Modified fiber and preparation method thereof

The silica insulation layer is formed on the surface of carbon fiber through dopamine coating treatment and sol-gel method, which solves the problem of poor interfacial bonding force of carbon fiber composite materials, realizes the control of electromagnetic parameters and the environmental stability of the material, and improves the insulation and It has excellent wave absorption performance, safe and environmentally friendly process, and high output.

CN118727438APending Publication Date: 2024-10-01SHENZHEN INST OF ADVANCED ELECTRONICS MATERIALS +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410930222.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing carbon fiber composite materials have poor interfacial bonding force, cumbersome methods, high costs, and cannot achieve mass production, resulting in uneven coating layers and insufficient interfacial bonding force.

Method used

Dopamine coating treatment and sol-gel method are used to grow a silica insulation layer on the surface of carbon fibers. By adjusting the ratio and reaction conditions of dopamine and silicon source compounds, a uniform silica insulation layer is formed and the adhesion between the fiber and the coating layer is enhanced. connection strength and realize the control of electromagnetic parameters.

Benefits of technology

It improves the insulation of carbon fiber, solves the problem of impedance mismatch, enhances the environmental stability of the material, realizes the controllable electromagnetic wave absorption characteristics, and the process is safe and environmentally friendly, with high output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727438A_ABST
    Figure CN118727438A_ABST
Patent Text Reader

Abstract

The invention provides a modified fiber and a preparation method thereof. The preparation method specifically comprises the following steps: S1) obtaining a coarsened fiber; s2) coating the coarsened fibers with dopamine; and S3) coating a silicon dioxide insulating layer: mixing the dopamine-coated fiber with a silicon source compound capable of being hydrolyzed to form silicon dioxide according to a ratio, dispersing in a solvent, heating, adding a reaction initiator, stirring to react completely, standing, washing to be neutral, and drying. The fiber prepared by the method disclosed by the invention is good in insulativity, avoids the impedance mismatch problem, and has a huge application prospect in the electronic packaging fields of wave absorption, shielding and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electronic materials, and in particular to a modified fiber and a preparation method thereof. Background Art

[0002] Carbon fiber is widely used due to its high specific strength, high specific modulus, high chemical resistance, high heat resistance and low thermal expansion. The use of chemical and physical methods to modify the carbon fiber interface can give the carbon fiber new functions, thereby achieving the effect of regulating electromagnetic parameters and optimizing impedance matching. There are many modification methods disclosed in the prior art, and the main methods are as follows:

[0003] Using the hydrothermal method: First, pre-treat the carbon fiber and use the organic solvent acetone to remove the surface oil. Then immerse the carbon fiber in a mixed solution of metal salts for ultrasonic dispersion, then add it to a high-pressure reactor for high-temperature hydrothermal reaction, and finally wash and dry the prepared functionalized carbon fiber with a solvent. This type of technology has the disadvantages of complicated methods, high cost, low yield, and limited coating thickness.

[0004] Using chemical plating method: First, pre-treat the carbon fiber, including ultrasonic dispersion to remove surface grease and impurities, and then wash with deionized water. The pretreated carbon fiber is immersed in a plating solution containing a specific chemical composition, which usually contains metal salts, reducing agents and complexing agents. During the chemical plating process, the metal ions are reduced and deposited on the surface of the carbon fiber to form a uniform metal layer. In some cases, the carbon fiber after chemical plating will undergo a high-temperature sintering step to form an array modified coating of ceramic materials such as SiC to enhance its wave absorption performance. This type of technology has the disadvantages of uneven coating, poor interface bonding, cumbersome methods, high cost, and environmental pollution. Summary of the invention

[0005] The methods in the prior art generally have the problems of poor interface bonding strength of carbon fiber composite materials, cumbersome methods, high costs, and inability to mass produce. In order to solve the above problems, the present invention proposes a method for carbon fiber interface modification and electromagnetic parameter control.

[0006] One aspect of the present invention provides a method for preparing a modified fiber, the method comprising the following steps:

[0007] S1) roughening treatment: roughening the fiber to obtain roughened fiber;

[0008] S2) dopamine coating treatment: treating the roughened fibers with dopamine or a dopamine derivative to obtain dopamine-coated fibers;

[0009] S3) Coating with a silica insulating layer: The dopamine-coated fibers obtained in step S2) are uniformly mixed with a silicon source compound that can be hydrolyzed to form silica in a mass ratio of 10:1-10:200, and dispersed in a solvent. After heating, a reaction initiator is added, the reaction is stirred until complete, and the mixture is allowed to stand to form a silica insulating layer.

[0010] Furthermore, the fiber is carbon fiber, glass fiber, aramid fiber or metal fiber.

[0011] Furthermore, the roughening treatment method in step S1) includes treatment with an acid solution and treatment with plasma.

[0012] Furthermore, the acid solution in step S1) is selected from nitric acid, sulfuric acid or a mixture of nitric acid and sulfuric acid.

[0013] Furthermore, heating is performed during the roughening process in step S1), and the heating temperature is 60-80°C.

[0014] Furthermore, the dopamine derivative in step S2) is dopamine hydrochloride or 6-hydroxydopamine hydrochloride.

[0015] Furthermore, the method of treating dopamine or dopamine derivatives in step S2) includes dispersing the roughened fibers and dopamine or dopamine derivatives in a solvent, adding a corrosion inhibitor, adjusting the solvent to alkalinity, performing light irradiation reaction until complete, and washing and drying to obtain dopamine-coated fibers.

[0016] Furthermore, in step S2), the mass ratio of the roughened fibers to dopamine or dopamine derivatives is 10:8-50:8; for example, 20:8, 30:8, or 40:8.

[0017] Furthermore, the corrosion inhibitor in step S2) is tris(hydroxymethyl)aminomethane.

[0018] Furthermore, in step S2), the alkalinity is a pH value not less than 8, preferably a pH value of 8-9.

[0019] Furthermore, the silicon source compound capable of hydrolyzing to form silicon dioxide in step S3) is selected from tetraethyl silicate and sodium silicate.

[0020] Furthermore, in step S3), the mass ratio of the dopamine-coated fibers to the silicon source compound capable of polycondensing to form silicon dioxide is 10:5-10:100, for example, 10:10, 10:20, 10:30, 10:40, 10:50, 10:60, 10:70, 10:80, 10:90, 10:100.

[0021] Furthermore, in step S3), the mass ratio of the dopamine-coated fiber to the solvent is 10:80-10:100, for example, 10:85, 10:90, 10:95.

[0022] Furthermore, the solvent is water, alcohol or a mixed solvent of alcohol and water, and the alcohol is methanol, ethanol or propanol.

[0023] Furthermore, in step S3), the initiator is aqueous ammonia, preferably aqueous ammonia with a mass volume ratio of 10%.

[0024] Furthermore, in step S3), the reaction time after adding the initiator is 3 hours, and the standing time is at least 1 hour.

[0025] Furthermore, the thickness of the silicon dioxide insulating layer is 1-1000 nm, for example, 10 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, or 900 nm.

[0026] Another aspect of the present invention provides fibers with adjustable interface modification and electromagnetic parameters obtained by the above-mentioned preparation method.

[0027] Another aspect of the present invention provides a method for modifying the electromagnetic parameters of modified fibers, the method comprising the following steps:

[0028] S01) roughening treatment: roughening the fiber to obtain roughened fiber;

[0029] S02) Dopamine coating treatment: treating the roughened fibers with dopamine or a dopamine derivative to obtain dopamine-coated fibers;

[0030] S03) regulating the coated silicon dioxide insulating layer: the dopamine-coated fiber obtained in step S2) is uniformly mixed with a silicon source compound that can be hydrolyzed to form silicon dioxide in proportion, and dispersed in a solvent, and then heated and a reaction initiator is added, and the reaction is stirred until complete, and then washed to neutral after standing, and then dried;

[0031] The electromagnetic parameters of carbon fibers are regulated by adjusting the mass ratio of dopamine-coated carbon fibers to silicon source compounds that can be hydrolyzed to form silicon dioxide, and the range of regulation is that the mass ratio of dopamine-coated carbon fibers to silicon source compounds that can be hydrolyzed to form silicon dioxide is 10:1-10:200.

[0032] Furthermore, the roughening treatment method in step S01) includes treatment with an acid solution and treatment with plasma. Furthermore, the acid solution in step S01) is selected from nitric acid, sulfuric acid or a mixture of nitric acid and sulfuric acid.

[0033] Furthermore, heating is performed during the roughening process in step S01), and the heating temperature is 60-80°C.

[0034] Furthermore, the dopamine derivative in step S02) is dopamine hydrochloride or 6-hydroxydopamine hydrochloride.

[0035] Furthermore, the method of treating dopamine or dopamine derivatives in step S02) includes dispersing the roughened carbon fiber and dopamine or dopamine derivatives in a solvent, adding a corrosion inhibitor, adjusting the solvent to alkalinity, performing light irradiation reaction until complete, and washing and drying to obtain dopamine-coated carbon fiber.

[0036] Furthermore, in step S02), the mass ratio of the roughened carbon fiber to dopamine or dopamine derivative is 20:8-50:8; for example, 30:8 or 40:8.

[0037] Furthermore, the corrosion inhibitor in step S02) is tris(hydroxymethyl)aminomethane.

[0038] Furthermore, in step S02), the alkalinity is a pH value not less than 8, preferably a pH value of 8-9.

[0039] Furthermore, in step S02), the mass ratio of the roughened carbon fiber to dopamine or dopamine derivative is 10:8-50:8.

[0040] Furthermore, the silicon source compound capable of hydrolyzing to form silicon dioxide in step S03) is selected from tetraethyl silicate and sodium silicate.

[0041] Furthermore, in step S03), the mass ratio of the dopamine-coated carbon fiber to the silicon source compound capable of polycondensing to form silica is 10:5-10:100, for example, 10:10, 10:20, 10:30, 10:40, 10:50, 10:60, 10:70, 10:80, 10:90, 10:100.

[0042] Furthermore, in step S03), the mass ratio of dopamine-coated carbon fiber to solvent is 10:80-10:100, for example, 10:85, 10:90, 10:95.

[0043] Furthermore, the solvent is water, alcohol or a mixed solvent of alcohol and water, and the alcohol is methanol, ethanol or propanol.

[0044] Furthermore, in step S03), the initiator is aqueous ammonia, preferably aqueous ammonia with a mass volume ratio of 10%.

[0045] Furthermore, in step S03), the reaction time after adding the initiator is 3 hours, and the standing time is at least 1 hour.

[0046] Furthermore, the thickness of the silicon dioxide insulating layer is 1-1000 nm.

[0047] Beneficial Effects

[0048] The present invention solves the problem that the surface energy of the carbon fiber and the insulating coating layer does not match, resulting in insufficient adhesion between the coating layer and the substrate and interlayer detachment. Therefore, the carbon fiber prepared by the method of the present invention has good insulation, eliminates the impedance mismatch problem, and has great application prospects in the fields of electronic packaging such as wave absorption and shielding.

[0049] The present invention uses a sol-gel method to grow a silicon dioxide insulating layer of a certain thickness on the surface of the carbon fiber. The insulating layer not only serves as a regulating layer for electromagnetic parameters, but also enhances the environmental stability of the material. In addition, the thickness of the silicon dioxide layer is adjusted by adjusting the parameters, that is, by adjusting the different ratios of carbon fiber and silicon source to obtain coating layers of different thicknesses, the impedance matching and electromagnetic wave absorption characteristics can be adjusted by this method.

[0050] The method of the invention enhances the bonding strength between the carbon fiber and the coating layer by treating the carbon fiber surface with polydopamine (PDA), improves the interface between the matrix and the coating layer, has universal adaptability, does not require high-temperature treatment, is safe and environmentally friendly, and has high yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 Schematic diagram of the method of the present invention.

[0052] Figure 2 The results of scanning electron microscopy (SEM) of the carbon fiber interface before and after modification of the present invention are compared. (a) is pure fiber (CF), (b) is carbon fiber coated with silicon dioxide insulation layer (CF@SiO 2 ), (c) SiO2 insulating layer coated dopamine interface nitrocarbon fiber (N-CF@PDA@SiO 2 ).

[0053] Figure 3 The SiO 2 Insulating layer coated with dopamine interface nitrocarbon fiber (N-CF@PDA@SiO 2 ) X-ray energy spectrum (EDS). (a) is the surface scan distribution diagram of carbon element, (b) is the surface scan distribution diagram of oxygen element, and (c) is the surface scan distribution diagram of silicon element.

[0054] Figure 4The SEM images of the nitrified carbon fibers with silicon dioxide insulation and dopamine interface obtained at different carbon fiber and tetraethyl silicate mass ratios of the present invention. (a) is N-CF@PDA:TEOS=10:5, (b) is N-CF@PDA:TEOS=10:10, (c) is N-CF@PDA:TEOS=10:20, and (d) is N-CF@PDA:TEOS=10:40. TEOS is tetraethyl silicate, and N-CF@PDA is dopamine-coated carbon fibers.

[0055] Figure 5 The following are the focused ion beam cutting (FIB) images of the nitrified carbon fibers with silica insulation coated with dopamine interface, with different insulating coating layers obtained under different carbon fiber and tetraethyl silicate mass ratios of the present invention. Wherein (a) is N-CF@PDA:TEOS=10:5, (b) is N-CF@PDA:TEOS=10:10, and the thickness of the silica insulation coating is 19.84nm-37.49nm. (c) is N-CF@PDA:TEOS=10:20, and the thickness of the silica insulation coating is 79.74nm-94.97nm. (d) is N-CF@PDA:TEOS=10:40, and the thickness of the silica insulation coating is 583.8nm-941.1nm. Wherein TEOS is tetraethyl silicate, and N-CF@PDA is dopamine-coated carbon fiber.

[0056] Figure 6 The SiO obtained by reacting dopamine-coated carbon fibers with different mass ratios with a silicon source compound that can be hydrolyzed to form silicon dioxide in the preparation process of the present invention is 2 Insulating layer coated with dopamine interface nitrocarbon fiber (N-CF@PDA@SiO 2 ) of the dielectric constant. (a) The real part of the dielectric constant, (b) the imaginary part of the dielectric constant, and (c) the dielectric loss tangent value vary with frequency. Different colors in the figure represent the performance of different paraffin wax mixed sample thicknesses.

[0057] Figure 7 N-CF@PDA@SiO with different thicknesses under different mass ratios in the present invention 2 Graph of impedance variation with frequency.

[0058] Where (a) is N-CF@PDA:TEOS=10:5, (b) is N-CF@PDA 2 :TEOS=10:10, (c) is N-CF@PDA:TEOS=10:20, and (d) is N-CF@PDA:TEOS=10:40.

[0059] Figure 8N-CF@PDA@SiO with different thicknesses under different mass ratios in the present invention 2 The absorption performance diagram of the wave varies with frequency.

[0060] Among them, (a) is N-CF@PDA:TEOS=10:5, (b) is N-CF@PDA:TEOS=10:10, (c) is N-CF@PDA:TEOS=10:20, and (d) is N-CF@PDA:TEOS=10:40. DETAILED DESCRIPTION

[0061] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are described in detail below, but it should not be understood as limiting the applicable scope of the present invention.

[0062] Example 1 Preparation of silicon dioxide insulating layer coated dopamine interface nitrocarbon fiber

[0063] S1) Roughening carbon fiber treatment: placing the carbon fiber in a nitric acid solution, heating it to 60-80° C. and stirring it, washing it with deionized water until it is neutral, and drying it in an oven to obtain a nitrated carbon fiber with oxygen-containing functional groups introduced on the surface of the carbon fiber, i.e., roughening the carbon fiber;

[0064] S2) Dopamine coating treatment: ultrasonically disperse the roughened carbon fiber in deionized water, add dopamine hydrochloride, and the mass ratio of the roughened carbon fiber to dopamine hydrochloride is 20:8; then add tris(hydroxymethyl)aminomethane, add hydrochloric acid to adjust the pH to 8-9, stir under light until the solution turns brown-yellow, wash with deionized water until neutral, and dry to obtain dopamine-coated carbon fiber N-CF@PDA;

[0065] S3) growing a silicon dioxide insulating layer by a sol-gel method: taking the dopamine-coated carbon fiber obtained in step S2) and tetraethyl silicate, the mass ratio of the two is 10:5, and dispersing them in water for ultrasonic treatment for 10 minutes, the mass ratio of the dopamine-coated carbon fiber to deionized water is 1:9, then mechanically stirring and heating to 50°C, adding 10% ammonia water to react, and reacting for 3 hours under stirring; after the stirring is completed, standing for 1 hour, washing to neutrality, and drying; obtaining a silicon oxide insulating layer coated with dopamine interface nitrified carbon fiber N-CF@PDA@SiO 2 .

[0066] Example 2 Preparation of dopamine interface nitrified carbon fibers coated with silicon dioxide insulating layers of different thicknesses

[0067] The same method as in Example 1 is used, except that in step S3), the dopamine-coated carbon fiber and tetraethyl silicate are mixed in a mass ratio of 10:10, 10:20 or 10:40.

[0068] By controlling the ratio of carbon fiber to polymer compound, different thickness of insulating coated carbon fiber can be obtained, thereby realizing electromagnetic parameter regulation. When the mass ratio of dopamine-coated carbon fiber to tetraethyl silicate is 10:20, the thickness of the insulating coating layer is about 200nm.

[0069] Example 3: Carbon fiber coated with silicon dioxide insulation layer

[0070] Sol-gel method for growing a silica insulating layer: carbon fiber and tetraethyl silicate are mixed in a mass ratio of 10:5, dispersed in anhydrous ethanol solvent and ultrasonically treated for 10 minutes, with a mass ratio of carbon fiber to anhydrous ethanol of 1:9, followed by mechanical stirring and heating to 50°C, adding 10% ammonia water to react, and reacting for 3 hours under stirring; after the stirring is completed, let stand for 1 hour, wash to neutrality, and dry; to obtain a silica insulating layer coated carbon fiber.

[0071] Example 4 Dopamine coating treatment comparison

[0072] The same method as in Example 1 is used, except that the mass ratio of the roughened carbon fiber to dopamine hydrochloride in step S2) is 10:8, 30:8, and 50:8. From the test results, the mass ratio of the roughened carbon fiber to dopamine hydrochloride has little effect on step 3), and uniform SiO can be generated. 2 layer.

[0073] Effect example

[0074] Scanning electron microscopy (SEM)

[0075] Compared with the untreated carbon fiber, the N-CF@PDA@SiO2 treated carbon fiber was prepared by using the silicon dioxide insulating layer coated with dopamine interface nitrified carbon fiber N-CF@PDA@SiO2. 2 ), and Example 3 (Silica insulation layer coated carbon fiber CF@SiO 2 )Scanning electron microscopy results of carbon fiber obtained by treatment.

[0076] The test results are shown in Figure 2 , Figure 2 Shown are typical scanned images of each group of carbon fibers. Figure 2 It can be seen that the surface of the untreated carbon fiber is smooth, and the silicon dioxide insulation layer covers the carbon fiber CF@SiO 2 The surface of the carbon fiber has a thin coating layer, but the coating layer has partially fallen off, exposing the internal carbon fiber surface, and the silicon dioxide insulating layer covers the dopamine interface nitrified carbon fiber N-CF@PDA@SiO 2 The surface is tightly covered without falling off.

[0077] In Example 1-2, different ratios of carbon fiber and tetraethyl silicate were used to obtain SEM images of insulating coated carbon fibers of different thicknesses. The experimental results are shown in FIG. Figure 4-5 As shown. Figure 4 As shown in Figure 2, as the ratio of carbon fiber to tetraethyl silicate increases, the thickness of the insulation layer increases. Figure 5 As shown, as the ratio of carbon fiber to tetraethyl silicate increases, the thickness of the insulating layer increases from 0 to 1000 nm.

[0078] The dielectric constant, dielectric loss angle, impedance change, and wave absorption performance are tested by mixing the insulating coated dopamine interface fiber powder with paraffin wax at a powder: paraffin mass ratio of 0.04:0.06 to make a coaxial ring. Figure 7-8 1-5 and different colored segments are the performance of different paraffin mixed sample thicknesses, i.e., 1-5 mm thickness.

[0079] The silicon dioxide coated carbon fiber composite materials with different coating thicknesses in Example 1-2 were tested by a vector grid analyzer, including testing their wave absorption performance at 1-18 GHz electromagnetic parameters and testing their resistivity using a high-frequency analyzer. The results showed that in the range of 1 to 18 GHz, the reflection loss increased from -8.31 dB to -42.65 dB, and the resistivity increased from 10 -3 Ω·cm increased to 10 13 Ω·cm.

[0080] Energy dispersive spectrometry (EDS)

[0081] The surface scanning distribution analysis of different elements was carried out by X-ray, and the experimental results are as follows Figure 3 As shown, Figure 3 SiO 2 The elemental surface scanning analysis diagram of carbon, oxygen and silicon of the nitrated carbon fiber with the insulating layer coated with dopamine interface. It can be seen that the cross section of the carbon fiber is carbon element, while the outer surface is oxygen element and silicon element, indicating that the surface of the carbon fiber is coated with silicon dioxide through the treatment of the present invention.

[0082] Dielectric Constant Diagram

[0083] In Example 1-2, the dielectric constants of the insulating coated carbon fibers with different thicknesses were obtained by using different ratios of carbon fiber and tetraethyl silicate. The experimental results are shown in FIG. Figure 6 As shown in the figure, as the ratio of carbon fiber to tetraethyl silicate increases, the thickness of the insulating layer increases, the resistance of the composite material increases, the real part of the dielectric constant ε' and the imaginary part of the dielectric constant ε" decrease, and the dielectric loss tangent also decreases. This shows that the electromagnetic parameters can be regulated by adjusting the thickness of the insulating layer.

[0084] impedance

[0085] The different ratios of carbon fiber and tetraethyl silicate in Example 1-2 were analyzed to obtain the impedance changes of insulating coated carbon fibers of different thicknesses. Figure 7The impedance changes of the above carbon fibers were analyzed, among which Z in represents the external input impedance, Z 0 It represents the impedance of free space. As the ratio of carbon fiber to tetraethyl silicate increases, the impedance value gradually increases, indicating that as the thickness of the insulating layer increases, more electromagnetic waves are absorbed into the material.

[0086] Wave absorbing performance

[0087] The different ratios of carbon fiber and tetraethyl silicate in Example 1-2 result in different absorption properties of insulating coated carbon fibers of different thicknesses. Figure 8 The absorption in the range of 1 to 18 GHz is analyzed. As the thickness of the insulating coating increases, the reflection loss increases from -8.31 dB to -42.65 dB.

Claims

1. A method for preparing a modified fiber, characterized in that: The preparation method comprises the following steps: S1) roughening treatment: roughening the fiber to obtain roughened fiber; S2) dopamine coating treatment: treating the roughened fibers with dopamine or a dopamine derivative to obtain dopamine-coated fibers; S3) coating with a silicon dioxide insulating layer: the dopamine-coated fiber obtained in step S2) is uniformly mixed with a silicon source compound that can be hydrolyzed to form silicon dioxide in a mass ratio of 10:1-10:200, and dispersed in a solvent, and a reaction initiator is added after heating, and the reaction is stirred until complete, and the mixture is allowed to stand to form a silicon dioxide insulating layer; Preferably, the silicon source compound capable of hydrolyzing to form silicon dioxide in step S3) is selected from tetraethyl silicate and sodium silicate.

2. The preparation method according to claim 1, characterized in that: The fiber is carbon fiber, glass fiber, aramid fiber or metal fiber.

3. The preparation method according to claim 1, characterized in that: The roughening treatment method in step S1) includes treatment with an acid solution, treatment with a plasma, corona treatment or sandblasting; Preferably, the acid solution is selected from nitric acid, sulfuric acid or a mixture of nitric acid and sulfuric acid; Preferably, heating is performed during the roughening process in step S1), and the heating temperature is 60-80°C.

4. The preparation method according to claim 1, characterized in that: The dopamine derivative in step S2) is dopamine hydrochloride or 6-hydroxydopamine hydrochloride.

5. The preparation method according to claim 1, characterized in that: The method of treating with dopamine or a dopamine derivative in step S2) comprises dispersing the roughened fiber and dopamine or a dopamine derivative in a solvent, adding a corrosion inhibitor, adjusting the solvent to alkalinity, performing light irradiation until the reaction is complete, and washing and drying to obtain the dopamine-coated fiber; Preferably, the mass ratio of the roughened fibers to dopamine or dopamine derivatives is 10:8-50:

8.

6. The preparation method according to claim 1, characterized in that: The corrosion inhibitor in step S2) is tris(hydroxymethyl)aminomethane.

7. The preparation method according to claim 1, characterized in that: In step S3), the mass ratio of the dopamine-coated fiber to the silicon source compound capable of polycondensing to form silicon dioxide is 10:5-10:

100.

8. The preparation method according to claim 1, characterized in that: In step S3), the initiator is aqueous ammonia, preferably aqueous ammonia with a mass volume ratio of 10%.

9. A fiber with interface modification and adjustable electromagnetic parameters obtained by the preparation method according to any one of claims 1 to 8.

10. A method for modifying the electromagnetic parameters of modified fibers, characterized in that: The control method comprises the following steps: S1) roughening treatment: roughening the fiber to obtain roughened fiber; S2) dopamine coating treatment: treating the roughened fibers with dopamine or a dopamine derivative to obtain dopamine-coated fibers; S3) regulating the coated silicon dioxide insulating layer: the dopamine-coated fiber obtained in step S2) is uniformly mixed with a silicon source compound that can be hydrolyzed to form silicon dioxide in proportion, and dispersed in a solvent, and then heated and a reaction initiator is added, and the reaction is stirred until complete, and then washed to neutral after standing, and then dried; The electromagnetic parameters of the fibers are regulated by adjusting the mass ratio of the dopamine-coated fibers to the silicon source compound that can be hydrolyzed to form silica. The range of regulation is within the range of 10:1-10:200.

Citation Information

Cited By

  • High-strength environment-friendly vulcanized fiber paper and preparation method thereof

    CN118958030A

  • Preparation method of heat insulation carbon fiber heat preservation material

    CN120193410A

  • Preparation method of thermal insulation carbon fiber thermal insulation material