources, shortened the working life of the system, but also often caused major accidents. In recent years, with the development of copper alloy metal materials, seawater systems have begun to be made of non-ferrous metals with excellent seawater corrosion resistance and anti-fouling ability. For example, copper alloys such as copper-nickel alloys and brass are widely used in condensers of various ships in marine engineering, heat exchangers of coastal power plants, and piping systems of seawater desalination equipment because of their good seawater corrosion resistance. Although this seawater system has a high initial investment, it has few maintenance times, low full-life working costs, and extremely high reliability, so it has been increasingly widely used in industries such as ships.

[0003] However, copper alloys have experienced serious corrosion and leakage accidents during their service in seawater environments. For example, in the seawater piping system of ships, TUP copper pipes were used in the past, and corrosion was a common problem; in recent years, the seawater piping system of ships has mostly adopted B10 materials with higher corrosion resistance, but there are still serious problems of corrosion and leakage of the piping system; the marine condenser tubes are made of B30 copper-nickel alloy, which is severely corroded when used in the seawater environment with a high sand content in the East China Sea. Frequent leakage of seawater pipelines seriously affects the normal use of equipment, reduces the rate of ships in navigation, and often causes potential accidents.

[0004] Domestic and foreign scholars have conducted a lot of research on the corrosion of copper alloys in seawater. At present, it can be considered that the surface state of the inner wall of the tube has an important influence on the corrosion of copper alloy tubes. In the document "Application of Chemical Plating Technology in Anti-corrosion of Ship Seawater Pipelines", Ni-P coating was prepared on the inner wall of TUP copper tubes and B10 tubes by chemical plating. The corrosion rate of Ni-P coated copper elbows is about 12% of the corrosion rate of copper elbows, and the corrosion rate of Ni-P coated B10 elbows is about 7% of the corrosion rate of B10 elbows. When there are defects such as residual carbon film and scratches on the inner wall of the copper alloy tube, it is difficult to form a complete coating in this area, and it is difficult to ensure the uniformity of the coating inside the tube with a small diameter and a large aspect ratio.

[0005] Invention patent CN 108000158 A "Device and method for grinding the inner wall of ultra-long and large-diameter aluminum alloy tubes, flattening and chamfering" realizes high-efficiency, high-quality, and automated grinding inside large-diameter aluminum alloy tubes. However, it is difficult to apply to copper alloy tubes with small diameters and large aspect ratios. Invention patent CN 111979390 A "A method for removing residual carbon on the inner surface of small-diameter seawater copper-nickel tubes" uses sandblasting to remove the residual carbon film on the surface, which can make the peak intensity of the residual carbon Raman spectrum on the inner surface of the copper-nickel tube equivalent to the carbon intensity inside the matrix, and the thinning of the tube wall is very low. After treatment by this method, the internal roughness of the copper alloy tube is relatively high, and it is difficult to form a protective film or even corrosion during use under static seawater conditions.

[0006] In the above invention, little attention has been paid to the method of uniformly treating the inner surface of small-diameter and large aspect ratio copper alloy tubes to improve their corrosion resistance. The method of polishing the inside of the tube by physical methods or forming a film layer inside the tube by chemical plating methods can have a certain effect in the short term, but it is difficult to meet the needs of actual use conditions in long-term use. Summary of the invention

[0007] In view of this, the present invention provides a method for homogenizing the inner wall of a copper alloy tube with a large aspect ratio, which solves the problem in the prior art that it cannot meet the long-term corrosion resistance requirements under seawater conditions.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A method for homogenizing the inner wall of a large aspect ratio copper alloy tube comprises the following steps:

[0010] S1: Sandblasting: connect the sandblasting gun muzzle with one end of the copper alloy tube, use clean oil-free brown corundum sand, and use compressed air to blow the sand material to the inner wall of the tube; then connect the sandblasting gun muzzle with the other end of the copper alloy tube, and repeat the above steps; after the sandblasting is completed, use compressed air to blow from both ends of the copper alloy tube to remove a small amount of residual sand material on the inner wall of the copper alloy tube;

[0011] S2: Degreasing: Use degreasing liquid to rinse the inner wall of the copper alloy tube. After degreasing, use tap water to rinse the inside of the copper alloy tube.

[0012] S3: pickling, preparing a pickling solution, passing the pickling solution into the inside of the copper alloy tube, and rinsing the inside of the copper alloy tube with tap water after the pickling;

[0013] S4: pre-passivation, preparing a pre-passivation solution, immersing the copper alloy tube in the pre-passivation solution to form a pre-passivation film; after the pre-passivation is completed, use distilled water to rinse the inside of the copper alloy tube;

[0014] S5: Film formation detection: prepare a film formation detection solution, drop it on the surface of the copper alloy tube after pre-passivation treatment, and detect its surface film layer;

[0015] S6: Corrosion resistance test: immerse the pre-passivated copper alloy tube in artificial seawater and observe the surface of the copper alloy tube;

[0016] S7: Natural passivation: The copper alloy tubes that have passed the film formation test and corrosion resistance test are immersed in flowing seawater for continuous flushing for 14-28 days to form a natural passivation film.

[0017] Furthermore, in step S1, the brown corundum sand is 24-60 mesh, the compressed air is 0.4-0.6 MPa, and the sandblasting time is 3-7 min.

[0018] Furthermore, the degreasing time in step S2 is 4-6 minutes.

[0019] Furthermore, the pickling solution in step S3 mainly includes 30-80 mL / L concentrated sulfuric acid, 200-350 mL / L hydrogen peroxide and 15-25 mL / L anhydrous ethanol, and the pickling time is 1-8 min.

[0020] Furthermore, the pre-passivation solution in step S4 includes 1-10 g / L of benzotriazole and 30-150 mL / L of anhydrous ethanol; and the pre-passivation time is 60-300 min.

[0021] Furthermore, the pre-passivation film in step S4 is a benzotriazole film.

[0022] Furthermore, the film-forming detection solution in step S5 is composed of distilled water and concentrated nitric acid, wherein the volume ratio of distilled water to concentrated nitric acid is 3:1.

[0023] Furthermore, the artificial seawater in step S6 contains 5 ppm of sodium sulfide, and the seawater immersion time does not exceed 5 days.

[0024] Furthermore, the electrochemical impedance of the natural passivation film in artificial seawater is Z≥10 5 Ω·cm 2 , corrosion current density J≤10 -6 A / cm 2 .

[0025] Furthermore, the copper alloy tube is a copper alloy tube with a small diameter and a large long diameter, wherein the copper alloy tube is TUP copper, tin bronze or iron white copper.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1) The present invention removes defects in the tube by sandblasting, then pickles to reduce the roughness of the tube, prepares a pre-passivation film in the tube by pre-passivation, and prepares a natural passivation film in the tube by flushing with flowing seawater. The inner wall of the copper alloy tube treated by this process is uniform, continuous, and complete, and can be used in a seawater environment for a long time, which can significantly improve its corrosion resistance and greatly reduce the risk of leakage.

[0028] 2) Sand blasting can effectively remove defects such as inclusions, scratches, and residual carbon film on the inner wall of copper alloy tubes with a large aspect ratio.

[0029] 3) A pre-passivation film is prepared inside the tube to effectively improve the corrosion resistance of the copper alloy tube in seawater environment; a complex film layer is prepared on the basis of removing the inner wall defects, which can effectively improve the corrosion resistance of the copper alloy tube in the initial use and promote the formation of the tube's own passivation film.

[0030] 4) The process of the present invention has strong applicability and can be used in the inner wall treatment of copper alloy tubes such as TUP copper, tin bronze, and nickel silver with different calibers and large aspect ratios. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is an endoscope image of the inner wall of the B30 tube in the original state in Example 1 of the present invention;

[0032] Figure 2 This is a morphology image of the inner wall of the B30 tube in the original state in Example 1 of the present invention;

[0033] Figure 3 This is an endoscopic image of the inner wall of a B30 tube after homogenization treatment in Example 1 of the present invention;

[0034] Figure 4 This is a morphology image of the inner wall of the B30 tube after homogenization treatment in Example 1 of the present invention;

[0035] Figure 5 This is an endoscope image of the inner wall of the B30 tube after being washed by seawater for 28 days in Example 1 of the present invention;

[0036] Figure 6 This is a morphology of the inner wall of the B30 tube after being washed by seawater for 28 days in Example 1 of the present invention;

[0037] Figure 7 This is an endoscope image of the inner wall of the B30 tube after half a year of operation under simulated working conditions in Example 1 of the present invention;

[0038] Figure 8 This is a morphology diagram of the inner wall of the B30 tube after half a year of operation under simulated working conditions in Example 1 of the present invention;

[0039] Fig. 9 This is a morphology of the inner wall of the untreated B30 pipe after being washed with seawater for 28 days in Comparative Example 1 of the present invention;

[0040] Fig.10 This is a morphology of the inner wall of the B30 pipe treated with only sandblasting in Comparative Example 1 of the present invention after being washed by seawater for 28 days;

[0041] Fig.11 This is a morphology of the inner wall of the B30 tube subjected to only pre-passivation treatment in Comparative Example 1 of the present invention after being flushed with seawater for 28 days; DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0043] The invention discloses a method for homogenizing the inner wall of a copper alloy tube with a large aspect ratio, which is suitable for copper alloy tubes with small diameter and large length, wherein the copper alloy tube is TUP copper, tin bronze or copper-nickel alloy.

[0044] The treatment method includes the following steps:

[0045] S1: Sandblasting: connect the sandblasting gun muzzle with one end of the copper alloy tube, use clean and oil-free 24-60 mesh brown corundum sand, and use compressed air with a pressure of 0.4-0.6MPa to blow the sand material to the inner wall of the tube. The sandblasting blowing time is 3-7min; then connect the sandblasting gun muzzle with the other end of the copper alloy tube, and repeat the above steps; after the sandblasting is completed, use compressed air to blow from both ends of the copper alloy tube to remove a small amount of residual sand material on the inner wall of the copper alloy tube. The compressed air blowing time at both ends is 1min;

[0046] S2: Degreasing: Use degreasing liquid to rinse the inner wall of the copper alloy tube for 4-6 minutes; after degreasing, use tap water to rinse the inside of the copper alloy tube;

[0047] S3: pickling, preparing a pickling solution, the pickling solution mainly includes 30-80mL / L concentrated sulfuric acid, 200-350mL / L hydrogen peroxide and 15-25mL / L anhydrous ethanol;

[0048] A pickling solution is passed into the copper alloy tube for 1-8 minutes. After the pickling is completed, the inside of the copper alloy tube is rinsed with tap water.

[0049] S4: Pre-passivation, preparing a pre-passivation solution, the pre-passivation solution includes 1-10 g / L of benzotriazole (BTA) and 30-150 mL / L of anhydrous ethanol;

[0050] The copper alloy tube is immersed in the pre-passivation solution for 60-300 minutes to form a pre-passivation film (BTA film). After the pre-passivation is completed, the inside of the copper alloy tube is rinsed with distilled water;

[0051] S5: Film formation test: prepare a film formation test solution with a volume fraction of distilled water: concentrated nitric acid = 3:1, and drop it on the surface of the copper alloy tube after pre-passivation treatment. No bubbles are generated within 30 seconds, which proves that a complete film layer has been formed on its surface;

[0052] S6: Corrosion resistance test: immerse the pre-passivated copper alloy tube in artificial seawater containing 5ppm sodium sulfide for no more than 5 days to observe whether there is verdigris on the surface of the copper alloy tube;

[0053] S7: Natural passivation: the copper alloy tubes that have passed the film formation test and corrosion resistance test are immersed in flowing seawater for continuous flushing for 14-28 days to form a natural passivation film. The electrochemical impedance of the generated natural passivation film in artificial seawater is Z ≥ 10 5 Ω·cm 2 , corrosion current density J≤10 -6 A / cm 2 .

[0054] Example 1

[0055] The material selected is copper-nickel alloy BFe30-1-1 (hereinafter referred to as B30) tube with a specification of φ16×1770×1.25mm.

[0056] (1) Acid cleaning solution preparation: 50 mL / L concentrated sulfuric acid, 250 mL / L hydrogen peroxide, 20 mL / L anhydrous ethanol, and the balance distilled water.

[0057] (2) Passivation solution preparation: BTA (benzotriazole) 5g / L, anhydrous ethanol 100mL / L, and distilled water as the balance.

[0058] (3) A method for homogenizing the inner wall of a copper alloy tube with a large aspect ratio:

[0059] S1: Sandblasting, connect the sandblasting gun nozzle to one end of the tube, pass compressed air with a pressure of 0.5MPa, use 24 mesh clean oil-free brown corundum sand to blow the inner wall of the tube for 5 minutes. Then connect the sandblasting gun nozzle to the other end of the tube, repeat the above steps, and blow for 5 minutes. After completion, use 0.5MPa compressed air to blow a small amount of residual sand on the inner wall of the tube, and blow for 1 minute at each end. The roughness of the inner wall of the tube after sandblasting is Ra 3.359μm,

[0060] S2: Degreasing: Use degreasing liquid to rinse the inner wall of the pipe for 5 minutes. After degreasing, use tap water to rinse the inside of the pipe for 5 minutes.

[0061] S3: Pickling: Use pickling liquid to rinse the inside of the tube for 5 minutes. After pickling, use tap water to rinse the inside of the tube for 5 minutes.

[0062] S4: Pre-passivation, soak the B30 tube in the passivation solution for 180 minutes, rinse the B30 tube with distilled water for 5 minutes, and blow dry with 0.5MPa compressed air after rinsing. After pickling and pre-passivation, the roughness is Ra2.217μm.

[0063] The inner wall of the B30 tube after pre-passivation treatment is uniform and silvery white, without black corrosion streaks and local contamination.

[0064] S5: Film formation test: prepare a solution of distilled water: concentrated nitric acid = 3:1, and drop it on the surface of the tube sample after pre-passivation treatment. No bubbles are generated within 30 seconds, proving that a complete film layer has been formed on its surface.

[0065] S6: The sample was immersed in artificial seawater containing 5 ppm sodium sulfide for 5 days, and no patina appeared, proving its excellent corrosion resistance.

[0066] S7: Natural passivation, the pre-treated B30 pipe was immersed in the Qinhuangdao sea area for a long time, and intermittent scouring was carried out to simulate the working condition assessment test. After running for half a year, there was no obvious corrosion mark. After continuous scouring for 28 days in the Qinhuangdao sea area, the pre-passivation film completed the transformation of the natural passivation film, forming a light yellow or golden dense film layer.

[0067] The electrochemical impedance of the natural passive film in artificial seawater is ≥10 5 Ω·cm 2 , corrosion current density ≤10 -6 A / cm 2 .

[0068] Example 2

[0069] The difference between this embodiment and Example 1 is that the specifications of the tube are φ16×2772×1.75 mm.

[0070] The corresponding performance tests were carried out on the BC30 tube after pre-passivation treatment. It was observed that the inside of the tube was uniform and silvery white after pre-passivation treatment. A solution of distilled water: concentrated nitric acid = 3:1 was prepared and dropped on the surface of the treated tube sample. No bubbles were generated within 30 seconds. The sample was immersed in artificial seawater containing 5ppm sodium sulfide, and no verdigris appeared for 5 days. The pre-treated B30 tube was immersed in the Qinhuangdao waters for a long time and intermittently flushed to simulate the working condition assessment test. After half a year of operation, there were some green attachments but no obvious signs of corrosion. After 28 days of continuous flushing in the Qinhuangdao waters, the pre-passivation film completed the transformation into the natural passivation film, forming a light yellow or golden dense film layer. The electrochemical impedance of the natural passivation film in artificial seawater is ≥10 5 Ω·cm 2 , corrosion current density ≤10 -6 A / cm 2 .

[0071] Comparative Example 1

[0072] Comparative Example 1: The sample materials and specifications used in Example 1 are the same, and no other pretreatment is performed on it. Only the natural passivation process is performed to observe its corrosion resistance and the state of natural passivation film formation:

[0073] The untreated B30 pipes were immersed in the Qinhuangdao sea area for a long time and intermittently scour to simulate the working condition assessment test. After 28 days of continuous scouring in the Qinhuangdao sea area, green corrosion products appeared on the inner wall of the untreated B30 pipes, and no complete natural passivation film was formed on the surface.

[0074] Comparative Example 2

[0075] Comparative Example 2: The sample materials and specifications used are the same as those used in Example 1. Only the sample is sandblasted to observe its corrosion resistance and the state of natural passivation film formation:

[0076] The B30 pipe that was only sandblasted was immersed in the Qinhuangdao sea area for a long time and intermittently scoured to simulate the working condition assessment test. After 28 days of continuous scouring in the Qinhuangdao sea area, there was no obvious corrosion on the inner wall of the B30 pipe that was only sandblasted, proving its excellent corrosion resistance; at the same time, no uniform natural passivation film was formed on the surface.

[0077] Comparative Example 3

[0078] Comparative Example 3: The sample materials and specifications used are the same as those used in Example 1. Only the sample is subjected to pre-filming treatment to observe its corrosion resistance and the state of natural passivation film formation:

[0079] The B30 pipes that had only been pre-filmed were immersed in the Qinhuangdao waters for a long time and subjected to intermittent scouring to simulate operating conditions. After 28 days of continuous scouring in the Qinhuangdao waters, green corrosion products appeared on the inner wall of the B30 pipes that had only been pre-filmed. After being scoured by seawater, the natural passivation film was incomplete and uneven.

[0080] The above results show that the inner wall of the copper alloy obtained by Example 1-2, i.e., the inner wall of the copper alloy tube after sandblasting, pickling, pre-passivation and formation of a natural passivation film, is uniform, continuous and complete, and its corrosion resistance is significantly improved, and it can be used in a seawater environment for a long time.

[0081] The results of Comparative Examples 1-3 also show that in the treatment method for homogenizing the inner wall of the copper alloy in the present invention, the lack of any of the treatment methods of natural passivation, sandblasting, or pre-passivation will affect the formation and corrosion resistance of the corrosion-resistant film on the inner wall of the copper alloy; when only natural passivation treatment is performed, green corrosion products appear on the inner wall of the copper alloy tube, and a complete natural passivation film is not formed on the surface; when only sandblasting and natural passivation treatment are performed, no obvious corrosion occurs on the inner wall of the copper alloy tube, and a uniform natural passivation film is not formed on the surface; when only pre-passivation and natural passivation treatment are performed, green corrosion products appear on the inner wall of the copper alloy tube, and the natural passivation film is not formed completely and uniformly.

[0082] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for homogenizing the inner wall of a copper alloy tube with a large aspect ratio, characterized in that: The following steps are involved: S1: Sandblasting: connect the sandblasting gun muzzle with one end of the copper alloy tube, use clean oil-free brown corundum sand, and use compressed air to blow the sand material to the inner wall of the tube; then connect the sandblasting gun muzzle with the other end of the copper alloy tube, and repeat the above steps; after the sandblasting is completed, use compressed air to blow from both ends of the copper alloy tube to remove a small amount of residual sand material on the inner wall of the copper alloy tube; S2: Degreasing: Use degreasing liquid to rinse the inner wall of the copper alloy tube. After degreasing, use tap water to rinse the inside of the copper alloy tube. S3: pickling, preparing a pickling solution, passing the pickling solution into the inside of the copper alloy tube, and rinsing the inside of the copper alloy tube with tap water after the pickling; S4: pre-passivation, preparing a pre-passivation solution, immersing the copper alloy tube in the pre-passivation solution to form a pre-passivation film; after the pre-passivation is completed, use distilled water to rinse the inside of the copper alloy tube; S5: Film formation detection: prepare a film formation detection solution, drop it on the surface of the copper alloy tube after pre-passivation treatment, and detect its surface film layer; S6: Corrosion resistance test: immerse the pre-passivated copper alloy tube in artificial seawater and observe the surface of the copper alloy tube; S7: Natural passivation: The copper alloy tubes that have passed the film formation test and corrosion resistance test are immersed in flowing seawater for continuous flushing for 14-28 days to form a natural passivation film.

2. The processing method according to claim 1, characterized in that: In step S1, the brown corundum sand is 24-60 mesh, the compressed air is 0.4-0.6 MPa, and the sandblasting time is 3-7 min.

3. The processing method according to claim 1, characterized in that: The degreasing time in step S2 is 4-6 minutes.

4. The processing method according to claim 1, characterized in that: The pickling solution in step S3 mainly includes 30-80 mL / L concentrated sulfuric acid, 200-350 mL / L hydrogen peroxide and 15-25 mL / L anhydrous ethanol, and the pickling time is 1-8 min.

5. The processing method according to claim 1, characterized in that: The pre-passivation solution in step S4 includes 1-10 g / L of benzotriazole and 30-150 mL / L of anhydrous ethanol; the pre-passivation time is 60-300 min.

6. The processing method according to claim 5, characterized in that: The pre-passivation film in step S4 is a benzotriazole film.

7. The processing method according to claim 1, characterized in that: In step S5, the film-forming detection solution is composed of distilled water and concentrated nitric acid, wherein the volume ratio of distilled water to concentrated nitric acid is 3:

1.

8. The processing method according to claim 1, characterized in that: The artificial seawater in step S6 contains 5 ppm of sodium sulfide, and the seawater immersion time does not exceed 5 days.

9. The processing method according to claim 1, characterized in that: The electrochemical impedance Z generated by the natural passivation film in the artificial seawater in step S7 is ≥ 10 5 Ω·cm 2 , corrosion current density J≤10 -6 A / cm 2 .

10. The processing method according to claim 1, characterized in that: The copper alloy tube is a copper alloy tube with a small diameter and a large long diameter, and the material of the copper alloy tube is TUP copper, tin bronze or iron white copper.

Citation Information

Cited By

  • Method for evaluating maturity of passive film of ship pipeline

    CN121454000A