Low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament and preparation method thereof

By using a new type of phosphorus-nitrogen-containing nano-flame retardant in ultra-high molecular weight polyethylene fiber to form a flame-retardant carbon layer and metal oxide, the problem of flammability and strength reduction of UHMWPE fiber is solved, achieving both high flame-retardant performance and strength. effect.

CN118727181AActive Publication Date: 2024-10-01NANTONG NTEC MONOFILAMENT TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410842926.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-01
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing ultra-high molecular weight polyethylene (UHMWPE) fibers are flammable when burned and produce a large amount of smoke. In order to improve the flame retardant performance, a large amount of flame retardants need to be added, resulting in a reduction in fiber strength.

Method used

Using a new phosphorus-containing nitrogen nano-flame retardant, flame-retardant substances such as ammonia and phosphoric acid are generated through thermal decomposition at high temperatures to form a carbonized surface layer and metal oxide, which are combined with silicon dioxide to form a C-Si bonded flame-retardant carbon layer, which significantly Improve the flame retardant properties of fibers while reducing the use of flame retardants.

Benefits of technology

While meeting the high flame retardant performance, it maintains the strength of the fiber, reduces the impact of the flame retardant on the strength of the fiber, and improves the limiting oxygen index, smoke suppression performance and droplet prevention performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727181A_ABST
    Figure CN118727181A_ABST
Patent Text Reader

Abstract

The invention discloses a low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament comprises the following components in parts by weight: 65-75 parts of ultra-high molecular weight polyethylene, 25-35 parts of high-density polyethylene, 2-5 parts of a novel phosphorus-nitrogen-containing nano flame retardant, 1-4 parts of an antioxidant and 1-2.5 parts of a lubricant. According to the low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament and the preparation method thereof provided by the invention, the novel phosphorus-nitrogen-containing nano flame retardant with better flame retardant property is used in the monofilament, so that the content of the flame retardant in the polyethylene monofilament is low when the ultra-high molecular weight polyethylene monofilament meets the required high flame retardant property, that is, the use amount of the flame retardant is reduced, and the production cost is reduced. The influence of the flame retardant on the strength and other mechanical properties of the ultra-high molecular weight polyethylene monofilament is reduced, so that the low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament has high flame retardance and better strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention generally relates to the technical field of monofilaments, and in particular to low-smoke flame-retardant ultra-high molecular weight polyethylene monofilaments and a preparation method thereof. Background Art

[0002] Ultra-high molecular weight polyethylene (UHMWPE) fiber is a new generation of high-performance fiber made from linear polyethylene with a molecular weight of more than 1 million. UHMWPE fiber is widely used in marine ropes and protective nets, fishing lines, cut-resistant gloves, lightweight bulletproof armor and other products due to its advantages of light weight, weak adhesion, low surface tension, strong impact resistance, good chemical resistance, good cut resistance, self-lubrication, etc. UHMWPE fiber is flammable and will produce large amounts of smoke and molten droplets during the combustion process, so flame retardants are added to existing UHMWPE fibers to improve the safety of UHMWPE fibers.

[0003] Since the flame retardant properties of existing flame retardants are average, in order to meet the high flame retardant properties of UHMWPE fibers, more flame retardants need to be added to the UHMWPE fibers, resulting in a decrease in the strength of the UHMWPE fibers. Summary of the invention

[0004] In view of the above-mentioned defects or deficiencies in the prior art, it is desirable to provide a low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament and a preparation method thereof.

[0005] In a first aspect, the present application provides a low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament, comprising the following components in parts by weight:

[0006] 65-75 parts of ultra-molecular weight polyethylene, 25-35 parts of high-density polyethylene, 2-5 parts of phosphorus-nitrogen nano flame retardant, 1-4 parts of antioxidant, 1-2.5 parts of lubricant;

[0007] Wherein, the phosphorus-nitrogen-containing nano flame retardant is prepared by the following preparation method:

[0008] S100: adding nano-silica particles, a silane modifier and an acidic pH value regulator to a 60-90% ethanol aqueous solution in sequence to prepare a first mixed solution, wherein the pH value of the first mixed solution is 3-4, then heating the first mixed solution to 60-70° C. and reacting for 4-6 hours, and then filtering, washing and drying the first mixed solution to prepare nano-silica particles having double bond groups on the surface;

[0009] S200: Under a nitrogen atmosphere, acrylamide and 37% formaldehyde solution are mixed in an aqueous solution and then phosphorous acid is added to prepare a second mixed solution, and then the second mixed solution is heated to 60-70° C. and reacted for 1-3 hours to prepare an acryl diphosphoric acid flame retardant solution;

[0010] S300: mixing nano-silica particles containing double bond groups and an initiator in an acryloyl diphosphoric acid flame retardant solution to obtain a third mixed solution, and then heating the third mixed solution to 60-70° C. and reacting for 7-9 hours to prepare nano-silica modified particles;

[0011] S400: Add nano-silica modified particles and alkaline pH regulator to the aqueous solution in sequence to obtain a fourth mixed solution, the pH value of the fourth mixed solution is 4-6, then add metal salt to the fourth mixed solution and soak for 2-8 hours, and then filter, wash and dry the fourth mixed solution to obtain a phosphorus-nitrogen nano flame retardant.

[0012] Furthermore, the weight ratio of the nano-silica particles to the silane modifier is 1:(0.4-0.6).

[0013] Furthermore, the weight ratio of acrylamide, phosphorous acid, formaldehyde solution, nano-silica particles containing double bond groups and initiator is 100:(230-265):(230-260):(60-70):(6-13).

[0014] Furthermore, the weight ratio of the nano-silicon dioxide modified particles to the metal salt is 1:(0.1-0.2).

[0015] Furthermore, the silane modifier is selected from one or more of vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, and 3-methacryloxypropyltrimethoxysilane.

[0016] Furthermore, the initiator is selected from one or more of sodium persulfate, potassium persulfate, and azobisisobutylcyanide.

[0017] Furthermore, the metal salt is selected from Cu 2+ 、Zn 2+ , Ca 2+ Mg 2+ , Fe 3+ 、A l 3+ One or more of nitrates, acetates, and chlorides.

[0018] Furthermore, the antioxidant is selected from one or more of antioxidant 1010 , antioxidant 168 , and antioxidant 1024 .

[0019] Furthermore, the lubricant is selected from one or more of polyethylene wax and calcium stearate.

[0020] In a second aspect, the present application also provides a method for preparing a low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament, comprising the following steps:

[0021] Mixing ultra-molecular weight polyethylene, high-density polyethylene, phosphorus-nitrogen-containing nano flame retardant, antioxidant, and lubricant to prepare a raw material mixture;

[0022] The raw material mixture is sequentially granulated and spun to obtain low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament.

[0023] The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament and the preparation method thereof provided by the present application use a new type of phosphorus-nitrogen-containing nano flame retardant with better flame retardant properties in the monofilament, so that the ultra-high molecular weight polyethylene monofilament has a low flame retardant content while meeting the required high flame retardant properties, that is, the amount of flame retardant used is reduced, and the influence of the flame retardant on the mechanical properties such as the strength of the ultra-high molecular weight polyethylene monofilament is reduced, thereby achieving the low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament having high flame retardant properties while also having good strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings:

[0025] Figure 1 The preparation route map of the phosphorus-nitrogen-containing nano flame retardant provided in this embodiment;

[0026] Figure 2 This is a flow chart for preparing the low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament provided in this embodiment. DETAILED DESCRIPTION

[0027] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It is also necessary to explain that, for ease of description, only the parts related to the invention are shown in the accompanying drawings.

[0028] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0029] Please refer to the attached Figure 1 The embodiment of the present application provides a low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament, comprising the following components in parts by weight: 65-75 parts of ultra-molecular weight polyethylene, 25-35 parts of high-density polyethylene, 2-5 parts of phosphorus-nitrogen nano flame retardant, 1-4 parts of antioxidant, and 1-2.5 parts of lubricant.

[0030] The phosphorus-nitrogen-containing nano flame retardant in the above components is prepared by the following preparation method:

[0031] S100: adding nano-silica particles, a silane modifier and an acidic pH value regulator to a 60-90% ethanol aqueous solution in sequence to prepare a first mixed solution, wherein the pH value of the first mixed solution is 3-4, then heating the first mixed solution to 60-70° C. and reacting for 4-6 hours, and then filtering, washing and drying the first mixed solution to prepare nano-silica particles having double bond groups on the surface;

[0032] S200: Under a nitrogen atmosphere, acrylamide and 37% formaldehyde solution are mixed in an aqueous solution and then phosphorous acid is added to prepare a second mixed solution, and then the second mixed solution is heated to 60-70° C. and reacted for 1-3 hours to prepare an acryl diphosphoric acid flame retardant solution;

[0033] S300: mixing nano-silica particles containing double bond groups and an initiator in an acryloyl diphosphoric acid flame retardant solution to obtain a third mixed solution, and then heating the third mixed solution to 60-70° C. and reacting for 7-9 hours to prepare nano-silica modified particles;

[0034] S400: Add nano-silica modified particles and alkaline pH regulator to the aqueous solution in sequence to obtain a fourth mixed solution, the pH value of the fourth mixed solution is 4-6, then add metal salt to the fourth mixed solution and soak for 2-8 hours, and then filter, wash and dry the fourth mixed solution to obtain a phosphorus-nitrogen nano flame retardant.

[0035] This embodiment provides a novel phosphorus-nitrogen-containing nano flame retardant, which improves the flame retardant properties of ultra-high molecular weight polyethylene monofilaments through the following aspects, specifically:

[0036] On the one hand, when the ultra-high molecular weight polyethylene monofilament is subjected to high temperature, the phosphorus-nitrogen-containing nano flame retardant will thermally decompose at high temperature to produce nitrogen-containing non-flammable gases such as ammonia; on the other hand, the phosphorus-nitrogen-containing nano flame retardant will also thermally decompose at high temperature to produce phosphoric acid, metaphosphoric acid and other phosphorus-containing flame retardants, which can dehydrate and carbonize the surface layer of the ultra-high molecular weight polyethylene monofilament to form a carbonized surface layer on the surface of the ultra-high molecular weight polyethylene monofilament, and at the same time, polymer cross-linking will be induced between the silicon dioxide in the monofilament and the carbonized surface layer at high temperature, so that a flame-retardant carbon layer with C-Si bonds is formed between the carbonized surface layer and the silicon dioxide; on the third hand, the complexed metal ions in the phosphorus-nitrogen-containing nano flame retardant will thermally decompose to form metal oxides when heated, and the metal oxides are deposited on the surface layer of the ultra-high molecular weight polyethylene monofilament and part of the metal oxides are combined with the flame-retardant carbon layer. The nitrogen-containing non-combustible gas generated above can dilute the oxygen concentration in the environment surrounding the monofilament. The flame-retardant carbon layer and the metal oxide can both block external oxygen and heat from entering the ultra-high molecular weight polyethylene monofilament and reduce the amount of combustible gas decomposed and released from the ultra-high molecular weight polyethylene monofilament. Through the synergistic effect of the nitrogen-containing non-combustible gas and the flame-retardant carbon layer and the metal oxide attached to the surface of the monofilament, the limiting oxygen index, smoke suppression performance and anti-dripping performance of the ultra-high molecular weight polyethylene monofilament can be significantly improved, thereby improving the flame retardant performance of the ultra-high molecular weight polyethylene monofilament. At the same time, the flame retardant carbon layer has good adhesion stability under the dual fixation of the CSi bond and the metal oxide, thereby improving the flame retardant durability of the ultra-high molecular weight polyethylene monofilament.

[0037] In addition, the new phosphorus-nitrogen-containing nano flame retardant provided in this embodiment is not only halogen-free and has a high safety factor, but is also in the form of nanoparticles, so that the phosphorus-nitrogen-containing nano flame retardant can be evenly distributed in the polyethylene resin, thereby improving the distribution uniformity of the phosphorus-nitrogen-containing nano flame retardant in the ultra-high molecular weight polyethylene monofilament.

[0038] Compared with existing flame retardants, since the phosphorus-nitrogen-containing nano flame retardant provided in this embodiment has higher flame retardant properties, the flame retardant content in the ultra-high molecular weight polyethylene monofilament is low while meeting the required high flame retardant properties, that is, the amount of flame retardant used is reduced, and the influence of the flame retardant on the mechanical properties such as the strength of the ultra-high molecular weight polyethylene monofilament is reduced. Therefore, the low-smoke flame retardant ultra-high molecular weight polyethylene monofilament has high flame retardant properties while also having good strength.

[0039] Optionally, in step S100, adding nano-silica particles, silane modifiers and acidic pH regulators in 60-90% ethanol aqueous solution in sequence specifically includes: first adding nano-silica particles to 60-90% ethanol aqueous solution, then ultrasonically dispersing the ethanol aqueous solution containing nano-silica particles for 5-10 minutes to uniformly disperse the nano-silica particles in the ethanol aqueous solution, then adding the silane modifier, and continuing to add the acidic pH regulator after adding the silane modifier, so that the pH value of the first mixed solution is 3-4 to promote the hydrolysis of silane. After the reaction is completed, the first mixed solution is filtered to obtain solid matter, and the solid matter is washed with water and dried to obtain nano-silica particles containing double bond groups. Among them, the average particle size of the nano-silica particles can be, but not limited to, 20-30nm, the viscosity average molecular weight of the super molecular weight polyethylene resin can be, but not limited to, between 1 million and 2 million, and the viscosity average molecular weight of the high density polyethylene resin can be 100,000-300,000 and its melt index is 5-10g / 10min. Optionally, the weight ratio of the nano-silica particles to the silane modifier is 1:(0.4-0.6), that is, the weight of the silane modifier is 40%-60% of the weight of the nano-silica particles. Optionally, the silane modifier is selected from one or more of vinyl trimethoxy silane, vinyl triethoxy silane, allyl trimethoxy silane, allyl triethoxy silane, and 3-methacryloxypropyl trimethoxy silane. The acidic pH value regulator is selected from one or more of concentrated hydrochloric acid, concentrated sulfuric acid, and glacial acetic acid.

[0040] Optionally, in steps S200 and S300, after acrylamide and formaldehyde solution are mixed in an aqueous solution, they can be stirred for a period of time before adding phosphorous acid to make the reaction more complete. Nano-silicon dioxide particles containing double bond groups can be added to the acryl diphosphoric acid flame retardant solution before the initiator, and after the third mixed solution reacts, it is filtered and the filtered solid matter is washed and dried to prepare nano-silicon dioxide modified particles. Optionally, the weight ratio of acrylamide, phosphorous acid, formaldehyde solution, nano-silicon dioxide particles containing double bond groups and initiator is 100: (230-265): (230-260): (60-70): (6-13). Optionally, the initiator is selected from one or more of sodium persulfate, potassium persulfate and azobisisobutyl cyanide.

[0041] Optionally, in step S400, the weight ratio of the modified nano-silicon dioxide particles to the metal salt is 1:(0.1-0.2), that is, the weight of the metal salt is 10%-20% of the weight of the modified nano-silicon dioxide particles. Optionally, the metal salt is selected from Cu 2 + 、Zn 2+ , Ca2+ Mg 2+ , Fe 3+ 、A l 3+ One or more of nitrate, acetate, chloride. The alkaline pH value regulator is selected from sodium hydroxide, sodium bicarbonate, etc.

[0042] Optionally, the antioxidant may be, but is not limited to, one or more of antioxidant 1010, antioxidant 168, and antioxidant 1024, which can effectively prevent thermal degradation of the polyethylene resin and improve the aging resistance of the polyethylene resin.

[0043] Optionally, the lubricant may be, but is not limited to, one or more of polyethylene wax and calcium stearate to effectively improve the fluidity of the polyethylene resin.

[0044] Please refer to the attached Figure 2 The present application also provides a method for preparing a low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament, comprising the following steps:

[0045] The ultra-molecular weight polyethylene, high-density polyethylene, phosphorus-nitrogen-containing nano flame retardant, antioxidant, and lubricant are mixed to obtain a raw material mixture;

[0046] The raw material mixture is sequentially granulated and spun to obtain low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament.

[0047] Optionally, the above-mentioned mixing process can be carried out at room temperature using a high-speed mixer, wherein the speed of the high-speed mixer is 800-1000r / min and the mixing time is 10-15min. The raw material mixture is extruded and granulated by a twin-screw extruder, and then single-screw melt spinning is used and the spinning is water-cooled, high-multiple hot stretched and wound to prepare low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament. Among them, the extrusion temperature of the twin-screw extruder can be but not limited to 280-290°C, the single-screw spinning temperature can be but not limited to 290-310°C, the high-multiple hot stretching temperature can be but not limited to 70-100°C, and the stretching multiple can be but not limited to 9-12.

[0048] This embodiment adopts melt spinning, which has the advantages of low cost, simple process, no need to use organic solvents, etc. compared with gel spinning, low cost and little impact on the environment.

[0049] In addition, the present application also provides the following examples to illustrate the flame retardant properties and mechanical properties of the ultra-high molecular weight polyethylene monofilament provided in the present application, as follows:

[0050] Embodiment 1:

[0051] Preparation of phosphorus-nitrogen-containing nano flame retardant:

[0052] 10 g of nano-silica particles were added to an ethanol aqueous solution with a concentration of 80% and ultrasonically dispersed for 10 min, then 4 g of allyltriethoxysilane was added, and then glacial acetic acid was added to adjust the solution to obtain a first mixed solution, the pH value of the first mixed solution was 3.5, and then the first mixed solution was heated to 70° C. and reacted for 4 h. After the reaction was completed, the first mixed solution was filtered, washed with water and dried to obtain nano-silica particles containing double bond groups on the surface;

[0053] In a nitrogen atmosphere, 21.03 g of acrylamide and 48.69 g of formaldehyde solution were mixed and dissolved in 20 g of water, stirred for a period of time, and 49.2 g of phosphorous acid was added to prepare a second mixed solution, and then the second mixed solution was heated to 70° C. and reacted for 2 h to prepare a colorless and transparent acryloyl diphosphoric acid flame retardant solution;

[0054] 13 g of nano-silica particles containing double bond groups were added to the acryl diphosphoric acid flame retardant solution prepared above, and then 1.6 g of potassium persulfate was added to prepare a third mixed solution, and then the third mixed solution was heated to 60° C. and reacted for 4 hours. After the reaction, the third mixed solution was filtered and dried to prepare nano-silica modified particles.

[0055] 20 g of nano-silica modified particles were immersed in a NaOH aqueous solution to obtain a fourth mixed solution, and the pH value of the fourth mixed solution reached 4.5. Subsequently, 2 g of anhydrous calcium chloride was added to the fourth mixed solution and immersed for 4 hours. The fourth mixed solution was then filtered, washed with water and dried to obtain a phosphorus-nitrogen nano flame retardant.

[0056] Preparation of ultra-high molecular weight polyethylene monofilament:

[0057] 700g of ultra-high molecular weight polyethylene resin, 300g of high-density polyethylene resin, 40g of phosphorus-nitrogen nano flame retardant, 10g of antioxidant 1010, and 15g of calcium stearate were mixed in a high-speed mixer at room temperature for 10 minutes, then put into a twin-screw extruder, extruded and granulated at 280°C, and then single-screw melt spinning, water cooling, high-multiple hot stretching and winding were carried out in sequence to obtain low-smoke flame-retardant ultra-high molecular weight polyethylene monofilaments after winding. Among them, the spinning temperature is 300°C, the hot stretching temperature is 80°C, the initial stretching multiple is 5, and the high-multiple stretching multiple is 11.

[0058] Embodiment 2:

[0059] Preparation of phosphorus-nitrogen-containing nano flame retardant:

[0060] 25 g of nano-silica particles are added to an ethanol aqueous solution with a concentration of 70% and ultrasonically dispersed for 10 minutes, then 12.5 g of 3-methacryloxypropyltrimethoxysilane is added, and then glacial acetic acid is added to adjust the solution to obtain a first mixed solution, the pH value of the first mixed solution is 4, and then the first mixed solution is heated to 65° C. and reacted for 4 hours. After the reaction is completed, the first mixed solution is filtered, washed with water and dried to obtain nano-silica particles containing double bond groups on the surface;

[0061] In a nitrogen atmosphere, 54.3 g of acrylamide and 125.4 g of formaldehyde solution were mixed and dissolved in water, stirred for a period of time, and 127.2 g of phosphorous acid was added to prepare a second mixed solution, and then the second mixed solution was heated to 70° C. and reacted for 2 h to prepare a colorless and transparent acryloyl diphosphoric acid flame retardant solution;

[0062] 32.6 g of nano-silica particles containing double bond groups were added to the acryl diphosphoric acid flame retardant solution prepared above, and then 4 g of potassium persulfate was added to prepare a third mixed solution, and then the third mixed solution was heated to 60° C. and reacted for 4 hours. After the reaction, the third mixed solution was filtered and dried to prepare nano-silica modified particles.

[0063] 50 g of nano-silica modified particles were immersed in a NaOH aqueous solution to obtain a fourth mixed solution, and the pH value of the fourth mixed solution reached 4.5. Subsequently, 6 g of anhydrous calcium chloride was added to the fourth mixed solution and immersed for 6 hours. The fourth mixed solution was then filtered, washed with water and dried to obtain a phosphorus-nitrogen nano flame retardant.

[0064] Preparation of ultra-high molecular weight polyethylene monofilament:

[0065] 1500g of ultra-high molecular weight polyethylene resin, 642g of high-density polyethylene resin, 80g of phosphorus-nitrogen nano flame retardant, 28.75g of antioxidant 1010, and 42.86g of calcium stearate were mixed in a high-speed mixer at room temperature for 10 minutes, then put into a twin-screw extruder, extruded and granulated at 290°C, and then single-screw melt spinning, water cooling, high-multiple hot stretching and winding were carried out in sequence, and low-smoke flame-retardant ultra-high molecular weight polyethylene monofilaments were obtained after winding. Among them, the spinning temperature is 310°C, the hot stretching temperature is 80°C, the initial stretching multiple is 5.8, and the high stretching multiple is 10.

[0066] Embodiment 3-11:

[0067] Example 3: In the preparation of ultra-high molecular weight polyethylene monofilament, the weight of the phosphorus-nitrogen-containing nano flame retardant is 30 g, and the rest is the same as Example 1.

[0068] Example 4: In the preparation of the phosphorus-nitrogen-containing nano flame retardant, the metal salt is magnesium chloride hexahydrate and weighs 2 g, and the rest is the same as Example 1.

[0069] Example 5: In the preparation of the phosphorus-nitrogen-containing nano flame retardant, the metal salt is anhydrous aluminum chloride and weighs 2 g, and the rest is the same as Example 1.

[0070] Example 6: In the preparation of the phosphorus-nitrogen-containing nano flame retardant, the metal salt is cupric chloride dihydrate and weighs 2 g, and the rest is the same as Example 1.

[0071] Example 7: In the preparation of the phosphorus-nitrogen-containing nano flame retardant, the metal salt is ferric chloride hexahydrate and weighs 5 g, and the rest is the same as Example 2.

[0072] Example 8: In the preparation of the phosphorus-nitrogen-containing nano flame retardant, the metal salt is ferric chloride hexahydrate and weighs 7 g, and the rest is the same as Example 2.

[0073] Example 9: In the preparation of the phosphorus-nitrogen-containing nano flame retardant, the metal salt is ferric chloride hexahydrate and weighs 8 g, and the rest is the same as Example 2.

[0074] Example 10: In the preparation of the phosphorus-nitrogen-containing nano flame retardant, the metal salt is ferric chloride hexahydrate and weighs 9 g, and the rest is the same as Example 2.

[0075] Comparative Example 1:

[0076] Preparation of phosphorus-nitrogen-containing nano flame retardant:

[0077] 10 g of nano-silica particles were added to an ethanol aqueous solution with a concentration of 80% and ultrasonically dispersed for 10 min, then 4 g of allyltriethoxysilane was added, and then glacial acetic acid was added to adjust the solution to obtain a first mixed solution, the pH value of the first mixed solution was 3.5, and then the first mixed solution was heated to 70° C. and reacted for 4 h. After the reaction was completed, the first mixed solution was filtered, washed with water and dried to obtain nano-silica particles containing double bond groups on the surface;

[0078] In a nitrogen atmosphere, 21.03 g of acrylamide and 48.69 g of formaldehyde solution were mixed and dissolved in water, stirred for a period of time, and 49.2 g of phosphorous acid was added to prepare a second mixed solution, and then the second mixed solution was heated to 70° C. and reacted for 2 h to prepare a colorless and transparent acryloyl diphosphoric acid flame retardant solution;

[0079] 13 g of nano-silica particles containing double bond groups were added to the acryl diphosphoric acid flame retardant solution prepared above, and then 1.6 g of potassium persulfate was added to prepare a third mixed solution, and then the third mixed solution was heated to 60° C. and reacted for 4 hours. After the reaction, the third mixed solution was filtered and dried to prepare a phosphorus-nitrogen-containing nano flame retardant.

[0080] Preparation of ultra-high molecular weight polyethylene monofilament:

[0081] 700g of ultra-high molecular weight polyethylene resin, 300g of high-density polyethylene resin, 40g of phosphorus-nitrogen nano flame retardant, 10g of antioxidant 1010, and 15g of calcium stearate were mixed in a high-speed mixer at room temperature for 10 minutes, then put into a twin-screw extruder, extruded and granulated at 280°C, and then single-screw melt spinning, water cooling, high-multiple hot stretching and winding were carried out in sequence to obtain low-smoke flame-retardant ultra-high molecular weight polyethylene monofilaments after winding. Among them, the spinning temperature is 300°C, the hot stretching temperature is 80°C, the initial stretching multiple is 5.7, and the high-multiple stretching multiple is 11.6.

[0082] Comparative Example 2:

[0083] 700g of ultra-high molecular weight polyethylene resin, 300g of high-density polyethylene resin, 40g of phosphorus nitrogen flame retardant (the flame retardant is HF-831 flame retardant produced by Anhui Stable Jiaxin Material Technology Co., Ltd.), 8g of antioxidant 1010, and 14g of calcium stearate are mixed in a high-speed mixer at room temperature for 10 minutes, then put into a twin-screw extruder, extruded and granulated at 280°C, and then single-screw melt spinning is adopted, the spinning temperature is 290°C, water cooling, the initial stretching ratio is 5.5, the hot stretching temperature is 80°C, the stretching ratio is 10.3, and the ultra-high molecular weight polyethylene monofilament is obtained after winding.

[0084] Test method:

[0085] (1) Flame retardant performance test: The limiting oxygen index (LOI) of the fiber was tested according to GB / T5454-1997 "Determination of oxygen index of textile combustion performance"; 0.5±0.01g of UHMWPE fiber was placed on a wire mesh, and the fiber was heated with an outer flame. The flame height was controlled at about 4cm, and the melting droplets and smoke generation during the combustion of the fiber were recorded.

[0086] (2) Mechanical properties test: The breaking strength of the fiber was tested according to GB / T4344-2008 “Test method for tensile properties of chemical filaments”, with a tensile distance of 200 mm and a tensile speed of 200 m / min.

[0087] The performance tests were conducted on the ultra-high molecular weight polyethylene monofilaments prepared in the above embodiments, and the test results are shown in the following table:

[0088]

[0089] Based on the above table, we can see that:

[0090] 1. Compared with Comparative Example 2, the low-smoke flame-retardant ultra-high molecular weight polyethylene monofilaments in Examples 1-10 and Comparative Example 1 have significant improvements in limiting oxygen index, smoke emission and anti-dripping effect, while the strength of the ultra-high molecular weight polyethylene monofilament is less affected and not obvious, which further proves that the ultra-high molecular weight polyethylene monofilament provided in the present application has higher flame retardant properties while also ensuring the strength of the monofilament.

[0091] 2. Compared with Comparative Example 1, the low-smoke flame-retardant ultra-high molecular weight polyethylene monofilaments of Examples 1-10 have better limiting oxygen index, smoke emission and anti-dripping effects, which further proves that the phosphorus-nitrogen nano flame retardant encapsulated with metal ions has better flame retardant properties, smoke suppression and anti-dripping effects than the phosphorus-nitrogen nano flame retardant without encapsulated metal ions.

[0092] It should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like used above to indicate orientations or positional relationships are based on the orientations or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention; the orientation words "inside" and "outside" refer to the inside and outside relative to the contours of the components themselves. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0093] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used herein to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" may include both "above" and "below". The device may also be positioned in other different ways, rotated 90 degrees or in other orientations, and the spatially relative descriptions used herein are interpreted accordingly.

[0094] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.

Claims

1. A low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament, characterized in that: The composition comprises the following components in parts by weight: 65-75 parts of ultra-molecular weight polyethylene, 25-35 parts of high-density polyethylene, 2-5 parts of phosphorus-nitrogen nano flame retardant, 1-4 parts of antioxidant, 1-2.5 parts of lubricant; Wherein, the phosphorus-nitrogen-containing nano flame retardant is prepared by the following preparation method: S100: adding nano-silica particles, a silane modifier and an acidic pH value regulator to a 60-90% ethanol aqueous solution in sequence to prepare a first mixed solution, wherein the pH value of the first mixed solution is 3-4, then heating the first mixed solution to 60-70° C. and reacting for 4-6 hours, then filtering, washing and drying the first mixed solution to prepare nano-silica particles having double bond groups on the surface; S200: Under a nitrogen atmosphere, acrylamide and 37% formaldehyde solution are mixed in an aqueous solution and then phosphorous acid is added to prepare a second mixed solution, and then the second mixed solution is heated to 60-70° C. and reacted for 1-3 hours to prepare an acryl diphosphoric acid flame retardant solution; S300: mixing the nano-silica particles containing double bond groups and an initiator in the acryloyl diphosphoric acid flame retardant solution to obtain a third mixed solution, and then heating the third mixed solution to 60-70° C. and reacting for 7-9 hours to obtain nano-silica modified particles; S400: sequentially adding the nano-silica modified particles and the alkaline pH regulator into the aqueous solution to obtain a fourth mixed solution, wherein the pH value of the fourth mixed solution is 4-6, then adding a metal salt to the fourth mixed solution and immersing it for 2-8 hours, and then filtering, washing and drying the fourth mixed solution to obtain the phosphorus-nitrogen-containing nano flame retardant.

2. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to claim 1, characterized in that: The weight ratio of the nano-silicon dioxide particles to the silane modifier is 1:(0.4-0.6).

3. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to claim 1, characterized in that: The weight ratio of the acrylamide, the phosphorous acid, the formaldehyde solution, the nano-silicon dioxide particles containing double bond groups and the initiator is 100:(230-265):(230-260):(60-70):(6-13).

4. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to claim 1, characterized in that: The weight ratio of the nano-silicon dioxide modified particles to the metal salt is 1:(0.1-0.2).

5. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to claim 1, characterized in that: The silane modifier is selected from one or more of vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, and 3-methacryloxypropyltrimethoxysilane.

6. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to claim 1, characterized in that: The initiator is selected from one or more of sodium persulfate, potassium persulfate and azobisisobutylcyanide.

7. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to claim 1, characterized in that: The metal salt is selected from Cu 2+ 、Zn 2+ , Ca 2+ Mg 2+ , Fe 3+ 、Al 3+ One or more of nitrates, acetates, and chlorides.

8. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to claim 1, characterized in that: The antioxidant is selected from one or more of antioxidant 1010 , antioxidant 168 , and antioxidant 1024 .

9. The low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to claim 1, characterized in that: The lubricant is selected from one or more of polyethylene wax and calcium stearate.

10. A method for preparing the low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament according to any one of claims 1 to 9, characterized in that: The following steps are involved: The ultra-molecular weight polyethylene, the high-density polyethylene, the phosphorus-nitrogen-containing nano flame retardant, the antioxidant, and the lubricant are mixed to obtain a raw material mixture; The raw material mixture is sequentially subjected to granulation and spinning treatments to obtain the low-smoke flame-retardant ultra-high molecular weight polyethylene monofilament.

Citation Information

Patent Citations

  • Method for preparing N-hydroxymethyl-3-(dimethoxyphosphoryl) propionamide

    CN102060873A

  • Halogen-free flame-retardant polyethylene composite material and preparation method thereof

    CN102964667A

  • Preparation method and application of cotton environment-friendly flame retardant

    CN104727145A

  • Preparation method of phosphorus-nitrogen synergistic flame-retardant polyvinyl alcohol fiber

    CN110777444A

  • Antibacterial flame-retardant ultra-high molecular weight polyethylene fiber and preparation method thereof

    CN114086272A