Preparation method of aerogel loaded glass fiber thermal insulation material

Through freeze-thaw pretreatment, vacuum impregnation and ultraviolet curing technology, airgel is composited with glass fiber, which solves the problem of insufficient thermal insulation performance of traditional glass fiber insulation materials and prepares efficient and pressure-resistant airgel-loaded glass. Fiber insulation material.

CN118727431APending Publication Date: 2024-10-01TIANJIN CHENGJIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410720886.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The thermal insulation performance of traditional fiberglass insulation materials is insufficient, and airgel materials are costly and immature in construction projects, making it difficult to be widely used in buildings.

Method used

The freeze-thaw pretreatment technology is used to treat the glass fiber mat, the aerogel and glass fiber are composited through the vacuum impregnation process, and the surface is encapsulated using ultraviolet curing technology to prepare the airgel-loaded glass fiber insulation material.

Benefits of technology

It improves the thermal insulation performance of glass fiber, enhances the compressive strength, reduces the phenomenon of airgel powder shedding, and forms a high-performance thermal insulation material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HSA0000298016670000011
    Figure HSA0000298016670000011
Patent Text Reader

Abstract

The invention provides a preparation method of an aerogel-loaded glass fiber insulation board, which comprises the following steps: firstly, treating a glass fiber mat by adopting a freeze thawing pretreatment technology to improve the specific surface area, the average pore diameter and the pore volume of the glass fiber mat, so that the loading capacity of aerogel can be improved; and then the aerogel and the glass fiber mat are compounded by adopting a vacuum impregnation technology, so that the loading capacity of the aerogel can be further improved, and the compressive strength of the aerogel loaded glass fiber thermal insulation material can be improved. And finally, the surface of the glass fiber mat is packaged by adopting an ultraviolet curing technology, so that the phenomenon that the aerogel powder falls off from the glass fibers is reduced. The prepared aerogel loaded glass fiber thermal insulation material has excellent thermal insulation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation process of a thermal insulation product, and in particular to a preparation method of an aerogel-loaded glass fiber thermal insulation material. Background Art

[0002] Traditional building insulation materials have certain limitations during use. Glass fiber, as a commonly used inorganic insulation material, has excellent heat resistance, corrosion resistance and chemical stability. However, compared with organic insulation materials, the thermal insulation performance of glass fiber needs to be further improved. Aerogel insulation materials have significant insulation advantages, but the cost is too high and it is not yet mature to use them alone in construction projects. By loading aerogel on glass fiber, it is expected that the overall thermal insulation performance of glass fiber will be improved, which will help develop new insulation materials. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing an aerogel-loaded glass fiber thermal insulation material, wherein the glass fiber felt is treated by a freeze-thaw pretreatment technology, the aerogel and the glass fiber felt are compounded by a vacuum impregnation technology, and the surface of the glass fiber felt is encapsulated by an ultraviolet light curing technology, so that the prepared aerogel-loaded glass fiber thermal insulation material has excellent thermal insulation performance.

[0004] The technical solution adopted by the present invention is: a method for preparing an aerogel-loaded glass fiber thermal insulation material, comprising the following steps:

[0005] STEP 1: Preparation of aerogel solution: Place a certain amount of aerogel powder into a container, first add anhydrous ethanol, then add distilled water, control the weight ratio of anhydrous ethanol and distilled water to be 1:1, control the mass percentage of aerogel to be 2-5%, first mechanically stir for 30 minutes, then ultrasonically vibrate for 10 minutes

[0006] STEP 2: Freeze-thaw pretreatment of glass fiber mat: put the glass fiber mat into a container filled with distilled water and let it stand for 30 minutes. Then put the glass fiber mat and the container into a refrigerator at -5°C and let it stand for 10 hours before taking it out. After it melts at room temperature, take out the glass fiber mat and dry it in a 100°C oven for 4 hours.

[0007] STEP3: Vacuum impregnation treatment: Place the glass fiber mat prepared in STEP2 into a container, and then pour the aerogel solution prepared in STEP1 into it until the upper surface of the glass fiber mat is completely immersed in the aerogel solution, and perform ultrasonic vibration for 5 minutes. Then move the entire container into a vacuum box, control the vacuum degree to -0.1MPa, let it stand for 30 minutes, then take out the glass fiber mat and dry it in an oven at 60℃;

[0008] STEP 4: Surface packaging of glass fiber felt: Prepare a UV curing agent, spray all surfaces of the glass fiber felt prepared in STEP 3, and then irradiate with a UV lamp for 60 seconds to obtain an aerogel-loaded glass fiber thermal insulation material.

[0009] The ultraviolet curing agent is composed of epoxy resin CYD-128, photoinitiator 831 and photodiluent NVP.

[0010] Compared with the prior art, the present invention has the following positive effects:

[0011] 1. Freeze-thaw pretreatment can increase the specific surface area, average pore diameter and pore volume of glass fiber mat, and increase the loading capacity of aerogel.

[0012] 2. The vacuum impregnation process can further increase the aerogel loading and improve the compressive strength of aerogel-loaded glass fiber insulation materials.

[0013] 3. The surface of the glass fiber mat is encapsulated by UV curing technology to form an overall seal and reduce the phenomenon of aerogel powder falling from the glass fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] The attached figure is a SEM image of the aerogel-loaded glass fiber thermal insulation material prepared in Example 1. DETAILED DESCRIPTION

[0015] The present invention will be further explained below in conjunction with specific implementation modes. It should be understood that the following specific implementation modes are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0016] Embodiment 1: A method for preparing an aerogel-loaded glass fiber thermal insulation material, comprising the following steps:

[0017] STEP 1: Preparation of aerogel solution: Place a certain amount of aerogel powder into a container. The thermal conductivity of aerogel is 0.018 W·m -1 ·K -1 , with a specific surface area of ​​600-800m 2 / g, bulk density is 20-100kg / m 3 First, add anhydrous ethanol, then add distilled water, control the weight ratio of anhydrous ethanol and distilled water to be 1:1, control the mass percentage of aerogel to be 5%, first mechanically stir for 30 minutes, then ultrasonically shake for 10 minutes:

[0018] STEP2: Freeze-thaw pretreatment of glass fiber mat: The density of glass fiber mat is 0.120g / cm 3 , fiber diameter is 10μm, compressive strength is 0.017MPa, thermal conductivity is 0.051W·m -1 ·K-1 . Put the glass fiber felt into a container filled with distilled water and let it stand for 30 minutes. Then put the glass fiber felt and the container into a refrigerator at -5℃ and let it stand for 10 hours before taking it out. After it melts at room temperature, take out the glass fiber felt and dry it in an oven at 100℃ for 4 hours.

[0019] STEP3: Vacuum impregnation treatment: Place the glass fiber mat prepared in STEP2 into a container, and then pour the aerogel solution prepared in STEP1 into it until the upper surface of the glass fiber mat is completely immersed in the aerogel solution, and perform ultrasonic vibration for 5 minutes. Then move the entire container into a vacuum box, control the vacuum degree to -0.1MPa, let it stand for 30 minutes, then take out the glass fiber mat and dry it in an oven at 60℃;

[0020] STEP 4: Surface packaging of glass fiber felt: Prepare a UV curing agent, spray all surfaces of the glass fiber felt prepared in STEP 3, and then irradiate with a UV lamp for 60 seconds to obtain an aerogel-loaded glass fiber thermal insulation material.

[0021] The ultraviolet curing agent is composed of epoxy resin CYD-128, photoinitiator 831 and photodiluent NVP.

[0022] The thermal conductivity and compressive strength of the aerogel-loaded glass fiber insulation material of Example 1 were tested. The thermal conductivity test method is as follows: The thermal conductivity of the material is measured using a portable TC3000E thermal conductivity meter from Xi'an Xiaxi Electronic Technology Co., Ltd. Two pieces of insulation material of the same specification are placed above and below the measuring sensor chip, and a weight is used to fit the sensor chip and start the measurement. The measurement range is 0.001-10.0 W·m -1 ·K -1 , with a resolution of 0.005 W·m -1 ·K -1 The compressive strength test steps are as follows: The compressive strength of the sample is tested by a universal electronic tensile machine (CMT6104 SANS, GER). Each sample is measured three times and the average value is taken. The loading speed is 10mm / min. The compressive strength is the stress value of the composite insulation material at 50% strain. The compressive load is perpendicular to the direction of the fiber alignment surface. The test results are shown in Table 1.

[0023] Embodiment 2: A method for preparing an aerogel-loaded glass fiber thermal insulation material, comprising the following steps:

[0024] STEP 1: Preparation of aerogel solution: put a certain amount of aerogel powder into a container, first add anhydrous ethanol, then add distilled water, control the weight ratio of anhydrous ethanol and distilled water to be 1:1, control the mass percentage of aerogel to be 2%, first mechanically stir for 30 minutes, then ultrasonically shake for 10 minutes;

[0025] STEP 2: Freeze-thaw pretreatment of glass fiber mat: put the glass fiber mat into a container filled with distilled water and let it stand for 30 minutes. Then put the glass fiber mat and the container into a refrigerator at -5°C and let it stand for 10 hours before taking it out. After it melts at room temperature, take out the glass fiber mat and dry it in a 100°C oven for 4 hours.

[0026] STEP3: Vacuum impregnation treatment: Place the glass fiber mat prepared in STEP2 into a container, and then pour the aerogel solution prepared in STEP1 into it until the upper surface of the glass fiber mat is completely immersed in the aerogel solution, and perform ultrasonic vibration for 5 minutes. Then move the entire container into a vacuum box, control the vacuum degree to -0.1MPa, let it stand for 30 minutes, then take out the glass fiber mat and dry it in an oven at 60℃;

[0027] STEP 4: Surface packaging of glass fiber felt: Prepare a UV curing agent, spray all surfaces of the glass fiber felt prepared in STEP 3, and then irradiate with a UV lamp for 60 seconds to obtain an aerogel-loaded glass fiber thermal insulation material.

[0028] The aerogel and glass fiber felt are the same as those in Example 1.

[0029] The ultraviolet curing agent is composed of epoxy resin CYD-128, photoinitiator 831 and photodiluent NVP.

[0030] The thermal conductivity and compressive strength of the aerogel-loaded glass fiber thermal insulation material of Example 2 were tested in the same manner as in Example 1. The test results are shown in Table 1.

[0031] Comparative Example: A method for preparing an aerogel-loaded glass fiber thermal insulation material, comprising the following steps:

[0032] STEP 1: Place a certain amount of aerogel powder into a container, first add anhydrous ethanol, then add distilled water, control the weight ratio of anhydrous ethanol to distilled water to be 1:1, control the mass percentage of aerogel to be 5%, first mechanically stir for 30 minutes, then ultrasonically vibrate for 10 minutes;

[0033] STEP 2: Place the glass fiber felt in a container, and then pour the aerogel solution prepared in STEP 1 into it until the upper surface of the glass fiber felt is completely immersed in the aerogel solution. Ultrasonic oscillate for 5 minutes, let it stand for 30 minutes, then take out the glass fiber felt and dry it in an oven at 60°C.

[0034] The thermal conductivity and compressive strength of the aerogel-loaded glass fiber thermal insulation material of the comparative example were tested in the same manner as in Example 1. The test results are shown in Table 1.

[0035] Table 1 Performance parameters of aerogel-loaded glass fiber thermal insulation materials prepared in the examples of the present invention and the comparative examples.

[0036] index <![CDATA[Thermal conductivity (W·m -1 ·K -1 )]]> Compressive strength(MPa) Example 1 0.020 2.183 Example 2 0.028 1.590 Comparative Example 0.048 0.869

[0037] By comparing the data in Table 1, it can be seen that compared with the comparative example, the thermal conductivity of Examples 1 and 2 is greatly reduced, the thermal insulation performance is excellent, the compressive strength is improved, and they can be directly applied to construction.

[0038] The present invention has been described in detail above through embodiments, but the contents described are only preferred implementation examples of the present invention and cannot be considered to limit the scope of implementation of the embodiments of the present invention. The protection scope of the embodiments of the present invention is defined by the claims. Anyone who utilizes the technical solutions described in the embodiments of the present invention, or who, inspired by the technical solutions of the embodiments of the present invention, designs similar technical solutions within the essence and protection scope of the embodiments of the present invention to achieve the above-mentioned technical effects, or who makes equal changes and improvements to the scope of application, shall still be included in the protection scope of the patent covered by the embodiments of the present invention.

Claims

1. A method for preparing an aerogel-loaded glass fiber thermal insulation material, characterized in that: The steps include: STEP 1: Preparation of aerogel solution: Place a certain mass of aerogel powder into a container, first add anhydrous ethanol, then add distilled water, control the weight ratio of anhydrous ethanol and distilled water to be 1:1, control the mass percentage of aerogel to be 2-5%, first mechanically stir for 30 minutes, then ultrasonically oscillate for 10 minutes. STEP 2: Freeze-thaw pretreatment of glass fiber felt: Place the glass fiber felt in a container filled with distilled water, let it stand for 30 minutes, then put the glass fiber felt and the container into a -5°C refrigerator, let it stand for 10 hours, then take it out. After it melts at room temperature, take out the glass fiber felt and dry it in a 100°C oven for 4 hours. STEP3: Vacuum impregnation treatment: Place the glass fiber mat prepared in STEP2 into a container, and then pour the aerogel solution prepared in STEP1 into it until the upper surface of the glass fiber mat is completely immersed in the aerogel solution, and ultrasonically vibrate for 5 minutes. Then move the entire container into a vacuum box, control the vacuum degree to -0.1MPa, stand for 30 minutes, then take out the glass fiber mat and dry it in an oven at 60℃. STEP 4: Surface packaging of glass fiber felt: Prepare a UV curing agent, spray all surfaces of the glass fiber felt prepared in STEP 3, and then irradiate with a UV lamp for 60 seconds to obtain an aerogel-loaded glass fiber insulation board.

2. The method for preparing an aerogel-loaded glass fiber thermal insulation material according to claim 1, characterized in that: The ultraviolet curing agent is composed of epoxy resin CYD-128, photoinitiator 831 and photodiluent NVP.