Device and method for testing abrasion resistance of concrete

By designing a concrete anti-abrasion test device including a sand box, a filter box and a water tank, the nozzle and siphon principles are used to form a sand flow, which solves the problem of waterway blockage, achieves an accurate assessment of the anti-abrasion performance of concrete, and improves hydraulic construction wear resistance and service life.

CN118730790APending Publication Date: 2024-10-01JIANYANHUACE (HANGZHOU) SCI & TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411083016.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing concrete erosion and abrasion test equipment has problems such as waterway blockage and inaccurate test results, making it difficult to simulate the concrete erosion and abrasion resistance under actual working conditions.

Method used

A test device including a sand box, a filter box and a water tank was designed. The nozzle and siphon principles were used to form sand flow to prevent waterway blockage. By comparing multiple test blocks and comparison test blocks, the anti-abrasion index was calculated to ensure that the test accuracy and consistency.

Benefits of technology

It realizes the concrete wear-resistant performance test in simulated actual hydraulic environment, reduces energy consumption, ensures the smooth progress of the test, and evaluates the wear-resistant characteristics of the material through the anti-abrasion index, which improves the service life of the hydraulic construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118730790A_ABST
    Figure CN118730790A_ABST
Patent Text Reader

Abstract

The invention relates to a concrete abrasion resistance test device and method. The device comprises a test carrier, and a sand box, a filter box and a water tank which are at least partially communicated are arranged in the test carrier; the test block fixing table is positioned obliquely above the sand box, a plurality of test blocks and reference test blocks are fixed on the test block fixing table through a clamp, and the test blocks and the reference test blocks are positioned in water or sand water; the nozzle is movably connected above the test block fixing table; the top of the nozzle is connected with a water pipe, and the side facing the sand box is connected with a sand suction pipe entering the sand box; the sand grains are sucked into the nozzle under the driving of high-speed water flow to form sand water; wherein an overflow hole is formed in the top of the sand box and communicated with the filter box, a water outlet of the filter box is communicated with the water tank, and a water pump communicated with the water pipe is arranged in the water tank. According to the method, the abrasion volume of the ultra-high performance concrete test block and the abrasion volume of the contrast glass test block are compared, and the abrasion resistance index is calculated, so that the abrasion resistance of a material in a simulated environment is quantitatively evaluated, and the accuracy and consistency of data are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete detection, and more particularly to a concrete anti-abrasion test device and method. Background Art

[0002] Ultra-high performance concrete (UHPC) is a new type of cement-based composite material with excellent mechanical properties and durability. However, hydraulic structures are exposed to high-speed water flow for a long time and are subjected to repeated erosion and abrasion by high-speed water flow with sand and stones. This causes severe scouring and abrasion of the concrete, greatly shortening the service life of the building.

[0003] In the prior art, the sample block is usually placed horizontally on one side of the box, and the mixed sand and water are sent to the top of the sample block for scouring and grinding through a high-pressure pump. The water channel of the above structure is relatively long. In order to ensure that the sand particles in the water do not settle, continuous stirring is required by a stirring mechanism. In addition, during the sand and water transportation process, pipeline block blockage incidents are prone to occur, making it difficult to ensure the continuous progress of the test and achieve the preset test effect. The concrete sample block is only in a water and sand environment, and the scouring and grinding mode is somewhat different from the actual working conditions, making it difficult to feedback the scouring and grinding resistance of concrete in actual engineering.

[0004] Therefore, how to provide a concrete abrasion resistance test device and method is a problem that technical personnel in this field need to solve urgently. Summary of the invention

[0005] The present invention aims to solve one of the above-mentioned technical problems in the prior art at least to a certain extent.

[0006] To this end, one object of the present invention is to provide a concrete anti-abrasion test device, and another object is to provide a concrete anti-abrasion test method to solve the problems in the prior art.

[0007] The technical solution of the present invention is a concrete abrasion resistance test device, comprising:

[0008] A test carrier, wherein the test carrier has a sand box, a filter box and a water tank at least partially connected thereto;

[0009] A test block fixing table, the test block fixing table is located obliquely above the sand box, and multiple test blocks and comparison test blocks are fixed thereon by clamps, and the multiple test blocks and comparison test blocks are in water or sand water;

[0010] A nozzle, the nozzle is movably connected to the top of the test block fixing table; the top of the nozzle is connected to a water pipe, and the side of the nozzle facing the sand box is connected to a sand suction pipe entering the sand box; sand particles are sucked into the nozzle driven by high-speed water flow to form sand water;

[0011] The top of the sand box is provided with an overflow hole, the overflow hole is connected to the filter box, the water outlet of the filter box is connected to the water tank, and the water tank is provided with a water pump connected to the water pipe.

[0012] According to the technical solution of the present invention, the angle between the nozzle and the grinding surfaces of the multiple test blocks and the comparison test blocks is 45°±0.5°, and the distance between the center of the nozzle and the grinding surfaces of the multiple test blocks and the comparison test blocks is 62mm±2mm.

[0013] According to the technical solution of the present invention, the top of the test block fixing platform is an inclined surface, on which a plurality of test block fixtures are arranged.

[0014] According to the technical solution of the present invention, a slider is provided on the side of the nozzle, and a guide rail is provided on the top of the sand box along the fixed length direction of the multiple test blocks and the comparison test blocks. The slider cooperates with the guide rail, and the slider moves along the guide rail through the driving assembly to cover the punching and grinding range to all the multiple test blocks and the comparison test blocks.

[0015] According to the technical solution of the present invention, the water pipe is provided with a pressure display portion.

[0016] According to the technical solution of the present invention, the water tank has a water shortage protection part.

[0017] According to the technical solution of the present invention, the first sedimentation chamber, the second sedimentation chamber and the third sedimentation chamber are arranged in sequence in the filter box from close to the sand box to close to the water tank side. The first sedimentation chamber is provided with a grid, and its top has overflow hole two, and the overflow hole two is connected to the second sedimentation chamber. The second sedimentation chamber has overflow hole three, and the overflow hole three is connected to the third sedimentation chamber. The water outlet is located at the upper part of the third sedimentation chamber.

[0018] The present invention provides a test method based on the above concrete abrasion resistance test device, comprising the following steps:

[0019] S1. Take out the abrasion resistance test block from the standard curing room, wipe off the surface moisture, mark it, and use a camera to photograph the abrasion surface for measuring the abrasion wear volume modeling. The number of photographs should be no less than 2 times;

[0020] S2. Place the abrasion test block on the test block fixing table and adjust the nozzle position so that the abrasion surface of the test block forms an angle of 45°±0.5° with the nozzle, and the distance between the abrasion test block surface and the nozzle center is 62mm±2mm;

[0021] S3. Pour water into the sand box to submerge the test block until the water level reaches the specified height, start the water pump, and grind for 75min±1min before stopping;

[0022] S4. Remove the test block from the test block fixing table, wipe off the surface moisture, and use a camera to photograph the abrasion surface for measuring the abrasion wear volume modeling. The number of photographs should be no less than 2 times;

[0023] S5. After modeling the grinding surface data taken by the camera before and after grinding, the volume of the wear is calculated by photogrammetry software. Each test block should have two sets of grinding surface data modeling. When the difference in the volume of wear calculated by the photogrammetry software is less than 5%, the average of the two results is used as the representative value of the wear of a single test block; otherwise, the test result is invalid and the test should be repeated.

[0024] According to the test method of the present invention, each group of test blocks uses three ultra-high performance concrete test blocks and two comparison glass test blocks.

[0025] According to the test method of the present invention, the calculation and processing of the test results in S5 should meet the following requirements:

[0026] S51. The wear volume of ultra-high performance concrete should be calculated as follows:

[0027]

[0028] Where: V U is the average wear volume of ultra-high performance concrete (mm 3 ), accurate to 1mm 3 ;

[0029] V Ui is the wear volume of a single UHP concrete specimen (mm 3 ), accurate to 1mm 3 ;

[0030] If the difference between the maximum or minimum value and the middle value exceeds 10% of the middle value, the middle value should be taken as the measured value; if both the maximum and minimum values ​​exceed 10% of the middle value, the sample should be re-prepared for testing;

[0031] S52. The wear volume of the comparison glass should be calculated as follows:

[0032]

[0033] Where: V G ——Comparison of the average volume of glass wear (mm 3 ), accurate to 1mm 3 ;

[0034] V Gi ——Compare the wear volume of a single glass test piece (mm 3 ), accurate to 1mm 3 ;

[0035] When the difference between the maximum and minimum values ​​and the average value exceeds 20% of the average value, the sample should be re-prepared for testing;

[0036] S53. The impact and abrasion resistance index should be calculated as follows:

[0037]

[0038] Where: I——anti-impact and abrasion index, accurate to 0.1;

[0039] V U ——Average wear volume of ultra-high performance concrete (mm 3 ), accurate to 1mm 3 ;

[0040] V G ——Comparison of the average volume of glass wear (mm 3 ), accurate to 1mm 3 .

[0041] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0042] The test device provided by the present invention can place multiple test blocks and comparison test blocks at the same time during the test, and the grinding results can be compared after the test; the water level in the sand box is higher than the overflow hole and then enters the filter box for filtration, and then enters the water tank after filtration. The water pump pumps water of a certain pressure into the nozzle according to the test needs, and the nozzle uses the siphon principle to suck in the sand particles and mix them to form sand and water for grinding onto the grinding surface of the test block to prevent water channel block blockage. At the same time, no power stirring is required in the sand box, so energy consumption is reduced, sand and water are recycled, and water resources are saved, thereby ensuring the smooth progress of the test.

[0043] Evaluate the wear resistance of concrete materials under high-speed sand-containing water flow. The test device simulates the abrasion conditions in actual hydraulic environments and provides a reliable testing platform for the wear resistance of concrete materials by precisely controlling the abrasion conditions (such as abrasion angle, distance, time, etc.).

[0044] The test method of the present invention calculates the impact wear index by comparing the wear volume of the ultra-high performance concrete test block and the comparative glass test block, thereby quantitatively evaluating the wear resistance of the material under the simulated environment, ensuring the accuracy and consistency of the data, and taking re-testing measures for abnormal data.

[0045] The test device and method of the present invention provide an effective evaluation means for the durability and wear resistance of concrete materials, and are helpful to improve the service life and reliability of hydraulic structures in harsh environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0047] Figure 1 A longitudinal cross-sectional view of a concrete anti-abrasion test device provided by the present invention;

[0048] Figure 2 A top view of a concrete abrasion resistance testing device provided by the present invention;

[0049] Figure 3 The schematic diagram of the structure inside the filter box is shown. DETAILED DESCRIPTION

[0050] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0051] The existing laboratory simulation of concrete abrasion test conditions is different from the actual working conditions, which will affect the accurate feedback of the test results. For example, the test specimen is usually placed horizontally on one side of the box, and the mixed sand and water are sent to the top of the test specimen for abrasion by a high-pressure pump. However, this method requires the mixing mechanism to repeatedly stir the sand and water, and the sand and water delivery pipeline is long, which is easy to cause waterway blockage. It is impossible to truly simulate the abrasion of concrete under actual working conditions, and it is difficult to truly reflect the anti-abrasion performance of concrete in actual engineering.

[0052] In view of this, the present invention provides a concrete anti-abrasion test device, see the attached Figure 1-3 ,include:

[0053] The test carrier is used to create a water flow environment containing sand particles and circulate water, and can be a box or a cylinder. The test carrier has a sand box 1, a filter box 7 and a water tank 8 that are at least partially connected.

[0054] The test block fixing table 9 ensures that the test block is stable and can be effectively tested. The test block fixing table 9 is located obliquely above the sand box 1, and multiple test blocks and a comparison test block 2 are fixed thereon by a clamp. The multiple test blocks and the comparison test block 2 are in water or sand water, and a certain test angle is maintained;

[0055] The nozzle 4 is used to uniformly grind the test block. The nozzle 4 is movably connected to the top of the test block fixing platform 9. The top of the nozzle 4 is connected to a water pipe 6, and the side of the nozzle 4 facing the sand box 1 is connected to a sand suction pipe 3 that enters the sand box 1. The sand particles are sucked into the nozzle 4 driven by the high-speed water flow to form sand water.

[0056] The top of the sand box 1 has an overflow hole, the overflow hole is connected to the filter box 7, the water outlet of the filter box 7 is connected to the water tank 8, and the water tank 8 has a water pump 81 connected to the water pipe 6.

[0057] The above technical solution utilizes the structure of the test carrier to maintain water circulation supply. The sand and water are sent into the water tank after filtering, which prevents the blockage of the pipeline and ensures the smooth progress of the test. The siphon principle is used to suck in sand particles for mixing. No power mechanism is required, which reduces energy consumption.

[0058] The angle and distance between the nozzle and the multiple test blocks and the comparison test block 2 will directly affect the impact effect of the water-sand flow. In the present invention, it is preferred that the nozzle 4 and the grinding surface of the multiple test blocks and the comparison test block 2 are 45°±0.5°, and the distance between the center of the nozzle 4 and the grinding surface of the multiple test blocks and the comparison test block 2 is 62mm±2mm, and the grinding effect is better.

[0059] In this solution, the top of the test block fixing platform 9 is an inclined surface, on which a plurality of test block clamps are arranged, wherein the clamps adopt existing designs and can stably fix the test blocks on the test block fixing platform 9 .

[0060] In the description of the present invention, it is necessary to understand that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0061] The side of the nozzle 4 is provided with a slider, and the top of the sand box 1 is provided with a guide rail along the fixed length direction of the multiple test blocks and the comparison test block 2. The slider cooperates with the guide rail, and the slider moves along the guide rail through the driving assembly to cover the punching and grinding range to all the multiple test blocks and the comparison test block 2. The driving assembly can be a motor and a nut screw structure, the motor rotates to drive the screw, the slider is equivalent to the nut, and drives the nozzle to move along the guide rail, and the slide rail ensures that the nozzle can move smoothly to ensure the consistency and repeatability of the test.

[0062] The water pipe 6 is provided with a pressure display portion, which may be a pressure gauge.

[0063] The pressure water provided by the water pump to the nozzle in the present invention is adjustable and can be freely adjusted according to the strength of the concrete test block and the flushing effect, and the range is 0-1 MPa.

[0064] Advantageously, the nozzle where the nozzle is located can be adjusted up and down according to the test needs when the test block is arranged. The lifting structure can be provided with a fixed plate on the slider, and the fixed plate has different mounting holes. According to the test requirements, the nozzle is installed in the corresponding mounting hole to change the position of the nozzle in the height direction.

[0065] Advantageously, the water tank 8 has a water shortage protection part. When the water in the water tank reaches the lower water level limit, the water pump automatically stops working, thereby protecting the motor; the water shortage protection part can be a water level sensor.

[0066] In an embodiment of the present invention, a first sedimentation chamber 71, a second sedimentation chamber 72 and a third sedimentation chamber 73 are sequentially arranged in the filter box 7 from close to the sand box 1 to close to the water tank 8. The first sedimentation chamber 71 has a grid to filter the turbid sand water overflowing. The top of the first sedimentation chamber 71 has an overflow hole 2, which is connected to the second sedimentation chamber 72 to subject the filtered water to secondary sedimentation. At this time, the water flow is relatively stable, and fine sand and mud can be precipitated compared to the first time. The second sedimentation chamber 72 has an overflow hole 3, which is connected to the third sedimentation chamber 73. The water outlet is located at the upper part of the third sedimentation chamber 73. Finally, the water that has been precipitated three times will re-enter the water tank, forming a water cycle and avoiding water waste.

[0067] The sand box, filter box and water tank are all equipped with discharge ports at the bottom, which is conducive to the discharge of sediment at the bottom.

[0068] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0069] A test method is provided for the durability test of ultra-high performance concrete, which is mainly used for the anti-abrasion performance test of concrete. The constituent materials of ultra-high performance concrete have particles of different sizes in the best proportion to form the most compact stacking, and the strength is generally above C120Mpa. It can be called the most durable engineering material with excellent wear resistance and explosion resistance. Therefore, in order to better apply ultra-high performance concrete to bridges, tunnels, high-rise buildings, etc., the present invention provides a test method for its wear resistance based on the above-mentioned concrete anti-abrasion test device, including the following steps:

[0070] S1. Take out the abrasion resistance test block from the standard curing room, wipe off the surface moisture, mark it, and use a camera to photograph the abrasion surface for measuring the abrasion wear volume modeling. The number of photographs should be no less than 2 times;

[0071] S2. Place the abrasion test block on the test block fixing table and adjust the nozzle position so that the abrasion surface of the test block forms an angle of 45°±0.5° with the nozzle, and the distance between the abrasion test block surface and the nozzle center is 62mm±2mm;

[0072] S3. Pour water into the sand box to submerge the test block until the water level reaches the specified height, start the water pump, and grind for 75min±1min before stopping;

[0073] S4. Remove the test block from the test block fixing table, wipe off the surface moisture, and use a camera to photograph the abrasion surface for measuring the abrasion wear volume modeling. The number of photographs should be no less than 2 times;

[0074] S5. After modeling the grinding surface data taken by the camera before and after grinding, the volume of the wear is calculated by photogrammetry software. Each test block should have two sets of grinding surface data modeling. When the difference in the volume of wear calculated by the photogrammetry software is less than 5%, the average of the two results is used as the representative value of the wear of a single test block; otherwise, the test result is invalid and the test should be repeated.

[0075] In the present invention, unless otherwise clearly required or limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0076] Each group of test blocks uses three ultra-high performance concrete test blocks and two comparison glass test blocks. The first and last of the five test blocks are comparison glass test blocks, and the three in the middle are a group of concrete test blocks; among them, the glass test blocks are made of glass with a Knoop hardness of 500. Concrete impact and abrasion test blocks should be cast into 100mm×100mm×35mm test blocks in a 100mm cubic test mold, or they can be cast into 100mm cubes at one time. After the concrete hardens, it is cut into 100mm×100mm×35mm test blocks with a diamond saw.

[0077] Glass specimens and concrete specimens were subjected to abrasion tests in the same environment, and the abrasion resistance index was used to determine the abrasion resistance of ultra-high performance concrete.

[0078] In the above test, the water pump should be able to provide a jet of 0.3MPa (0-1MPa) pressure water to the nozzle outlet; the diameter of the nozzle center nozzle is 20mm±2mm; the test block fixing platform and guide rail: fix the test block grinding surface at a position of 45°±0.5° and 62mm±2mm away from the nozzle; the sand used for grinding should be quartz sand, the SiO2 content of quartz sand should be not less than 97%, the Mohs hardness is 7, and the content of 1mm~4mm particles is not less than 95%. When the wear volume of the glass test block is reduced to (60±5)% of the wear volume of the new sand when it is first used, the quartz sand should be replaced; the sand box should be set at a position that can ensure that 4mm quartz sand particles can be sucked into the jet water-sand mixture to participate in grinding.

[0079] The standard curing of ultra-high performance concrete test blocks should be carried out in water under standard curing conditions for 28 days. Ultra-high performance concrete cured by conventional steam should be placed in water under standard conditions for curing after steam curing and continue to be cured for 28 days. Ultra-high performance concrete cured by high temperature heat curing to improve performance should be placed in water under standard conditions for curing and continue to be cured for 7 days after the high temperature heat curing is completed.

[0080] The calculation and processing of test results in S5 shall meet the following requirements:

[0081] S51. The wear volume of ultra-high performance concrete should be calculated as follows:

[0082]

[0083] Where: V U is the average wear volume of ultra-high performance concrete (mm 3 ), accurate to 1mm 3 ;

[0084] V Ui is the wear volume of a single UHP concrete specimen (mm 3 ), accurate to 1mm 3 ;

[0085] If the difference between the maximum or minimum value and the middle value exceeds 10% of the middle value, the middle value should be taken as the measured value; if both the maximum and minimum values ​​exceed 10% of the middle value, the sample should be re-prepared for testing;

[0086] S52. The wear volume of the comparison glass should be calculated as follows:

[0087]

[0088] Where: V G ——Comparison of the average volume of glass wear (mm 3 ), accurate to 1mm 3 ;

[0089] V Gi ——Compare the wear volume of a single glass test piece (mm 3 ), accurate to 1mm 3 ;

[0090] When the difference between the maximum and minimum values ​​and the average value exceeds 20% of the average value, the sample should be re-prepared for testing;

[0091] S53. The impact and abrasion resistance index should be calculated as follows:

[0092]

[0093] Where: I——anti-impact and abrasion index, accurate to 0.1;

[0094] V U ——Average wear volume of ultra-high performance concrete (mm 3 ), accurate to 1mm 3 ;

[0095] V G ——Comparison of the average volume of glass wear (mm 3 ), accurate to 1mm 3 .

[0096] The present invention calculates the impact and wear resistance index by comparing the wear volume of the ultra-high performance concrete test block with the comparison glass test block, thereby quantitatively evaluating the wear resistance of the material under the simulated environment. The accuracy and consistency of the data are ensured, and the abnormal data is retested. This test device and method provides an effective evaluation method for the durability and wear resistance of concrete materials, which helps to improve the service life and reliability of hydraulic structures in harsh environments.

[0097] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0098] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A concrete abrasion resistance test device, It is characterized in that include: A test carrier, wherein the test carrier has a sand box (1), a filter box (7) and a water tank (8) which are at least partially connected; A test block fixing table (9), the test block fixing table (9) is located obliquely above the sand box (1), and a plurality of test blocks and a comparison test block (2) are fixed thereon by means of a clamp, and the plurality of test blocks and the comparison test block (2) are in water or sand water; A nozzle (4), the nozzle (4) being movably connected to the top of the test block fixing platform (9); the top of the nozzle (4) is connected to a water pipe (6), and the side of the nozzle (4) facing the sand box (1) is connected to a sand suction pipe (3) for entering the interior of the sand box (1); sand particles are sucked into the nozzle (4) driven by a high-speed water flow to form sand water; The top of the sand box (1) is provided with an overflow hole, the overflow hole is connected to the filter box (7), the water outlet of the filter box (7) is connected to the water tank (8), and the water tank (8) is provided with a water pump (81) connected to the water pipe (6).

2. A concrete abrasion resistance testing device according to claim 1, It is characterized in that The nozzle (4) is at an angle of 45°±0.5° to the grinding surfaces of the multiple test blocks and the comparison test block (2), and the distance between the center of the nozzle (4) and the grinding surfaces of the multiple test blocks and the comparison test block (2) is 62 mm±2 mm.

3. A concrete abrasion resistance testing device according to claim 1, It is characterized in that The top of the test block fixing platform (9) is an inclined surface, on which a plurality of test block fixtures are arranged.

4. A concrete abrasion resistance testing device according to claim 1, It is characterized in that The side of the nozzle (4) is provided with a slide block, and the top of the sand box (1) is provided with a guide rail along the fixed length direction of the multiple test blocks and the comparison test blocks (2). The slide block cooperates with the guide rail, and the slide block moves along the guide rail through the driving component to cover the punching and grinding range to all the multiple test blocks and the comparison test blocks (2).

5. A concrete abrasion resistance testing device according to claim 1, It is characterized in that The water pipe (6) is provided with a pressure display portion.

6. A concrete abrasion resistance testing device according to claim 1, It is characterized in that The water tank (8) has a water shortage protection portion.

7. A concrete abrasion resistance testing device according to any one of claims 1 to 6, It is characterized in that The filter box (7) is provided with a first sedimentation chamber (71), a second sedimentation chamber (72) and a third sedimentation chamber (73) in sequence from the side close to the sand box (1) to the side close to the water tank (8). The first sedimentation chamber (71) has a grille, and a second overflow hole is provided on the top thereof, and the second overflow hole is connected to the second sedimentation chamber (72). The second sedimentation chamber (72) has a third overflow hole, and the third overflow hole is connected to the third sedimentation chamber (73). The water outlet is located at the upper part of the third sedimentation chamber (73).

8. A test method based on the concrete abrasion resistance test device according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1. Take out the abrasion resistance test block from the standard curing room, wipe off the surface moisture, mark it, and use a camera to photograph the abrasion surface for measuring the abrasion wear volume modeling. The number of photographs should be no less than 2 times; S2. Place the abrasion test block on the test block fixing table and adjust the nozzle position so that the abrasion surface of the test block forms an angle of 45°±0.5° with the nozzle, and the distance between the abrasion test block surface and the nozzle center is 62mm±2mm; S3. Pour water into the sand box to submerge the test block until the water level reaches the specified height, start the water pump, and grind for 75min±1min before stopping; S4. Remove the test block from the test block fixing table, wipe off the surface moisture, and use a camera to photograph the abrasion surface for measuring the abrasion wear volume modeling. The number of photographs should be no less than 2 times; S5. After modeling the grinding surface data taken by the camera before and after grinding, the volume of the wear loss is calculated by photogrammetry software. Each test block should have two sets of grinding surface data modeling. When the difference in the volume of wear loss calculated by the photogrammetry software is less than 5%, the average of the two results is used as the representative value of the wear loss of a single test block; otherwise, the test result is invalid and the test should be repeated.

9. The test method according to claim 8, It is characterized in that Each group of test blocks used three ultra-high performance concrete test blocks and two comparison glass test blocks.

10. The test method according to claim 9, It is characterized in that The calculation and processing of test results in S5 shall meet the following requirements: S51. The wear volume of ultra-high performance concrete should be calculated as follows: Where: V U is the average wear volume of ultra-high performance concrete (mm 3 ), accurate to 1mm 3 ; V Ui is the wear volume of a single UHP concrete specimen (mm 3 ), accurate to 1mm 3 ; If the difference between the maximum or minimum value and the middle value exceeds 10% of the middle value, the middle value should be taken as the measured value; if both the maximum and minimum values ​​exceed 10% of the middle value, the sample should be re-prepared for testing; S52. The wear volume of the comparison glass should be calculated as follows: Where: V G ——Comparison of the average volume of glass wear (mm 3 ), accurate to 1mm 3 ; V Gi ——Compare the wear volume of a single glass test piece (mm 3 ), accurate to 1mm 3 ; When the difference between the maximum and minimum values ​​and the average value exceeds 20% of the average value, the sample should be re-prepared for testing; S53. The impact and abrasion resistance index should be calculated as follows: Where: I——anti-impact and abrasion index, accurate to 0.1; V U ——Average wear volume of ultra-high performance concrete (mm 3 ), accurate to 1mm 3 ; V G ——Comparison of the average volume of glass wear (mm 3 ), accurate to 1mm 3 .