A production process of rubber active microfiber skeleton material
By performing plasma surface treatment and nano calcium carbonate homogenization treatment on carbon fiber powder, combined with composite active additives and rubber latex spinning, a rubber active microfiber skeleton material with smaller fineness is formed, and fibers and rubbers in the prior art are solved. The problem of poor adhesion of the substrate significantly improves the adhesion and interface bonding of the material.
Patent Information
- Application Number
- CN202411226059.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The adhesion between the existing rubber fiber skeleton materials and the rubber matrix is poor, resulting in easy dissolution or separation during use, and insufficient interface bonding force, affecting the flexibility of the composite material.
By plasma surface treatment of carbon fiber powder, the surface contains oxygen functional groups, combined with nano calcium carbonate and composite active additives for low-speed shear homogenization, and then mixed with rubber latex to form rubber active microfibers with a diameter of 25~50μm Skeleton material, improving adhesion and interface bonding between fibers and rubber matrix.
It significantly improves the adhesion and interface bonding between rubber active microfiber skeleton materials and rubber matrix, enhances the fineness and uniformity of fiber skeleton materials, and is suitable for large-scale production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a production process of a rubber active microfiber skeleton material, belonging to the technical field of rubber production. Background Art
[0002] Rubber fiber skeleton material is one of the important raw materials that affects the development of the rubber industry. As the skeleton layer of rubber products, rubber fiber skeleton material is the main stress-bearing layer of rubber products. It is widely used in rubber products such as tires, hoses, belts and seals, and plays a role in strengthening and supporting rubber products. However, some existing rubber fiber skeleton materials, such as carbon fiber, have certain problems: 1) The adhesion with the rubber matrix is poor, and the rubber products formed by combining with rubber will delaminate or separate during use; 2) The interfacial bonding force between the rubber matrix and the rubber matrix is weak, which may affect the flexural resistance of the composite material. Summary of the invention
[0003] In order to address at least one problem existing in the above-mentioned prior art, the present invention provides a process for producing a rubber active microfiber skeleton material, which is capable of producing a rubber active microfiber skeleton material with good activity and smaller fineness, thereby greatly improving the adhesion and interfacial bonding strength between the rubber active microfiber skeleton material and the rubber matrix.
[0004] In order to achieve the above object, the present invention adopts the following technical scheme: a production process of rubber active microfiber skeleton material, comprising the following steps:
[0005] (1) treating the carbon fiber powder with plasma to form carbon fiber powder having oxygen functional groups on the surface;
[0006] (2) The carbon fiber powder and nano-calcium carbonate having oxygen functional groups on the surface are homogenized at a low speed and heated to 155-165° C., a composite active agent is added, and the mixture is homogenized at a low speed at a temperature of 155-165° C. for 5-10 minutes, and then the mixture is cooled to room temperature during the low speed shear homogenization to obtain an active mixture;
[0007] (3) The active mixture is mixed with rubber latex and polyacrylic acid latex, and then sheared and homogenized at a low speed to form an active fiber latex solution, which is then wet-spun to form a filamentous rubber active microfiber skeleton material with a diameter of 25 to 50 μm.
[0008] Preferably, the production process of the rubber active microfiber skeleton material further comprises: slicing the above-mentioned filamentous rubber active microfiber skeleton material, wherein the thickness of the slices is 5-50 μm, and drying to obtain powdery rubber active microfiber skeleton material.
[0009] Preferably, the plasma conditions are as follows: the plasma radio frequency power is 120-150 W, the time is 4-5 min; and the plasma gas is oxygen.
[0010] Preferably, the low-speed shear homogenization condition is: a rotation speed of 250-350 rpm.
[0011] Preferably, the mass ratio of the carbon fiber powder containing oxygen functional groups, nano-calcium carbonate, and composite active additive is 100:5~8:3~4.
[0012] Preferably, the mass ratio of the active mixture, rubber latex and polyacrylic acid latex is 5:80-90:0.4-0.5.
[0013] Preferably, the rubber latex is a mixture of rubber and an aliphatic hydrocarbon organic solvent, and the mass ratio of the rubber to the aliphatic hydrocarbon organic solvent is 1:25.
[0014] Preferably, the rubber latex is one or more of styrene-butadiene rubber latex, natural rubber latex, EPDM latex or butyl rubber latex.
[0015] Preferably, the aliphatic hydrocarbon organic solvent is one of cyclohexane, n-heptane and the like.
[0016] Preferably, the composite active agent is prepared by mixing a silane coupling agent and a titanate coupling agent in a mass ratio of 3 to 5:1.
[0017] Preferably, the silane coupling agent is one of silane coupling agent KH560, silane coupling agent KH570 and silane coupling agent Si69.
[0018] Preferably, the titanate coupling agent is one of titanate coupling agent TMC-101 or titanate coupling agent TMC-102.
[0019] Preferably, the particle size of the carbon fiber powder is 2000-2500 mesh.
[0020] Preferably, the preparation method of the carbon fiber powder is as follows: the filamentary carbon fiber is placed in a crusher for crushing to 125-150 meshes, then placed in a grinder for grinding to 500-600 meshes, and finally placed in an air flow mill for ultrafine grinding to 2000-2500 meshes to obtain carbon fiber powder.
[0021] The beneficial effects of the present invention are as follows: the production process of the present invention activates the carbon fiber, and further activates it through a composite active agent, so that the fiber skeleton material has good activity; at the same time, through the action of nano-calcium carbonate, the dispersibility of the carbon fiber powder containing oxygen functional groups can be effectively improved, which is beneficial to improving the fineness and uniformity of the fiber skeleton material; the production process of the present invention mixes the activated carbon fiber powder containing oxygen functional groups, nano-calcium carbonate, rubber emulsion, and polyacrylic acid emulsion to form microfibers with a diameter of tens of microns during the spinning process, thereby obtaining a rubber active microfiber skeleton material, and at the same time, it can also promote the improvement of the adhesion and interface bonding between the rubber active microfiber skeleton material and the rubber matrix; the production process of the present invention has simple steps and is easy to operate, and can be well adapted to large-scale production and use. DETAILED DESCRIPTION
[0022] The following is a clear and complete description of the technical solutions in the implementation of the present invention. The described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents, instruments, and components used, they are all conventional products that can be purchased commercially.
[0023] The carbon fiber powder used in the present invention has a particle size of 2000-2500 meshes, and is prepared by the following process: placing the filamentary carbon fiber in a crusher for crushing to 125-150 meshes, then placing it in a grinder for grinding to 500-600 meshes, and finally placing it in an air flow mill for ultrafine grinding to 2000-2500 meshes to obtain the carbon fiber powder.
[0024] The rubber latex used in the present invention is a mixture of rubber and an aliphatic hydrocarbon organic solvent, wherein the rubber and the aliphatic hydrocarbon organic solvent are in a mass ratio of 1:25, and is prepared by the following process: firstly, the rubber and the aliphatic hydrocarbon organic solvent are mixed in a mass ratio of 1:10, so that the rubber swells in the aliphatic hydrocarbon organic solvent for 18 to 24 hours, and then an aliphatic hydrocarbon organic solvent of 15 times the mass of the rubber is added, and the mixture is stirred and mixed uniformly to obtain the rubber latex; the aliphatic hydrocarbon organic solvent is one of cyclohexane, n-heptane, etc., and cyclohexane is preferred; the rubber latex is one or more of styrene-butadiene rubber latex, natural rubber latex, ethylene-propylene-diene rubber latex or butyl rubber latex.
[0025] Example
[0026] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0027] (1) The carbon fiber powder is surface treated by plasma, the plasma radio frequency power is 120-150W, the time is 4-5min, and the plasma gas is oxygen, so as to form a carbon fiber powder with oxygen functional groups on the surface;
[0028] (2) The carbon fiber powder and nano calcium carbonate containing oxygen functional groups on the surface are homogenized at a speed of 250-350 rpm and heated to 155-165° C., a composite active additive prepared by mixing a silane coupling agent and a titanate coupling agent in a mass ratio of 3-5:1 is added, and the mixture is homogenized at a temperature of 155-165° C. and a speed of 250-350 rpm for 5-10 min, and then cooled to room temperature after low-speed shear homogenization to obtain an active mixture; the mass ratio of the carbon fiber powder containing oxygen functional groups, the nano calcium carbonate and the composite active additive is 100:5-8:3-4; the silane coupling agent is one of silane coupling agent KH560, silane coupling agent KH570 and silane coupling agent Si69; the titanate coupling agent is one of titanate coupling agent TMC-101 or titanate coupling agent TMC-102;
[0029] (3) The active mixture is mixed with rubber latex and polyacrylic acid emulsion, and then sheared and homogenized at a low speed of 250-350 rpm to form an active fiber latex solution, which is then wet-spun to form a filamentous rubber active microfiber skeleton material with a diameter of 25-50 μm; the mass ratio of the active mixture, rubber latex and polyacrylic acid emulsion is 5:80-90:0.4-0.5.
[0030] In addition, according to needs, the production process of the rubber active microfiber skeleton material of the present invention also includes: rolling and bundling the above-mentioned filamentous rubber active microfiber skeleton material into bundles, then slicing the slices with a thickness of 5-50 μm, and drying to obtain powdered rubber active microfiber skeleton material.
[0031] Example 1
[0032] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0033] (1) The carbon fiber powder is surface treated by plasma, the plasma radio frequency power is 135 W, the time is 5 min, and the plasma gas is oxygen, so as to form a carbon fiber powder with oxygen functional groups on the surface;
[0034] (2) The carbon fiber powder and nano-calcium carbonate containing oxygen functional groups on the surface are homogenized at a low speed of 300 rpm and heated to 155-165° C., a composite active additive prepared by mixing silane coupling agent KH560 and titanate coupling agent TMC-101 in a mass ratio of 3:1 is added, and the mixture is homogenized at a low speed of 155-165° C. and a speed of 300 rpm for 8 min, and then the mixture is cooled to room temperature after low speed shear homogenization at a speed of 300 rpm to obtain an active mixture; the mass ratio of the carbon fiber powder containing oxygen functional groups, nano-calcium carbonate, and the composite active additive is 100:5:3;
[0035] (3) The active mixture is mixed with butyl rubber latex and polyacrylic acid latex, and then sheared and homogenized at a low speed of 300 rpm to form an active fiber latex solution, and then wet-spun to form a filamentous rubber active microfiber skeleton material with a diameter of 25 to 50 μm; the mass ratio of the active mixture, butyl rubber latex, and polyacrylic acid latex is 5:80:0.4;
[0036] In addition, according to needs, the filamentous rubber active microfiber skeleton material of this embodiment can be rolled into bundles, and then sliced, and the thickness of the slices is 5-50 μm, and dried to obtain the rubber active microfiber skeleton material.
[0037] Example 2
[0038] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0039] The difference from Example 1 is that the mass ratio of the active mixture, the butyl rubber emulsion and the polyacrylic acid emulsion is 5:85:0.45, and the rest is exactly the same.
[0040] Example 3
[0041] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0042] The difference from Example 1 is that the mass ratio of the active mixture, the butyl rubber emulsion and the polyacrylic acid emulsion is 5:90:0.5, and the rest is exactly the same.
[0043] Example 4
[0044] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0045] The difference from Example 1 is that styrene-butadiene rubber latex is used, and the mass ratio of the active mixture, styrene-butadiene rubber latex and polyacrylic acid emulsion is 5:90:0.4, and the rest is exactly the same.
[0046] Example 5
[0047] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0048] The difference from Example 1 is that EPDM latex is used, and the mass ratio of the active mixture, EPDM latex and polyacrylic acid latex is 5:80:0.45, and the rest is exactly the same.
[0049] Example 6
[0050] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0051] The difference from Example 1 is that the mass ratio of the carbon fiber powder containing oxygen functional groups, nano calcium carbonate and the composite active additive is 100:6:3.5, and the rest is exactly the same.
[0052] Example 7
[0053] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0054] The difference from Example 1 is that the mass ratio of the carbon fiber powder containing oxygen functional groups, nano-calcium carbonate and the composite active additive is 100:8:3.5, and the rest is exactly the same.
[0055] Example 8
[0056] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0057] The difference from Example 1 is that the mass ratio of the carbon fiber powder containing oxygen functional groups, nano-calcium carbonate and the composite active additive is 100:7:4, and the rest is exactly the same.
[0058] Example 9
[0059] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0060] The difference from Example 1 is that the composite active agent is prepared by mixing silane coupling agent KH570 and titanate coupling agent TMC-102 in a mass ratio of 4:1, and the rest are exactly the same.
[0061] Example 10
[0062] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0063] The difference from Example 1 is that the composite active agent is prepared by mixing the silane coupling agent Si69 and the titanate coupling agent TMC-101 in a mass ratio of 3.5:1, and the rest are exactly the same.
[0064] Embodiment 11
[0065] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0066] The difference from Example 1 is that the plasma RF power is 120 W and the time is 4 min; the speed of low-speed shear homogenization is 250 rpm, and after adding the composite active additive, low-speed shear homogenization is carried out at a temperature of 155-165° C. and a speed of 250 rpm for 5 min, and the rest is exactly the same.
[0067] Comparative Example 1
[0068] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0069] The difference from Example 1 is that the carbon fiber powder and nano-calcium carbonate are sheared homogenized at a low speed of 300 rpm and heated to 155-165° C., and the mass ratio of the carbon fiber powder, nano-calcium carbonate and the composite active additive is 100:5:3; the surface of the carbon fiber powder is not treated with oxygen functional groups; the rest is exactly the same.
[0070] Comparative Example 2
[0071] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0072] The difference from Example 1 is that: in step (2), the carbon fiber powder containing oxygen functional groups is homogenized at a low speed of 300 rpm and heated to 155-165° C., a composite active additive prepared by mixing silane coupling agent KH560 and titanate coupling agent TMC-101 in a mass ratio of 3:1 is added, and the mixture is homogenized at a low speed of 155-165° C. and a speed of 300 rpm for 8 min, and then the mixture is cooled to room temperature after being homogenized at a low speed of 300 rpm to obtain an active mixture; the mass ratio of the carbon fiber powder containing oxygen functional groups to the composite active additive is 100:3;
[0073] (3) The active mixture is mixed with butyl rubber latex, polyacrylic acid latex and nano-calcium carbonate, and then sheared and homogenized at a low speed of 300 rpm to form an active fiber latex liquid, and then wet-spun to form a filamentous rubber active microfiber skeleton material with a diameter of 25-50 μm; the mass ratio of the active mixture, butyl rubber latex and polyacrylic acid latex is 5:80:0.4; the mass ratio of the carbon fiber powder containing oxygen functional groups and the nano-calcium carbonate is 100:5; the nano-calcium carbonate is not treated with a composite active agent;
[0074] The rest is exactly the same.
[0075] Comparative Example 3
[0076] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0077] The difference from Example 1 is that: in step (2), the carbon fiber powder containing oxygen functional groups is homogenized at a low speed of 300 rpm and heated to 155-165° C., a composite active additive prepared by mixing silane coupling agent KH560 and titanate coupling agent TMC-101 in a mass ratio of 3:1 is added, and the mixture is homogenized at a low speed of 155-165° C. and a speed of 300 rpm for 8 min, and then the mixture is cooled to room temperature after being homogenized at a low speed of 300 rpm to obtain an active mixture; the mass ratio of the carbon fiber powder containing oxygen functional groups to the composite active additive is 100:3; and no nano calcium carbonate is added;
[0078] The rest is exactly the same.
[0079] Comparative Example 4
[0080] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0081] The difference from Example 1 is that: in step (2), the composite active agent is prepared by mixing silane coupling agent KH560 and titanate coupling agent TMC-201 in a mass ratio of 3:1; the rest are exactly the same.
[0082] Comparative Example 5
[0083] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0084] The difference from Example 1 is that in step (2), only silane coupling agent KH560 is added; the mass ratio of carbon fiber powder containing oxygen functional groups, nano calcium carbonate and silane coupling agent KH560 is 100:5:3; and the rest is exactly the same.
[0085] Comparative Example 6
[0086] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0087] The difference from Example 1 is that in step (2), only titanate coupling agent TMC-101 is added; the mass ratio of carbon fiber powder containing oxygen functional groups, nano-calcium carbonate and titanate coupling agent TMC-101 is 100:5:3; and the rest are exactly the same.
[0088] Comparative Example 7
[0089] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0090] The difference from Example 1 is that the particle size of the carbon fiber powder is 500-600 mesh; the rest is exactly the same.
[0091] Comparative Example 8
[0092] A production process of rubber active microfiber skeleton material, the process steps are as follows:
[0093] The difference from Example 1 is that: in step (3), the active mixture and butyl rubber emulsion are added without adding polyacrylic acid emulsion; the mass ratio of the active mixture to the butyl rubber emulsion is 5:90; and the rest are exactly the same.
[0094] The filamentous rubber active microfiber skeleton materials prepared in the above-mentioned Examples 1 to 11 and Comparative Examples 1 to 7 are compounded with rubber: 100 parts by mass of natural rubber are plasticized in an internal mixer, and the following active agents are added in sequence: 5 parts by mass of zinc oxide, 2 parts by mass of stearic acid; 1 part by mass of antioxidant 4010NA; 1 part by mass of coumarone resin; tackifiers: 1 part by mass of RA, 1 part by mass of RS; plasticizer: 10 parts by mass of aromatic oil; and finally, 1 part by mass of sulfur and 4 parts by mass of accelerator CZ are added. The mixed rubber material was packaged into triangles with an open mixer to obtain 5 mm rubber sheets; the mixed rubber was then cut into strips matching the extraction mold and filled into the mold cavity of the extraction test mold, the filamentous rubber active microfiber skeleton material was added to the rubber strip and the mold, and another layer of rubber strip was placed, and the mold was closed; the extraction test specimens were vulcanized on a flat vulcanizer at a vulcanization temperature of 150°C, a vulcanization pressure of 15 MPa, and a vulcanization time of 30 min; then the interfacial strength (IFSS) (MPa) and extraction force (N) of the composite material were tested, and no less than 6 samples were tested, and the average value of at least 6 valid data was recorded. The results are shown in Table 1.
[0095] Table 1
[0096]
[0097] From Table 1 above, it is found that after the rubber active microfiber skeleton material is compounded with the rubber matrix, the rubber active microfiber skeleton material produced by the present invention requires a greater extraction force, and the composite material of the rubber active microfiber skeleton material and the rubber matrix also has a stronger interface strength. Therefore, the adhesion and interface bonding force between the rubber active microfiber skeleton material produced by the present invention and the rubber matrix.
[0098] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit and essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0099] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A process for producing a rubber active microfiber skeleton material, characterized in that: The following steps are involved: (1) treating the carbon fiber powder with plasma to form carbon fiber powder having oxygen functional groups on the surface; the particle size of the carbon fiber powder is 2000-2500 mesh; (2) The carbon fiber powder and nano-calcium carbonate having oxygen functional groups on the surface are homogenized at a low speed and heated to 155-165° C., a composite active agent is added, and the mixture is homogenized at a low speed at a temperature of 155-165° C. for 5-10 minutes, and then the mixture is cooled to room temperature during the low speed shear homogenization to obtain an active mixture; (3) mixing the above active mixture with rubber latex and polyacrylic acid latex, and then shearing and homogenizing at a low speed to form an active fiber latex solution, and then wet spinning to form a filamentous rubber active microfiber skeleton material with a diameter of 25 to 50 μm; The composite active agent is prepared by mixing a silane coupling agent and a titanate coupling agent in a mass ratio of 3 to 5:1; The silane coupling agent is one of silane coupling agent KH560, silane coupling agent KH570 or silane coupling agent Si69; the titanate coupling agent is one of titanate coupling agent TMC-101 or titanate coupling agent TMC-102.
2. A process for producing a rubber active microfiber skeleton material according to claim 1, characterized in that: The plasma conditions are as follows: the plasma radio frequency power is 120-150 W, the time is 4-5 min, and the plasma gas is oxygen.
3. The process for producing a rubber active microfiber skeleton material according to claim 1, characterized in that: The low-speed shear homogenization condition is: the rotation speed is 250~350rpm.
4. The process for producing a rubber active microfiber skeleton material according to claim 1, characterized in that: The mass ratio of the carbon fiber powder containing oxygen functional groups, nano calcium carbonate and composite active additive is 100:5-8:3-4.
5. The process for producing a rubber active microfiber skeleton material according to claim 1, characterized in that: The mass ratio of the active mixture, rubber latex and polyacrylic acid latex is 5:80-90:0.4-0.
5.
6. The process for producing a rubber active microfiber skeleton material according to claim 1, characterized in that: The rubber latex is a mixture of rubber and an aliphatic hydrocarbon organic solvent, and the mass ratio of the rubber to the aliphatic hydrocarbon organic solvent is 1:
25.
7. A process for producing a rubber active microfiber skeleton material according to claim 6, characterized in that: The rubber latex is one or more of styrene-butadiene latex, natural rubber latex, EPDM latex or butyl latex; the aliphatic hydrocarbon organic solvent is one of cyclohexane and n-heptane.
8. The process for producing a rubber active microfiber skeleton material according to claim 1, characterized in that: The preparation method of the carbon fiber powder comprises the following steps: placing the filamentary carbon fiber in a crusher to crush it to 125-150 meshes, placing it in a grinder to grind it to 500-600 meshes, and finally placing it in an air flow mill to ultrafinely grind it to 2000-2500 meshes to obtain the carbon fiber powder.