Conductive silicon target and preparation method thereof

By using hot-press sintering and annealing processes in the preparation of polysilicon targets, combined with the addition of an appropriate amount of boron powder, the problem of introducing metal impurities into boron alloys is solved, the conductive properties are improved, and the thermal stress and cracking risk of the target are reduced, improving the Density and pass rate of target materials.

CN118727140APending Publication Date: 2024-10-01XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982186.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the preparation process of polysilicon targets, metallic impurities are easily introduced when incorporating boron alloys to control resistivity, resulting in reduced target quality and affecting subsequent use.

Method used

Mix silicon powder and boron powder under an inert atmosphere, perform hot-pressing sintering and annealing processes to prepare a conductive silicon target. By adjusting the amount of boron powder and sintering conditions, the conductive performance is improved and the thermal stress of the target is reduced.

Benefits of technology

It is possible to improve the electrical conductivity without reducing the quality of the target material, reduce the possibility of target cracking through the annealing process, and improve the density and qualification rate of the target material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the field of target materials, and discloses a preparation method of a conductive silicon target, which comprises the following steps: step 1, mixing silicon powder and boron powder to obtain mixed powder; 2, the mixed powder is subjected to hot pressing sintering at the temperature of 1000-1100 DEG C and then annealed; and step 3, cooling and demolding to obtain the silicon target. The conductivity of the target material can be improved by doping the boron powder, and the possibility of cracking of the target material can be greatly reduced by setting an annealing process after sintering. In addition, the invention also discloses the conductive silicon target prepared by the preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of target materials, and relates to a conductive target material and preparation thereof, and specifically to a conductive silicon target and a preparation method thereof. Background Art

[0002] As a key sputtering coating material, polysilicon targets are widely used in optics, electronics and other fields. Currently, polysilicon targets are mainly classified into high resistivity targets (resistivity>0.5Ω·cm) and low resistivity targets (resistivity<0.002Ω·cm) based on resistivity. During the preparation of polysilicon targets, a certain amount of boron needs to be added to adjust the resistivity. The outer layer of the B atom has only three valence electrons, and one atom is missing to replace silicon to form the original four covalent bonds. Therefore, the valence electrons of the adjacent silicon atoms need to jump over to fill the gap, leaving a hole. This hole can carry current and form a p-type semiconductor.

[0003] In the production process of low-resistance polysilicon ingots, the resistivity is usually controlled by adding boron alloys. However, metal impurities are easily introduced when adding boron alloys, resulting in reduced quality of the silicon target and affecting the subsequent use of the silicon target. Summary of the invention

[0004] In view of the defects and shortcomings of the prior art, in a first aspect, the present invention provides a method for preparing a conductive silicon target; in a second aspect, the present invention provides a conductive silicon target prepared by the above preparation method.

[0005] In a first aspect, a method for preparing a conductive silicon target comprises the following steps: Step 1, mixing silicon powder and boron powder under an inert atmosphere to obtain a mixed powder; Step 2, hot pressing and sintering the mixed powder at 1000-1100° C. and then annealing; Step 3, cooling and demoulding to obtain the silicon target.

[0006] Preferably, in step 1, the mass of the boron powder in the mixed powder is 100 to 300 ppm.

[0007] Preferably, the particle size of the silicon powder is ≤150 μm; and the particle size of the boron powder is ≤100 μm.

[0008] Preferably, the purity of silicon powder is 4N; the purity of boron powder is 3N.

[0009] Preferably, in step 2, the heating rate is 8-12° C. / min; the hot pressing sintering time is 90-120 min; and the hot pressing sintering pressure is 60-70 MPa.

[0010] More preferably, in step 2, after the temperature is raised to 1000-1100° C., it is kept at this temperature for 90-120 min; the mixed powder is pressed at a pressure of 60-70 MPa for 20 min, and the mixed powder is continuously pressed until the temperature drops.

[0011] Preferably, in step 2, during annealing, the temperature is lowered to 500-600° C. at a rate of 3-5° C. / min and maintained at that temperature for 120-180 min.

[0012] In a second aspect, a conductive silicon target is prepared by the above preparation method.

[0013] Preferably, the relative density of the conductive silicon target is greater than 95%; the resistivity of the conductive silicon target is less than 1Ω•cm Compared with the prior art, the present invention has the following obvious beneficial effects: The conductivity of the target material can be increased by doping with boron powder, and an annealing process is provided after sintering, which can greatly reduce the possibility of cracking of the target material. DETAILED DESCRIPTION

[0014] The present invention provides the following specific technical solutions.

[0015] Mixing: Mix 4N or higher silicon powder and 3N or higher boron powder in an inert atmosphere to obtain a mixed powder; wherein the silicon powder particle size is ≤150μm, the boron powder particle size is ≤100μm, and the amount of boron powder is 100-300ppm; Hot pressing sintering: put the mixed powder into a mold, put it into a vacuum hot pressing furnace, heat it to 1000-1100°C at 8-12°C / min, and keep it warm for 90-120min; after heating to 1000-1100°C, pressurize it to 60-70Mpa within 20min to press the mixed powder, and keep the pressure until cooling; Annealing: cool down to 500-600℃ at 3-5℃ / min, keep warm for 120-180min.

[0016] After cooling to room temperature, demolding is performed and the silicon target is obtained through mechanical processing.

[0017] During mixing, the mass of boron powder in the mixed powder is 100-300 ppm.

[0018] In practical applications, the amount of boron powder added can be adjusted according to actual conditions. If the amount of boron powder added is too little, the effect of improving the conductive properties will be limited.

[0019] During the hot pressing sintering process, the sintering temperature affects the density of the target material. If the sintering temperature is too low, the target material density will be low; if the sintering temperature is too high, the target material density will not increase with the increase of temperature, but will increase the thermal stress inside the target material. The hot pressing sintering process is combined with the annealing process to reduce the thermal stress inside the target material and avoid cracking of the target material.

[0020] In order to make the technical problems, technical solutions and technical advantages to be solved by the present invention more clear, they will be described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the following specific embodiments.

[0021] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0022] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0023] Embodiment 1: A method for preparing a conductive silicon target comprises the following steps: Step 1: put 1000 g of 4N pure silicon powder and 0.12 g of 3N pure boron powder into an atmosphere mixer, mix them evenly, and obtain a mixed powder; wherein the particle size of the silicon powder is ≤150 μm, and the particle size of the boron powder is ≤100 μm.

[0024] Step 2: Load the mixed powder into the mold with a filling height of 13 mm. Then place the mold in a vacuum hot pressing furnace and heat it to 1100°C at a heating rate of 10°C / min and keep it warm for 90 minutes. After heating to 1100°C, pressurize the mixed powder in the mold to 60 MPa within 20 minutes and continue pressing until it cools down.

[0025] Step 3, cool down to 600°C at 3°C / min and keep warm for 120 min.

[0026] Step 4, after naturally cooling down to room temperature, demolding, and obtaining a conductive silicon target.

[0027] Embodiment 2: A method for preparing a conductive silicon target comprises the following steps: Step 1, put 2000g of silicon powder with a purity of 4N and 0.3g of boron powder with a purity of 3N into an atmosphere mixer, mix them evenly, and obtain a mixed powder; wherein the particle size of the silicon powder is ≤150μm, and the particle size of the boron powder is ≤100μm.

[0028] Step 2: Load the mixed powder into the mold with a filling height of 10 mm. Then place the mold in a vacuum hot pressing furnace and heat it to 1000°C at a heating rate of 8°C / min and keep it warm for 110 minutes. After heating to 1000°C, pressurize the mixed powder in the mold to 65 MPa within 20 minutes and continue pressing until it cools down.

[0029] Step 3, cool down to 500°C at 4°C / min and keep warm for 150 min.

[0030] Step 4, after naturally cooling down to room temperature, demolding, and obtaining a conductive silicon target.

[0031] Embodiment 3: A method for preparing a conductive silicon target comprises the following steps: Step 1: put 1000 g of 4N pure silicon powder and 0.2 g of 3N pure boron powder into an atmosphere mixer, mix them evenly, and obtain a mixed powder; wherein the particle size of the silicon powder is ≤150 μm, and the particle size of the boron powder is ≤100 μm.

[0032] Step 2: Load the mixed powder into the mold with a filling height of 10 mm. Then place the mold in a vacuum hot pressing furnace for hot pressing. Then heat the temperature to 1200°C at a heating rate of 12°C / min and keep it warm for 110 minutes. After heating to 1200°C, pressurize it to 70 MPa within 20 minutes and keep the pressure until cooling.

[0033] Step 3, cool down to 600°C at 5°C / min and keep warm for 180 min.

[0034] Step 4, after naturally cooling down to room temperature, demolding, and obtaining a conductive silicon target.

[0035] Comparative Example 1: A method for preparing a conductive silicon target comprises the following steps: Step 1, prepare 1000g of silicon powder with a purity of 4N and a particle size of ≤150μm.

[0036] Step 2: Load silicon powder into the mold with a filling height of 13 mm for the mixed powder in the mold. Then place the mold in a vacuum hot pressing furnace and heat it to 1100°C at a heating rate of 10°C / min and keep it warm for 90 minutes. After heating to 1100°C, pressurize the mixed powder in the mold to 60 MPa within 20 minutes and continue pressing until it cools down.

[0037] Step 3, cool down to 600°C at 3°C / min and keep warm for 120 min.

[0038] Step 4, after naturally cooling down to room temperature, demoulding, and mechanical processing to obtain a silicon target.

[0039] Comparative Example 2: A method for preparing a conductive silicon target comprises the following steps: Step 1: put 1000 g of 4N pure silicon powder and 0.12 g of 3N pure boron powder into an atmosphere mixer, mix them evenly, and obtain a mixed powder; wherein the particle size of the silicon powder is ≤150 μm, and the particle size of the boron powder is ≤100 μm.

[0040] Step 2: Load the mixed powder into the mold with a filling height of 13 mm. Then place the mold in a vacuum hot pressing furnace and heat it to 850°C at a heating rate of 10°C / min for 90 minutes. After heating to 1100°C, pressurize the mixed powder in the mold to 60 MPa within 20 minutes and continue pressing until it cools down.

[0041] Step 3, cool down to 600°C at 3°C / min and keep warm for 120 min.

[0042] Step 4, after naturally cooling down to room temperature, demoulding, and mechanical processing to obtain a silicon target.

[0043] Comparative Example 3: A method for preparing a conductive silicon target comprises the following steps: Step 1: put 1000 g of 4N pure silicon powder and 0.12 g of 3N pure boron powder into an atmosphere mixer, mix them evenly, and obtain a mixed powder; wherein the particle size of the silicon powder is ≤150 μm, and the particle size of the boron powder is ≤100 μm.

[0044] Step 2: Load the mixed powder into the mold with a filling height of 13 mm. Then place the mold in a vacuum hot pressing furnace and heat it to 1100°C at a heating rate of 10°C / min and keep it warm for 90 minutes. After heating to 1100°C, pressurize the mixed powder in the mold to 60 MPa within 20 minutes and continue pressing until it cools down.

[0045] Step 3, after natural cooling to room temperature, demoulding, and mechanical processing to obtain a silicon target.

[0046] The resistivity and density of the silicon targets prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested. The test results are shown in Table 1.

[0047] Table 1 - Resistivity and density of silicon targets obtained in Examples 1 to 3 and Comparative Examples 1 to 3 It can be seen from Comparative Example 1 that the silicon target made of only silicon powder is not conductive and has a very high resistivity, and the conductivity of the silicon target can be enhanced by adding a small amount of boron. By comparing Example 1 with Comparative Example 2, it can be seen that the density of the silicon target decreases as the sintering temperature decreases.

[0048] It was observed that no cracks were generated on the surface of the silicon target prepared in Example 1; cracks appeared on the surface of the silicon target prepared in Comparative Example 3. It can be seen that the internal stress of the silicon target was reduced after annealing. In the process of producing silicon targets, the annealing process can improve the qualified rate of silicon targets and reduce costs.

[0049] The embodiments described above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and concepts of the present invention within the technical scope of the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a conductive silicon target, characterized in that: The steps include: Step 1, mixing silicon powder and boron powder under an inert atmosphere to obtain a mixed powder; Step 2, hot pressing and sintering the mixed powder at 1000-1100° C. and then annealing; Step 3, cooling and demoulding to obtain the silicon target.

2. The method for preparing a conductive silicon target according to claim 1, characterized in that: In step 1, the mass of the boron powder in the mixed powder is 100 to 300 ppm.

3. The method for preparing a conductive silicon target according to claim 1, wherein: In step 2, the heating rate is 8-12° C. / min; the hot pressing sintering time is 90-120 min; and the hot pressing sintering pressure is 60-70 MPa.

4. The method for preparing a conductive silicon target according to claim 1 or 3, characterized in that: In step 2, when the temperature is raised to 1000-1100° C., it is kept at this temperature for 90-120 minutes; the mixed powder is pressed at 60-70 MPa for 20 minutes, and the mixed powder is continuously pressed until the temperature drops.

5. The method for preparing a conductive silicon target according to claim 1 or 3, characterized in that: In step 2, during annealing, the temperature is lowered to 500-600°C at a rate of 3-5°C / min and maintained at that temperature for 120-180 minutes.

6. The method for preparing a conductive silicon target according to claim 1 or 2, characterized in that: The particle size of silicon powder is ≤150μm; the particle size of boron powder is ≤100μm; the purity of silicon powder is 4N; the purity of boron powder is 3N.

7. A conductive silicon target, characterized in that: Prepared by the preparation method described in any one of claims 1 to 6.

8. The conductive silicon target according to claim 7, characterized in that: The relative density of the conductive silicon target is greater than 95%; the resistivity of the conductive silicon target is less than 1Ω•cm.