Polarizing plate

By using a combination of a light diffusion layer, a polyester resin film, and a (meth)acrylic resin film in a polarizing plate, the problem in the prior art that the polarizing plate has a poor rainbow pattern suppression effect in the oblique direction is solved, and a better effect is achieved. Good brightness and visibility.

CN118732115APending Publication Date: 2024-10-01SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410349743.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing polarizing plate has insufficient rainbow pattern suppression effect when viewed in an oblique direction, and the brightness is insufficient, which affects the visibility of the liquid crystal display device.

Method used

Using a layer structure composed of a light diffusion layer, a polyester resin film, an adhesive layer, a polarizing plate and a (meth)acrylic resin film, by adjusting the phase difference value and arrangement of the polyester resin film, a combination of ( The protective film of the meth)acrylic resin film forms a polarizing plate to improve the brightness in the oblique direction and suppress rainbow streaks.

Benefits of technology

It effectively suppresses the occurrence of rainbow patterns on the polarizing plate in the oblique direction, increases the brightness, and improves the visibility of the liquid crystal display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118732115A_ABST
    Figure CN118732115A_ABST
Patent Text Reader

Abstract

The invention provides a polarizing plate, an adhesive-layer-equipped polarizing plate comprising the polarizing plate, and a liquid crystal display device comprising the adhesive-layer-equipped polarizing plate, wherein rainbow patterns observed from the inclined direction of the polarizing plate are suppressed, and the polarizing plate has good brightness in the inclined direction. Provided is a polarizing plate including a light diffusion layer, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and a (meth) acrylic resin film in this order, in which a phase difference value Re defined by Re = (nx-ny) * d of the polyester resin film is 6000 nm or more as measured in a first arrangement, and a phase difference value Re2 measured in a second arrangement is 5000 nm or more as measured in a second arrangement, the phase difference value Re3 measured in the third arrangement is 6000 nm or more, and the phase difference value Re4 measured in the fourth arrangement is 7000 nm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing plate, and also to a polarizing plate with an adhesive layer and a liquid crystal device including the polarizing plate. Background Art

[0002] In recent years, it has been required to improve the visibility of liquid crystal display devices. In order to improve the visibility of liquid crystal display devices, it is also required that the polarizing plate, which is one of the components constituting the liquid crystal display, suppress unevenness and increase brightness so as to improve visibility from an oblique direction.

[0003] In order to suppress the unevenness of the polarizing plate and improve the brightness from the oblique direction, the types and combinations of polarizer protective films in the polarizing plate have been studied. For example, Patent Document 1 states that, when a 38 μm biaxially stretched polyethylene terephthalate film is used as one polarizer protective film, a film containing an acrylic compound whose composition of a cellulose ester resin is adjusted is used as another polarizer protective film, so that the unevenness of the polarization degree of the polarizing plate can be suppressed.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2011-123402 Summary of the invention

[0007] Problems to be solved by the invention

[0008] The polarizing plate described in Patent Document 1 is not sufficiently capable of suppressing rainbow fringes observed in an oblique direction of the polarizing plate and providing insufficient visibility in an oblique direction.

[0009] An object of the present invention is to provide a polarizing plate that suppresses rainbow fringes observed from an inclined direction of the polarizing plate and has good brightness in the inclined direction, a polarizing plate with an adhesive layer including the polarizing plate, and a liquid crystal display device including the polarizing plate with an adhesive layer.

[0010] Means for solving problems

[0011] The present invention includes the following inventions.

[0012] [1] A polarizing plate comprising, in this order, a light diffusion layer, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and a (meth)acrylic resin film,

[0013] The polyester resin film satisfies the following [i] to [iv] with respect to the retardation value Re defined by the formula (1).

[0014] Re=(n x -ny )×d (1)

[0015] [Where n x Represents the refractive index in the slow axis direction of the film surface, n y represents the refractive index in the fast axis direction of the film surface, and d represents the thickness of the film.]

[0016] [i] The phase difference value Re1 measured in the first arrangement in which the polyester resin film is arranged so that the angle between the surface of the polyester resin film and the measurement direction is 90° is 6000 nm or more.

[0017] [ii] The phase difference value Re2 measured in the second configuration is greater than 5000 nm, wherein the polyester resin film in the first configuration is configured in such a way that the angle between the surface of the polyester resin film and the measuring direction becomes 60 degrees by rotating the polyester resin film about its fast axis by 30 degrees.

[0018] [iii] The phase difference value Re3 measured in the third configuration is greater than 6000nm, wherein the polyester resin film in the first configuration is configured in such a way that the angle between the surface of the polyester resin film and the measuring direction becomes 60° by rotating the polyester resin film by 30° around an axis forming an angle of 45° with respect to its fast axis within the surface of the polyester resin film.

[0019] [iv] The phase difference value Re4 measured in the 4th configuration is greater than 7000nm, and in the 4th configuration, the polyester resin film in the above-mentioned 1st configuration is arranged in a manner such that the angle between the surface of the polyester resin film and the measuring direction becomes 60° by rotating the polyester resin film about its slow axis by 30°.

[0020] [2] The polarizing plate according to [1], wherein the polyester resin film has a thickness of 60 μm or more.

[0021] [3] The polarizing plate according to [1] or [2], wherein the ratio of the retardation value Re1 of the polyester resin film to the retardation value Rth in the thickness direction defined by formula (2) is 0.5 or more.

[0022] Rth=〔(n x +n y ) / 2-n z 〕 ×d (2)

[0023] [Where n x Represents the refractive index in the slow axis direction of the film surface, n y Represents the refractive index in the fast axis direction of the film surface, n zrepresents the refractive index in the thickness direction of the film, and d represents the thickness of the film.]

[0024] [4] The polarizing plate according to any one of [1] to [3], wherein the total haze of the light diffusion layer is 20% or more.

[0025] [5] A polarizing plate with an adhesive layer, comprising the polarizing plate according to any one of [1] to [4] and an adhesive layer.

[0026] The pressure-sensitive adhesive layer is laminated on the surface of the (meth)acrylic resin film opposite to the polarizer.

[0027] [6] A liquid crystal display device comprising the polarizing plate with a pressure-sensitive adhesive layer as described in [5].

[0028] Effects of the Invention

[0029] According to the present invention, a polarizing plate that suppresses rainbow fringes observed in an inclined direction of the polarizing plate and has good brightness in the inclined direction, a polarizing plate with an adhesive layer including the polarizing plate, and a liquid crystal display device including the polarizing plate with an adhesive layer can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic cross-sectional view schematically showing an example of the polarizing plate of the present invention.

[0031] Figure 2 It is a schematic three-dimensional diagram for explaining the phase difference value Re1 and its measurement method.

[0032] Figure 3 It is a schematic three-dimensional diagram for explaining the phase difference value Re2 and its measurement method.

[0033] Figure 4 It is a schematic three-dimensional diagram for explaining the phase difference value Re3 and its measurement method.

[0034] Figure 5 It is a schematic stereoscopic diagram for explaining the phase difference value Re4 and its measurement method.

[0035] Figure 6 This is a schematic cross-sectional view schematically showing an example of the pressure-sensitive adhesive layer-attached polarizing plate of the present invention.

[0036] Description of Reference Numerals

[0037] 1: polarizing plate, 2: polarizing plate with adhesive layer, 5: light diffusion layer, 10: polyester resin film, 15: first adhesive layer, 20: (meth) acrylic resin film, 25: second adhesive layer, 30: polarizer, 40: adhesive layer, 100: polyester resin film (first configuration), 110: polyester resin film (second configuration), 120: polyester resin film (third configuration), 130: polyester resin film (fourth configuration), 201: light source, 202: observer, 210: measurement direction, 300, 310, 320: central axis, 400: fast axis of the polyester resin film in the first configuration, 500: slow axis of the polyester resin film in the first configuration. DETAILED DESCRIPTION

[0038] The polarizing plate of the present invention includes a light diffusion layer, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and a (meth)acrylic resin film in this order.

[0039] Examples of the layer constitution of the polarizing plate of the present invention are shown in Figure 1 . Figure 1 The polarizing plate 1 shown includes a light diffusion layer 5 , a polyester resin film 10 , a first adhesive layer 15 , a polarizer 30 , a second adhesive layer 25 , and a (meth)acrylic resin film 20 in this order.

[0040] like Figure 1 As shown, in the polarizing plate of the present invention, the polyester resin film 10 is preferably in direct contact with the first adhesive layer 15. In addition, the (meth) acrylic resin film 20 is preferably in direct contact with the second adhesive layer 25. The polarizer 30 is preferably in direct contact with the first adhesive layer 15. The polarizer 30 is preferably in direct contact with the second adhesive layer 25. Although not shown in the figure, an adhesive layer or a pressure-sensitive adhesive layer may be arranged between the light diffusion layer 5 and the polyester resin film 10.

[0041] <Light diffusion layer>

[0042] The light diffusion layer is a layer having a light-transmitting resin as a base material, and may be a layer in which light-transmitting fine particles are dispersed in the light-transmitting resin, and is disclosed in, for example, Japanese Patent Application Laid-Open Nos. 2012-048223 and 2012-212120.

[0043] As the light-transmitting resin, there is no particular limitation as long as it has light transmittance, and for example, ionizing radiation-curing resins such as ultraviolet-curing resins and electron beam-curing resins, cured products of thermosetting resins, thermoplastic resins, and cured products of metal alkoxides can be used. When an ionizing radiation-curing resin, a thermosetting resin, or a metal alkoxide is used, the resin is cured by irradiation or heating with ionizing radiation to form a light-transmitting resin. Among them, ionizing radiation-curing resins are suitable from the perspective of having high hardness and being able to impart high scratch resistance when used as a polarizer protective film provided on the surface of a liquid crystal display device.

[0044] As ionizing radiation curing resins, there can be mentioned multifunctional acrylates such as acrylic acid or methacrylic acid esters of polyols; multifunctional urethane acrylates synthesized from diisocyanates, polyols and hydroxy esters of acrylic acid or methacrylic acid, etc. In addition to these, polyether resins, polyester resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiol polyene resins, etc. having acrylate functional groups can also be used.

[0045] Examples of the thermosetting resin include thermosetting urethane resins including acrylic polyol and isocyanate prepolymers, phenol resins, urea melamine resins, epoxy resins, unsaturated polyester resins, and silicone resins.

[0046] Examples of the thermoplastic resin include cellulose derivatives such as acetyl cellulose, nitro cellulose, acetobutyl cellulose, ethyl cellulose, and methyl cellulose; vinyl resins such as vinyl acetate and its copolymers, vinyl chloride and its copolymers, and vinylidene chloride and its copolymers; acetal resins such as polyvinyl formal and polyvinyl butyral; acrylic resins such as acrylic resins and their copolymers, and methacrylic resins and their copolymers; polystyrene resins; polyamide resins; polyester resins; polycarbonate resins, and the like.

[0047] As the metal alkoxide, a silicon oxide matrix made of silicon alkoxide materials can be used, for example, tetramethoxysilane, tetraethoxysilane, etc., which can be made into an inorganic or organic-inorganic composite matrix (translucent resin) by hydrolysis and dehydration condensation.

[0048] In addition, as translucent particles, organic particles or inorganic particles with translucency can be used. For example, organic particles containing acrylic resins, melamine resins, polyethylene, polystyrene, silicone resins, acrylic acid-styrene copolymers, etc., inorganic particles containing calcium carbonate, silicon dioxide, aluminum oxide, barium carbonate, barium sulfate, titanium oxide, glass, etc., etc. can be cited. In addition, balls of organic polymers and hollow glass beads can also be used. Translucent particles can be composed of one kind of particles, or can contain more than two kinds of particles. The shape of the translucent particles can be any one of spherical, flat, plate-like, needle-like, amorphous, etc., preferably spherical or roughly spherical.

[0049] The filling rate of the light-transmitting fine particles is preferably 40% or more, more preferably 50% or more.

[0050] The weight average particle size of the light-transmitting particles is preferably 0.5 μm or more and 15 μm or less, more preferably 3 μm or more and 9 μm or less. If the weight average particle size of the light-transmitting particles is less than 0.5 μm, it is sometimes impossible to fully scatter visible light in the wavelength region of 380 nm to 800 nm. In addition, when the weight average particle size exceeds 15 μm, the thickness of the entire light diffusion layer becomes thicker, which sometimes hinders the thinning of polarizing plates and displays. It should be noted that the weight average particle size of the light-transmitting particles is measured using a Coulter Multisizer (manufactured by BECKMAN COULTER) using the Coulter principle (pore resistance method).

[0051] The refractive index of the light-transmitting microparticles is preferably greater than that of the light-transmitting resin, and the difference is preferably in the range of 0.04 to 0.15. By setting the refractive index difference between the light-transmitting microparticles and the light-transmitting resin to be within the above range, appropriate internal scattering caused by the refractive index difference between the light-transmitting microparticles and the light-transmitting resin can be generated, and a light diffusion function can be imparted.

[0052] In addition, as light diffusion layer, it is possible to form a layer by a light diffusive adhesive composition (hereinafter, also referred to as light diffusive adhesive composition) having spherical particles in acrylic resin. At this time, the refractive index difference between acrylic resin and spherical particles is a scope exceeding 0.01 and less than 0.09. The refractive index difference is preferably more than 0.01 and is less than 0.07, and more preferably more than 0.01 and is less than 0.04. If the refractive index difference between the two is less than 0.01, the resulting adhesive layer will not show the desired optical performance, and as a result, becomes an adhesive close to a transparent adhesive. On the other hand, if the refractive index difference between acrylic resin and spherical particles becomes too large, the light diffusive performance is strong, so the brightness when the liquid crystal display device is observed from the front is reduced.

[0053] Spherical particles that satisfy the above conditions may be used alone or in combination of two or more. When two or more spherical particles are mixed, spherical particles having different refractive indices or particles having different particle sizes may be mixed.

[0054] The acrylic resin contained in the adhesive composition can be composed of an acrylic resin with a weight average molecular weight in the range of 1,000 to 2,000,000. In addition, the spherical particles are selected to have an average particle diameter in the range of 0.5 to 15 μm, and are mixed in a ratio of 20 to 80 parts by mass relative to 100 parts by mass of the acrylic resin. By setting such a specific combination, good adhesive performance and optical performance are exhibited.

[0055] The light diffusing adhesive composition may contain a crosslinking agent in order to form a good crosslinked structure when forming an adhesive layer, and may contain an ionic compound in order to impart antistatic properties.

[0056] As the material of spherical particles, there is no particular restriction, and known organic particles and inorganic particles can be used. As organic particles, for example, resin particles such as (methyl) acrylic resins such as polyolefin resins, polymethacrylate resins, and polyacrylate resins including polystyrene, polyethylene, and polypropylene can be enumerated, and crosslinked polymers can also be crosslinked. In addition, copolymer resins formed by copolymerization of 2 or more monomers selected from ethylene, propylene, styrene, methyl methacrylate, benzoguanamine, formaldehyde, melamine, butadiene, etc. can also be used. As inorganic particles, for example, particles including silicon dioxide, silicone resin, titanium oxide, aluminum oxide, etc. can be enumerated. If the dispersibility of acrylic resin, the coating property of adhesive composition, the optical properties of the obtained adhesive layer, etc. are taken into consideration, the particles preferably include silicone resin or polymethyl methacrylate resin.

[0057] The blending amount of the spherical fine particles is 20 to 80 parts by mass relative to 100 parts by mass of the nonvolatile components of the acrylic resin. If the blending amount is less than 20 parts by mass relative to 100 parts by mass of the acrylic resin, the desired optical properties, particularly haze, will not be exhibited, while if the blending amount exceeds 80 parts by mass, the adhesive properties such as peeling due to the decrease in the adhesive force of the obtained adhesive layer will be reduced.

[0058] It should be noted that the light diffusion layer may further include an anti-reflection layer on the observation side when the polarizing plate is stacked on the liquid crystal display device. The anti-reflection layer is provided to reduce the reflectivity as much as possible. By forming the anti-reflection layer, reflected glare on the display screen can be prevented. As the anti-reflection layer, a low refractive index layer composed of a material having a lower refractive index than the light diffusion layer can be cited.

[0059] The light diffusion layer preferably has a total haze of 20% or more and an internal haze of 20% or more. "Total haze" refers to the value obtained by the following formula [1] based on the ratio of the total light transmittance (Tt) representing the total amount of light transmitted by irradiating the light diffusion layer with light and the diffuse light transmittance (Td) diffused by the light diffusion layer.

[0060] Total haze (%) = (Td / Tt) × 100〔1〕

[0061] The total light transmittance (Tt) is the sum of the parallel light transmittance (Tp) and the diffuse light transmittance (Td) transmitted coaxially with the incident light. The total light transmittance (Tt) and the diffuse light transmittance (Td) are values ​​measured in accordance with JIS K 7361.

[0062] In addition, the "internal haze" of the light diffusion layer refers to the haze other than the haze (surface haze) caused by the surface shape of the light diffusion layer in the total haze.

[0063] When the total haze and / or internal haze is less than 20%, the light scattering is insufficient and it is difficult to obtain sufficient wide viewing angle performance. In addition, when the total haze and / or internal haze exceeds 90%, the light scattering becomes stronger, and when a polarizing plate with a light diffusion layer is used in a liquid crystal display device, the front contrast is sometimes reduced. In addition, when the total haze and / or internal haze exceeds 90%, there is a tendency for the transparency of the light diffusion layer to be impaired. The total haze and / or internal haze are preferably 25% or more, more preferably 30% or more, and further preferably 35% or more, respectively. In addition, it is preferably 85% or less, more preferably 80% or less, and further preferably 75% or less.

[0064] When a layer with a light-transmitting resin as a substrate is used as a light diffusion layer, it can be bonded to a polyester resin film with the help of an adhesive layer. In addition, the adhesive layer that can be used for bonding can be an adhesive layer with light diffusion formed by a light diffusion adhesive composition, or an adhesive layer without light diffusion. It should be noted that when an adhesive layer with light diffusion is used, both the adhesive layer with light diffusion and the layer (film) with a light-transmitting resin as a substrate are regarded as light diffusion layers.

[0065] Alternatively, as the light diffusion layer, only a pressure-sensitive adhesive layer having light diffusion properties may be used.

[0066] <Polyester resin film>

[0067] The polyester resin film used in the present invention satisfies the following [i] to [iv] with respect to the retardation value Re defined by the formula (1).

[0068] Re=(n x -n y)×d (1)

[0069] [Where n x Represents the refractive index in the slow axis direction of the film surface, n y represents the refractive index in the fast axis direction of the film plane (the direction perpendicular to the slow axis direction of the film plane), and d represents the thickness of the film.]

[0070] [i] The phase difference value Re1 measured in the first arrangement in which the polyester resin film is arranged so that the angle between the surface of the polyester resin film and the measurement direction is 90° is 6000 nm or more.

[0071] [ii] The phase difference value Re2 measured in the second configuration is greater than 5000 nm, wherein the polyester resin film in the first configuration is configured in such a way that the angle between the surface of the polyester resin film and the measuring direction becomes 60 degrees by rotating the polyester resin film about its fast axis by 30 degrees.

[0072] [iii] The phase difference value Re3 measured in the third configuration is greater than 6000nm, wherein the polyester resin film in the first configuration is configured in such a way that the angle between the surface of the polyester resin film and the measuring direction becomes 60° by rotating the polyester resin film by 30° around an axis forming an angle of 45° with respect to its fast axis within the surface of the polyester resin film.

[0073] [iv] The phase difference value Re4 measured in the 4th configuration is greater than 7000nm, and in the 4th configuration, the polyester resin film in the above-mentioned 1st configuration is arranged in a manner such that the angle between the surface of the polyester resin film and the measuring direction becomes 60° by rotating the polyester resin film about its slow axis by 30°.

[0074] The slow axis direction in the film plane refers to the direction in which the refractive index becomes maximum in the plane. In addition, in this specification, the phase difference value Re is the phase difference value at a wavelength of 587nm.

[0075] Figure 2 2 is a schematic three-dimensional diagram for explaining the phase difference value Re1 and its measurement method. The phase difference value Re1 is the phase difference value measured in the first configuration in which the polyester resin film 100 is arranged so that the angle between the surface of the polyester resin film 100 and the measurement direction 210 is 90°. The measurement direction refers to the direction from the light source 201 of the phase difference measurement device toward the observer 202 for detecting and observing the light transmitted through the polyester resin film, and is the so-called optical path of the phase difference measurement device.

[0076] Figure 32 is a schematic three-dimensional diagram for explaining the phase difference value Re2 and its measuring method. The phase difference value Re2 is a phase difference value measured for the polyester resin film 100 in the first configuration which is tilted by rotating the polyester resin film 100 in the first configuration by 30° about its fast axis 400 as the central axis 300, that is, the polyester resin film 110 in the second configuration. The angle between the surface of the polyester resin film 110 in the second configuration and the measuring direction 210 is 60°.

[0077] Figure 4 2 is a schematic three-dimensional diagram for explaining the phase difference value Re3 and its measuring method. The phase difference value Re3 is a phase difference value measured for the polyester resin film 100 in the first configuration, which is tilted by rotating the polyester resin film 100 by 30° about an axis forming an angle of 45° with respect to its fast axis 400 in the polyester resin film plane as a central axis 310, that is, the polyester resin film 120 in the third configuration. The angle between the surface of the polyester resin film 120 in the third configuration and the measuring direction 210 is 60°.

[0078] Figure 5 2 is a schematic three-dimensional diagram for explaining the phase difference value Re4 and its measurement method. The phase difference value Re4 is a phase difference value measured for the polyester resin film 100 in the first configuration which is tilted by rotating 30° about its slow axis 500 as the central axis 320, that is, the polyester resin film 130 in the fourth configuration. The angle between the surface of the polyester resin film 130 in the fourth configuration and the measurement direction 210 is 60°.

[0079] The phase difference Re1 of the polyester resin film is preferably 7000nm or more, more preferably 7500nm or more, and further preferably 8000nm or more. In addition, the phase difference Re1 of the polyester resin film is usually 30000nm or less, preferably 20000nm or less, more preferably 15000nm or less, further preferably 10000nm or less, and further preferably 9000nm or less. When the upper limit of the phase difference Re1 exceeds 30000nm, in order to meet the phase difference, the thickness of the polyester resin film becomes quite large, and there is a tendency that the handleability as an optical film is greatly reduced. By making the phase difference Re1 of the polyester resin film 6000nm or more, it is easy to reduce the rainbow streaks (rainbow-like color spots) when observed from an oblique direction.

[0080] In addition, the phase difference Re2 of the polyester resin film is 5000nm or more. The phase difference Re2 is preferably 5500nm or more, more preferably 6000nm or more, further preferably 6500nm or more, and further preferably 7000nm or more. In addition, the phase difference Re2 is usually 30000nm or less, preferably 20000nm or less, more preferably 15000nm or less, further preferably 10000nm or less, and further preferably 9000nm or less. By making the phase difference Re2 of the polyester resin film 5000nm or more, it is easy to reduce the rainbow pattern when observed from an oblique direction.

[0081] The phase difference Re3 of the polyester resin film is 6000nm or more. The phase difference Re3 is preferably 7000nm or more, more preferably 7500nm or more, and further preferably 8000nm or more. In addition, the phase difference Re3 is usually 30000nm or less, preferably 20000nm or less, more preferably 15000nm or less, further preferably 10000nm or less, and further preferably 9000nm or less. By making the phase difference Re3 of the polyester resin film 6000nm or more, it is easy to reduce rainbow lines when observed from an oblique direction.

[0082] The phase difference value Re4 of the polyester resin film is 7000nm or more. The phase difference value Re4 is preferably 8000nm or more, more preferably 8500nm or more, and further preferably 9000nm or more. In addition, the phase difference value Re4 is usually 30000nm or less, preferably 20000nm or less, more preferably 15000nm or less, and further preferably 10000nm or less. By making the phase difference value Re4 of the polyester resin film 7000nm or more, it is easy to reduce rainbow lines when observed from an oblique direction.

[0083] Re1 to Re4 can be measured using a phase difference measuring device (manufactured by Oji Scientific Instruments Co., Ltd., KOBRA-HB-RESPC).

[0084] By using a polyester resin film in which Re1 to Re4 are respectively within the above ranges, rainbow fringes observed in the tilted direction of the polarizing plate can be suppressed.

[0085] The ratio of the phase difference value Re1 of the polyester resin film to the phase difference value Rth in the thickness direction (Re1 / Rth) is usually 0.4 or more, preferably 0.5 or more, more preferably 0.6 or more, further preferably 0.7 or more, and further preferably 0.9 or more. If the ratio Re1 / Rth is larger, there is a tendency that rainbow patterns caused by the observation angle are not easily generated. In a completely uniaxial (uniaxially symmetrical) film, the ratio Re1 / Rth is 2.0, so the ratio Re1 / Rth is preferably 2.0 or less, and the ratio Re1 / Rth is more preferably 1.5 or less.

[0086] The retardation value Rth in the thickness direction is represented by the following formula (2): The retardation value Rth in the thickness direction is the retardation value in the thickness direction at a wavelength of 587 nm.

[0087] Rth=〔(n x +n y ) / 2-n z 〕 ×d (2)

[0088] [Where n x Represents the refractive index in the slow axis direction of the film surface, n y Represents the refractive index in the fast axis direction of the film surface, n z It represents the refractive index in the film thickness direction (the direction perpendicular to the film surface), and d represents the thickness of the film.]

[0089] The angle between the fast axis or slow axis of the polyester resin film and the transmission axis of the polarizer is, for example, -20° to +20°, preferably -15° to +15°, more preferably -10° to +10°, further preferably -5° to +5°, further preferably -3° to +3°, further preferably -2° to +2°, and particularly preferably -1° to +1°. In a preferred embodiment, the fast axis or slow axis of the polyester resin film is substantially parallel to the transmission axis of the polarizer. Here, substantially parallel means that the transmission axis of the polarizer is parallel to the fast axis or slow axis of the polyester resin film to a degree that allows for the inevitable deviation when the polarizer is bonded to the polyester resin film.

[0090] The smaller the angle between the fast axis or slow axis of the polyester resin film and the transmission axis of the polarizer, the smaller the change in polarization state caused by linearly polarized light passing through the polyester resin film, and thus the generation of rainbow fringes tends to be suppressed.

[0091] In addition, in order to suppress the degradation of optical functional pigments such as iodine contained in the polarizer, the light transmittance of the polyester resin film at a wavelength of 380nm is preferably 40% or less. The light transmittance at 380nm is more preferably 35% or less, further preferably 30% or less, and particularly preferably 20% or less. If the light transmittance is 40% or less, the deterioration of the optical functional pigment caused by ultraviolet rays can be suppressed.

[0092] At least one selected from an antireflection layer and a low reflection prevention layer may be provided on at least one surface of the polyester resin film.

[0093] The surface reflectivity of the anti-reflection layer is preferably 5.7% or less. If the surface reflectivity of the anti-reflection layer exceeds 5.7%, there is a tendency for rainbow patterns to be easily observed. The surface reflectivity of the anti-reflection layer is more preferably 5.3% or less, further preferably 5.0% or less, and particularly preferably 4.5% or less. The lower limit of the surface reflectivity of the anti-reflection layer is not particularly limited, for example, 2.0%. The surface reflectivity can be measured by any method. For example, for a polyester resin film in which the side opposite to the anti-reflection layer is bonded to a black acrylic plate with an adhesive, a spectrophotometer (CM-2600d manufactured by Konica Minolta Japan Co., Ltd.) can be used to measure the reflectivity of light at a wavelength of 550nm from the surface on the anti-reflection layer side.

[0094] The anti-reflection layer can be a single layer or a multilayer. As the anti-reflection layer, there can be cited an anti-glare hard coating having a fine concavo-convex shape on the surface to prevent the reflected glare of external light, etc. The anti-glare hard coating has an anti-glare hard coating in which a filler is dispersed inside the hard coating to form a surface concavo-convex shape, and an anti-glare hard coating in which a surface concavo-convex shape is formed on the hard coating by an embossing method, etc. For example, when an anti-glare hard coating is formed using an ultraviolet curable resin, a resin composition formed by dispersing fillers in the ultraviolet curable resin can be applied to a polyester resin film and irradiated with ultraviolet rays, or an ultraviolet curable resin can be applied to a polyester resin film and irradiated with ultraviolet rays in a state where the coating film is closely attached to the concavo-convex surface of the mold.

[0095] As a material for forming the antiglare hard coat layer, ultraviolet curable resins, thermosetting resins, electron beam curable resins and the like can be used. From the viewpoint of productivity, hardness and the like, ultraviolet curable resins are preferably used.

[0096] The surface reflectivity of the low reflection prevention layer is preferably 4.0% or less. The surface reflectivity of the low reflection prevention layer is more preferably 3.0% or less, further preferably 2.0% or less, further preferably 1.5% or less, and particularly preferably 1.0% or less. The lower limit of the surface reflectivity of the low reflection prevention layer is not particularly limited, and may be, for example, 0.01%.

[0097] The low reflection preventing layer can be a single layer or a multilayer. When the low reflection preventing layer is a single layer, if the thickness of the low refractive index layer consisting of the material whose refractive index is lower than that of the polyester resin film is formed as 1 / 4 wavelength or an odd number of times of the wavelength of light, then the anti-reflection effect can be obtained. In addition, when the anti-reflection layer is a multilayer, if the low refractive index layer and the high refractive index layer are alternately set to more than 2 layers, and the thickness of each layer is appropriately controlled to be stacked, then the anti-reflection effect can be obtained. In addition, a hard coating layer can also be stacked between the low reflection preventing layer and the polyester resin film as required.

[0098] A known low reflection prevention layer can be used as the low reflection prevention layer. The low reflection prevention layer is preferably a layer formed by coating an organic thin film having a lower refractive index than the polyester resin film or a hard coat layer laminated on the polyester resin film.

[0099] The thickness of at least one selected from the antireflection layer and the low reflection prevention layer is usually 0.01 to 20 μm, preferably 0.03 to 1 μm, and more preferably 0.05 to 0.15 μm.

[0100] The surface reflectance of the polyester resin film is preferably 5.7% or less, more preferably 5.3% or less, further preferably 4.0% or less, further preferably 3.0% or less, particularly preferably 2.0% or less, and most preferably 1.5% or less. In addition, the surface reflectance of the polyester resin film is usually 0.01% or more.

[0101] When the surface reflectance of the polyester resin film is 5.7% or less, there is a tendency for rainbow of the polarizing plate to which the polyester resin film is applied to be suppressed more effectively.

[0102] It should be noted that, as described above, when at least one selected from an anti-reflection layer and a low-reflection layer is stacked, the surface reflectance of the entire at least one selected from the anti-reflection layer and the low-reflection layer can be 5.7% or less. It is speculated that by reducing the surface reflectance, the interface reflectance between the substrate film and the air can be reduced, and the rainbow pattern can be suppressed.

[0103] When at least one selected from the antireflection layer and the low reflection prevention layer is provided only on one side of the polyester resin film, at least one selected from the antireflection layer and the low reflection prevention layer is preferably provided on the side of the polyester resin film opposite to the polarizer.

[0104] When at least one selected from an anti-reflection layer and a low reflection prevention layer is provided, the polyester resin film preferably has an easy bonding layer on its surface. At this time, from the viewpoint of suppressing interference caused by reflected light, it is preferred that the refractive index of the easy bonding layer is adjusted to be near the geometric mean of the refractive index of the anti-reflection layer or the low reflection prevention layer and the refractive index of the polyester resin film. The refractive index of the easy bonding layer can be adjusted by a known method, for example, it can be easily adjusted by making the binder resin contain titanium, germanium, or other metal species.

[0105] In order to improve the adhesion with the polarizer, the polyester resin film preferably has an easy-adhesive layer with at least one of polyester resin, polyurethane resin or polyacrylic resin as the main component on at least one side thereof. Here, "main component" refers to a component of more than 50% by mass in the solid component constituting the easy-adhesive layer. The coating liquid used in the formation of the easy-adhesive layer is preferably an aqueous coating liquid comprising at least one of a water-soluble or water-dispersible copolyester resin, acrylic resin and polyurethane resin. As these coating liquids, for example, water-soluble or water-dispersible copolyester resin solution, acrylic resin solution, or polyurethane resin solution disclosed in Japanese Patent Gazette No. 3567927, Japanese Patent Gazette No. 3589232, Japanese Patent Gazette No. 3589233, Japanese Patent Gazette No. 3900191 and Japanese Patent Gazette No. 4150982 can be cited.

[0106] When a polyester resin is used as an easy-adhesive layer, a water-soluble or water-dispersible resin is preferably used from the viewpoint of compatibility with a polyvinyl alcohol resin. In order to make the polyester resin water-soluble or water-dispersible, it is preferred to copolymerize a compound containing a hydrophilic group such as a sulfonate group or a carboxylate group. Among them, from the viewpoint of keeping the acid value of the polyester resin low, controlling the reactivity with the cross-linking agent, and imparting hydrophilicity at the same time, a dicarboxylic acid component having a sulfonate group is suitable. As a dicarboxylic acid component having a sulfonate group, for example, sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfonaphthaleneisophthalic acid-2,7-dicarboxylic acid and 5-(4-sulfophenoxy)isophthalic acid or its alkali metal salt can be cited, among which 5-sulfoisophthalic acid is preferred. The dicarboxylic acid component having a sulfonate group is preferably 1 to 15 mol %, more preferably 1.5 to 12 mol %, and further preferably 2 to 10 mol % in the dicarboxylic acid component of the polyester resin. When the dicarboxylic acid component having a sulfonate group is greater than the above lower limit, it is suitable for water solubility or water dispersion of the polyester resin. In addition, when the dicarboxylic acid component having a sulfonate group is less than the above upper limit, it is suitable for adhesion to a polyester film substrate.

[0107] The adhesive layer can be obtained by applying the coating solution on one or both sides of a polyester resin film, drying at 100 to 150° C., and further stretching in the transverse direction. The final coating amount of the adhesive layer is preferably 0.05 to 0.20 g / m 2 If the coating amount is less than 0.05g / m 2 On the other hand, if the coating amount exceeds 0.20 g / m 2 When the adhesive layer is provided on both sides of the polyester resin film, the coating amount of the adhesive layer on both sides may be the same or different, and may be independently set within the above range.

[0108] In order to impart slipperiness, preferably particles are added to the easy bonding layer. The average particle size of the particles is preferably less than 2 μm. If the average particle size of the particles exceeds 2 μm, the particles easily fall off from the easy bonding layer. As the particles contained in the easy bonding layer, for example, inorganic particles such as titanium oxide, barium sulfate, calcium carbonate, calcium sulfate, silicon dioxide, aluminum oxide, talc, kaolin, clay, calcium phosphate, mica, hectorite, zirconium oxide, tungsten oxide, lithium fluoride and calcium fluoride, organic polymer particles such as styrene, acrylic acid, melamine, benzoguanamine and silicone can be cited. They can be added to the easy bonding layer alone, or two or more can be combined and added.

[0109] As a method for applying the coating liquid, a known method can be used, for example, reverse roll coating, gravure coating, kiss coating, roller brushing, spray coating, air knife coating, wire rod coating, tubular blade coating, etc., and these methods can be used alone or in combination.

[0110] The thickness of the polyester resin film is arbitrary, but is usually 15 to 200 μm, preferably 20 to 100 μm, more preferably 25 to 95 μm, further preferably 60 to 90 μm, and further preferably 75 to 85 μm.

[0111] If the thickness of the polyester resin film is less than 15 μm, the anisotropy of the mechanical properties of the film becomes significant, and cracks and breaks are easily generated, which tends to reduce practicality. On the other hand, if the thickness of the polyester resin film exceeds 200 μm, the thickness of the polarizing plate becomes too thick.

[0112] In addition, when at least one selected from the antireflection layer and the low reflection prevention layer is provided as described above, the total thickness including the antireflection layer and the low reflection prevention layer may be within the above range.

[0113] The polyester resin film used in the present invention can be produced according to a common method for producing a polyester film, and can be obtained by, for example, the method described in JP-A-2021-103319, JP-A-2021-99521, and the like.

[0114] The phase difference values ​​of Re1 to Re4 can be controlled to a specific range by appropriately setting the stretching ratio, stretching temperature, and film thickness. For example, a high phase difference value can be easily obtained by increasing the stretching ratio, lowering the stretching temperature, and increasing the thickness of the film. The phase difference values ​​of Re1 to Re4 can be set by selecting film making conditions and thickness from the above conditions in consideration of the physical properties required for processing.

[0115] The material forming the polyester resin film is not particularly limited, and polyethylene terephthalate and polyethylene naphthalate may be used, and other copolymer components may also be included. From the viewpoint of controlling the phase difference value of the polyester resin film, the material forming the polyester resin film is preferably polyethylene terephthalate resin.

[0116] <(Meth)acrylic resin film>

[0117] (Meth) acrylic resin film is excellent in mechanical properties, solvent resistance, scratch resistance, light resistance, transparency, cost, etc. By using (meth) acrylic resin film as a polarizer protective film, it is possible to improve the mechanical strength and thin the wall of the polarizing plate, the liquid crystal panel and the liquid crystal display device containing it. In addition, by using the above-mentioned polyester resin film as a polarizer protective film and using (meth) acrylic resin film as another polarizer protective film, rainbow patterns when observed from an oblique direction can be effectively suppressed. In addition, by using the above-mentioned polyester resin film as a polarizer protective film and using (meth) acrylic resin film as another polarizer protective film, light leakage in a high temperature environment can be effectively suppressed.

[0118] The (meth)acrylic resin constituting the (meth)acrylic resin film is a material obtained by mixing a (meth)acrylic resin and additives added as necessary, and then melt-kneading the mixture.

[0119] In the present specification, the term "(meth)acrylic resin" may be either an acrylic resin or a methacrylic resin, and "(meth)" in (meth)acrylate, (meth)acrylates, (meth)acryloyl, etc., has the same meaning.

[0120] The (meth)acrylic resin is preferably a polymer with (meth)acrylic acid ester as the main body. The (meth)acrylic resin can be a homopolymer of one (meth)acrylic acid ester, or a copolymer of (meth)acrylic acid ester and other (meth)acrylic acid esters. As (meth)acrylic acid esters, alkyl (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate can be mentioned, and the number of carbon atoms of the alkyl group is usually about 1 to 8. In addition, as polymerizable monomers that can be copolymerized with (meth)acrylic acid esters, for example, styrene monomers such as styrene and alkylstyrene can be mentioned; monofunctional monomers such as unsaturated nitriles such as acrylonitrile and methacrylonitrile, and alkenyl esters of unsaturated carboxylic acids such as allyl (meth)acrylate and methallyl (meth)acrylate; dienyl esters of dibasic acids such as diallyl maleate; polyfunctional monomers such as unsaturated carboxylic acid diesters of diols such as alkylene glycol di(meth)acrylate can be mentioned.

[0121] Moreover, the (meth)acrylic resin film may contain 2 or more types of (meth)acrylic resins.

[0122] When the (meth) acrylic resin film contains more than two (meth) acrylic resins, it is preferred that the syndiotacticity (rr) represented by the triad of at least one (meth) acrylic resin is 50% or more. From the viewpoint of improving the toughness of the film and the heat resistance of the film and the adhesion to the polarizer, the syndiotacticity (rr) represented by the triad is preferably 55% or more, more preferably 60% or more, further preferably 65% ​​or more, and further preferably 70% or more. The syndiotacticity (rr) represented by the triad is usually 90% or less, and can also be 85% or less.

[0123] The syndiotacticity (rr) of a triad is the ratio of two chains (diad) of a chain of three consecutive structural units (triad) that are both racemic (expressed as rr). The syndiotacticity (rr) (%) of a triad is calculated as follows: 1 The H-NMR spectrum was calculated by measuring the area (X) of the 0.6 to 0.95 ppm region and the area (Y) of the 0.6 to 1.35 ppm region when the internal standard TMS was set to 0 ppm based on the spectrum, and (X / Y)×100.

[0124] The (meth)acrylic resin having a syndiotacticity (rr) represented by a triad of 50% or more can be produced by the method described in, for example, International Publication No. 2016 / 080124.

[0125] In the case of containing a (meth)acrylic resin having a syndiotacticity (rr) expressed by a triad of 50% or more, from the viewpoint of the toughness of the film and the adhesion to the polarizer, the content of the (meth)acrylic resin having a syndiotacticity (rr) expressed by a triad of 50% or more is preferably 1% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 40% by mass or less, further preferably 10% by mass or more and 35% by mass or less, and still further preferably 15% by mass or more and 30% by mass or less, relative to the entire (meth)acrylic resin.

[0126] As the (meth)acrylic resin, a (meth)acrylic resin having a ring structure may also be used. As the (meth)acrylic resin having a ring structure, for example, a (meth)acrylic resin having a lactone ring structure, and a (meth)acrylic resin having a glutaric anhydride structure, a glutarimide structure, etc. may also be mentioned. The (meth)acrylic resin having a ring structure has high heat resistance, high moisture heat resistance, high transparency, and high mechanical strength by biaxial stretching, and is therefore preferred.

[0127] Examples of the (meth)acrylic resin having a ring structure such as a lactone ring structure include resins described in JP-A-2000-230016, JP-A-2001-151814, JP-A-2002-120326, JP-A-2002-254544, and JP-A-2005-146084.

[0128] Examples of the (meth)acrylic resin having a glutaric anhydride structure, a glutarimide structure, and the like include resins described in JP-A-6-256537, JP-A-6-11615, and JP-A-2009-203348.

[0129] The (meth)acrylic resin having a lactone ring structure preferably has a ring structure represented by the following general formula <1>.

[0130] [Chemical formula 1]

[0131]

[0132] (Where R 1 , R 2 and R 3 Each independently represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms. It should be noted that the organic residue may contain an oxygen atom. )

[0133] The content ratio of the lactone ring structure represented by the general formula <1> in the structure of the (meth) acrylic resin having a lactone ring structure is preferably 5 to 90% by mass, more preferably 10 to 70% by mass, further preferably 10 to 60% by mass, and particularly preferably 10 to 50% by mass. If the content ratio of the lactone ring structure represented by the general formula <1> in the structure of the (meth) acrylic resin having a lactone ring structure is less than 5% by mass, the heat resistance, solvent resistance, and surface hardness may become insufficient. If the content ratio of the lactone ring structure represented by the general formula <1> in the structure of the (meth) acrylic resin having a lactone ring structure is more than 90% by mass, the molding processability may be lacking. It should be noted that the ratio of the lactone ring structure in the (meth) acrylic resin having a lactone ring structure can be obtained by measuring gas chromatography and dynamic TG, for example, as described in Japanese Patent Laid-Open No. 2006-171464.

[0134] The (meth)acrylic resin having a lactone ring structure may have a structure other than the lactone ring structure represented by the general formula <1>. The structure other than the lactone ring structure represented by the general formula <1> is not particularly limited, but a method for producing the (meth)acrylic resin having a lactone ring structure is preferably to polymerize at least one selected from (meth)acrylic acid ester, a hydroxyl-containing monomer, an unsaturated carboxylic acid, and a monomer represented by the following general formula <2> to form a polymer structural unit (repeating structural unit).

[0135] [Chemical formula 2]

[0136]

[0137] (Where R 4 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group, an -OAc group, a -CN group, or a -CO-R 5 Ac represents acetyl, R 5 It represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms.

[0138] The content ratio of the structure other than the lactone ring structure represented by the general formula <1> in the (meth)acrylic resin structure having a lactone ring structure is preferably 10 to 95% by mass, more preferably 10 to 90% by mass, further preferably 40 to 90% by mass, and particularly preferably 50 to 90% by mass in the case of a polymer structural unit (repeating structural unit) formed by polymerizing a (meth)acrylic acid ester, and preferably 0 to 30% by mass, more preferably 0 to 20% by mass, further preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass in the case of a polymer structural unit (repeating structural unit) formed by polymerizing a hydroxyl group-containing monomer. In the case of a polymer structural unit (repeating structural unit) formed by polymerizing an unsaturated carboxylic acid, it is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, further preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass. In the case of a polymer structural unit (repeating structural unit) formed by polymerizing a monomer represented by the general formula <2>, it is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, further preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass.

[0139] The weight average molecular weight of the (meth)acrylic resin having a lactone ring structure is preferably 1,000 to 2,000,000, more preferably 5,000 to 1,000,000, further preferably 10,000 to 500,000, particularly preferably 50,000 to 500,000. If the weight average molecular weight is out of the above range, it is not preferred from the viewpoint of molding processability.

[0140] Examples of the thermoplastic resin to be mixed with the (meth)acrylic resin having a lactone ring structure include olefin polymers such as polyethylene, polypropylene, ethylene-propylene copolymers, and poly(4-methyl-1-pentene); halogen-containing polymers such as vinyl chloride and vinyl chloride resins; acrylic polymers such as polymethyl methacrylate; and phenylene polymers such as polystyrene, styrene-methyl methacrylate copolymers, styrene-acrylonitrile copolymers, and acrylonitrile-butadiene-styrene block copolymers. Ethylene polymers; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamides such as nylon 6, nylon 66, and nylon 610; polyacetal; polycarbonate; polyphenylene ether; polyphenylene sulfide; polyetheretherketone; polysulfone; polyethersulfone; polyoxybenzyl (Japanese: polyoxybenzyl); polyamideimide; rubber polymers such as ABS resin and ASA resin mixed with polybutadiene rubber and acrylic rubber, etc.

[0141] The (meth)acrylic resin having a glutaric anhydride structure, a glutarimide structure or the like preferably has a ring structure represented by the above-mentioned general formula <2> or the following general formula <3>.

[0142] [Chemical formula 3]

[0143]

[0144] (Where R 1 and R 2 are each independently hydrogen or an alkyl group having 1 to 8 carbon atoms, R 3 is hydrogen, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or a substituent containing an aromatic ring having 5 to 15 carbon atoms.

[0145] The content of the glutarimide structure is preferably 20% by mass or more, more preferably 20% to 95% by mass, further preferably 40% to 90% by mass, particularly preferably 50% to 80% by mass, of the (meth)acrylic resin having the glutarimide structure.

[0146] When the content of the glutarimide unit is within the above range, the heat resistance and transparency of the obtained (meth)acrylic resin having glutarimide groups will not be reduced, nor will the molding processability and the mechanical strength when processed into a film be extremely reduced.

[0147] On the other hand, if the content of the glutarimide unit is less than the above range, the heat resistance of the obtained glutarimide resin tends to be insufficient or the transparency tends to be impaired. On the other hand, if the content exceeds the above range, the heat resistance and melt viscosity tend to be unnecessarily high, the molding processability tends to be poor, or the mechanical strength during film processing tends to be extremely low or the transparency tends to be impaired.

[0148] The weight average molecular weight of the (meth) acrylic resin having a glutarimide structure is not particularly limited, and is preferably 10,000 to 500,000. If it is within the above range, there will be no reduction in molding processability or insufficient mechanical strength during film processing. On the other hand, if the weight average molecular weight is less than the above range, there is a tendency for insufficient mechanical strength when the film is made. In addition, if it is greater than the above range, there is a tendency for high viscosity during melt extrusion, reduced molding processability, and reduced productivity of molded products.

[0149] Moreover, as a (meth)acrylic resin, the mixture or copolymer of (meth)acrylic acid ester and the imide compound which is a thermoplastic resin is mentioned. Examples of the imide compound include maleimide, and N-substituted maleimides such as N-methylmaleimide, N-ethylmaleimide, N-n-propylmaleimide, N-isopropylmaleimide, N-n-butylmaleimide, N-isobutylmaleimide, N-sec-butylmaleimide, N-tert-butylmaleimide, N-n-pentylmaleimide, N-n-hexylmaleimide, N-n-heptylmaleimide, N-n-octylmaleimide, N-laurylmaleimide, N-stearylmaleimide, N-cyclopropylmaleimide, N-cyclobutylmaleimide, N-cyclopentylmaleimide, N-cyclohexylmaleimide, N-cycloheptylmaleimide, and N-cyclooctylmaleimide. These maleimide compounds can be used alone or in combination of two or more.

[0150] From the perspective of the impact resistance and film-forming properties of the film, the (meth) acrylic resin preferably contains acrylic rubber particles. The amount of acrylic rubber particles that can be included in the (meth) acrylic resin is preferably 5% by mass or more, more preferably 10% by mass or more relative to the total amount of the (meth) acrylic resin and the acrylic rubber particles, 100% by mass. The upper limit of the amount of acrylic rubber particles is not critical, but if the amount of acrylic rubber particles is too much, the surface hardness of the film is reduced, and in addition, when the film is subjected to surface treatment, the solvent resistance to organic solvents in the surface treatment agent is reduced. Therefore, the amount of acrylic rubber particles that can be included in the (meth) acrylic resin is preferably 80% by mass or less, more preferably 60% by mass or less.

[0151] Acrylic rubber particles are particles containing an elastic polymer mainly composed of acrylic ester as an essential component, and may be particles of a single-layer structure consisting essentially of the elastic polymer alone, or may be particles of a multilayer structure in which the elastic polymer is one layer. As the elastic polymer, specifically, a cross-linked elastic copolymer obtained by polymerization of monomers consisting of 50 to 99.9% by mass of an alkyl acrylate, 0 to 49.9% by mass of at least one other vinyl monomer copolymerizable therewith, and 0.1 to 10% by mass of a copolymerizable cross-linking monomer is preferably used.

[0152] Examples of the alkyl acrylate include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, etc., and the number of carbon atoms in the alkyl group thereof is generally about 1 to 8. In addition, examples of other vinyl monomers copolymerizable with the alkyl acrylate include compounds having one polymerizable carbon-carbon double bond in the molecule, more specifically, methacrylates such as methyl methacrylate, aromatic vinyl compounds such as styrene, vinyl cyanide compounds such as acrylonitrile, etc. In addition, examples of the copolymerizable crosslinking monomers include crosslinking compounds having at least two polymerizable carbon-carbon double bonds in the molecule, more specifically, (meth)acrylates of polyols such as ethylene glycol di(meth)acrylate and butanediol di(meth)acrylate, allyl (meth)acrylate, alkenyl (meth)acrylates such as methallyl (meth)acrylate, divinylbenzene, etc.

[0153] In addition to the acrylic rubber particles, the (meth)acrylic resin may contain common additives such as ultraviolet absorbers, organic dyes, pigments, inorganic pigments, antioxidants, antistatic agents, surfactants, etc. Among them, ultraviolet absorbers are preferably used in terms of improving weather resistance. Examples of the ultraviolet absorber include 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(5-methyl-2-hydroxyphenyl)-2H-benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-pentyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, Benzotriazole-based ultraviolet absorbers such as 2-(2'-hydroxy-5'-tert-octylphenyl)-2H-benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)-2H-benzotriazole; 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-4'-chlorobenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone; salicylic acid phenyl ester-based ultraviolet absorbers such as p-tert-butylphenyl salicylate and p-octylphenyl salicylate, and two or more thereof can be used as needed. When the (meth)acrylic resin contains a UV absorber, the amount thereof is usually 0.1% by mass or more, preferably 0.3% by mass or more, and preferably 2% by mass or less, based on 100% by mass of the total amount of the (meth)acrylic resin and the UV absorber.

[0154] As a method for obtaining a (meth) acrylic resin film, various methods commonly known such as a method using a flow divider, a method using a multi-manifold die head, etc. can be used. Wherein, from the aspect of being able to obtain a good film with surface properties, it is preferred that, for example, a flow divider is used for lamination, multilayer melt extrusion is performed from a T-die, and at least one side of the obtained laminated film-like object is contacted with a roller or a belt and a method for film making. Particularly from the viewpoint of improving the surface smoothness and surface glossiness of the (meth) acrylic resin film, it is preferred that the two sides of the laminated film-like object obtained by the above-mentioned multilayer melt extrusion are contacted with a roller surface or a belt surface and a method for filmization. In the roller or belt used at this time, in order to give smoothness to the (meth) acrylic resin film surface, the roller surface or the belt surface contacted with the (meth) acrylic resin preferably has a mirror surface. In order to improve film strength, the obtained film can be stretched.

[0155] The film formed by the (meth) acrylic resin is not easy to produce phase difference in the unstretched state, but it will produce phase difference if stretched, so a substance that functions as a phase difference reducing agent can be added to the (meth) acrylic resin, so that no phase difference will be produced even if stretched. As the phase difference reducing agent, styrene-acrylonitrile copolymer can be mentioned. The phase difference value can be controlled by the stretching ratio and the amount of the phase difference reducing agent.

[0156] The thickness of the (meth)acrylic resin film is usually 1 μm to 80 μm, preferably 3 μm to 65 μm, more preferably 5 μm to 55 μm, further preferably 7 μm to 45 μm, particularly preferably 20 μm to 45 μm.

[0157] The glass transition temperature of the (meth)acrylic resin film is 100°C or more, preferably 110°C or more, more preferably 115°C or more, and further preferably 120°C or more. In addition, the glass transition temperature is usually 170°C or less. When the glass transition temperature of the (meth)acrylic resin film is 110°C or more, there is a tendency that the change of the molecular orientation of the (meth)acrylic resin in the (meth)acrylic resin film under a high temperature environment is suppressed, the change of the phase difference value Re and the phase difference value Rth in the thickness direction is suppressed, and the light leakage under a high temperature environment is more effectively suppressed. The phase difference value Re and the phase difference value Rth in the thickness direction of the (meth)acrylic resin film are phase difference values ​​at a wavelength of 587nm.

[0158] When the absolute value of the retardation value Rth in the thickness direction of the (meth)acrylic resin film is 15 nm or less, the (meth)acrylic resin film can be used as both an optical compensation film and a polarizing plate protective film in an IPS liquid crystal display device.

[0159] The absolute value of the retardation value Rth in the thickness direction of the (meth)acrylic resin film is preferably 11 nm or less, more preferably 8 nm or less, and further preferably 5 nm or less.

[0160] The absolute value of the retardation value Rth in the thickness direction of the (meth)acrylic resin film after a test in which the film is stored for 360 hours at a temperature of 85° C. and a relative humidity of 85% RH is preferably 15 nm or less. The retardation value Rth in the thickness direction is defined by the above formula (2).

[0161] The absolute value of the retardation value Rth in the thickness direction of the (meth)acrylic resin film is more preferably 11 nm or less, further preferably 8 nm or less, and particularly preferably 5 nm or less.

[0162] The absolute value of the change in the thickness direction retardation Rth of the (meth)acrylic resin film before and after the test of storing the film at a temperature of 85°C and a relative humidity of 85% RH for 360 hours is preferably 10 nm or less. The thickness direction retardation Rth is defined by the above formula (2).

[0163] The absolute value of the variation amount of the retardation value Rth in the thickness direction of the (meth)acrylic resin film is more preferably 7 nm or less, further preferably 5 nm or less, and particularly preferably 3 nm or less.

[0164] If the absolute value of the change in the retardation value Rth in the thickness direction of the (meth)acrylic resin film is less than 10 nm, the change in the retardation value of the (meth)acrylic resin film in a high temperature environment is small, and thus it is more likely to suppress light leakage in a high temperature environment. If it is such a (meth)acrylic resin film, the reason is not clear, but it is speculated that changes in molecular orientation and molecular structure in the (meth)acrylic resin film caused by moisture in the polarizing plate laminate in a high temperature environment are suppressed.

[0165] <Polarizing Plate>

[0166] A polarizer is a film having the function of selectively transmitting linear polarized light in a certain direction from natural light. As polarizers, for example, there can be cited iodine-based polarizers formed by adsorbing and oriented iodine as a dichroic pigment on a polyvinyl alcohol resin film, dye-based polarizers formed by adsorbing and oriented dichroic dyes as dichroic pigments on a polyvinyl alcohol resin film, and coated polarizers formed by coating dichroic dyes in a lyotropic liquid crystal state and oriented and fixed. These polarizers selectively transmit linear polarized light in a certain direction from natural light and absorb linear polarized light in another direction, and are therefore called absorption-type polarizers.

[0167] The polarizer is not limited to an absorptive polarizer, but may also be a reflective polarizer that selectively transmits linear polarized light in a certain direction from natural light and reflects linear polarized light in another direction, or a scattering polarizer that scatters linear polarized light in another direction. From the perspective of excellent visibility when the polarizing plate is applied to a liquid crystal display device, etc., an absorptive polarizer is preferred.

[0168] Among them, the polarizer is more preferably a polyvinyl alcohol polarizer composed of a polyvinyl alcohol resin, further preferably a polyvinyl alcohol polarizer formed by adsorbing and oriented dichroic pigments such as iodine and dichroic dyes on a polyvinyl alcohol resin film, and particularly preferably a polyvinyl alcohol polarizer formed by adsorbing and oriented iodine on a polyvinyl alcohol resin film.

[0169] The polyvinyl alcohol-based polarizing plate can be produced by a conventionally known method using a polyvinyl alcohol-based resin film (or layer).

[0170] The thickness of the polarizer can be set to 30 μm or less, preferably 25 μm or less (e.g., 20 μm or less, further 15 μm or less, further 10 μm or less, further 8 μm or less). The thickness of the polarizer 30 is usually 2 μm or more. Reducing the thickness of the polarizer is beneficial to the thinning of the polarizing plate, and further the liquid crystal panel and liquid crystal display device using the polarizer.

[0171] The visibility-corrected polarization degree of the polarizing plate may be, for example, 99.00% or more, preferably 99.90% or more, more preferably 99.98% or more, further preferably 99.99% or more, and is usually 100% or less, for example, less than 100%.

[0172] The visibility-corrected transmittance of the polarizing plate may be, for example, 40% or more, preferably 41% or more, more preferably 42% or more, further preferably 43% or more, and is usually 50.0% or less, for example, less than 50.0%, or 49.0% or less.

[0173] The visibility-corrected polarization degree and visibility-corrected transmittance of the polarizing plate can be calculated by performing visibility correction on the polarization degree and transmittance obtained using a spectrophotometer with an integrating sphere (e.g., "V7100" manufactured by JASCO Corporation) using a 2-degree field of view (light source C) of "JIS Z8701".

[0174] <Adhesive layer>

[0175] The first adhesive layer for laminating polarizer with polyester resin film and the second adhesive layer for laminating polarizer with (methyl) acrylic resin film can be formed by known adhesive composition respectively. The first adhesive layer and the second adhesive layer can be adhesive layers formed by the same adhesive composition, or adhesive layers formed by different adhesive compositions. In addition, the first adhesive layer and the second adhesive layer can be adhesive layers formed by water-based adhesive compositions, or adhesive layers formed by curable adhesive compositions cured by irradiation of active energy rays such as heating or ultraviolet rays, visible light, electron beams, and X-rays.

[0176] As the water-based adhesive composition, for example, a composition obtained by dissolving a polyvinyl alcohol-based resin or a carbamate resin as a main component in water, and a composition obtained by dispersing a polyvinyl alcohol-based resin or a carbamate resin as a main component in water can be cited. The water-based adhesive composition can further contain curing components such as polyaldehyde, melamine-based compounds, zirconium oxide compounds, zinc compounds, glyoxal compounds, water-soluble epoxy resins, and crosslinking agents. As the water-based adhesive composition, for example, an adhesive composition described in Japanese Patent Publication No. 2010-191389, an adhesive composition described in Japanese Patent Publication No. 2011-107686, a composition described in Japanese Patent Publication No. 2020-172088, and a composition described in Japanese Patent Publication No. 2005-208456 can be cited.

[0177] The curable adhesive composition is preferably an active energy ray-curable adhesive composition that contains a curable (polymerizable) compound as a main component and is cured by irradiation with active energy rays. Examples of the active energy ray-curable adhesive composition include a cationic polymerizable adhesive composition containing a cationic polymerizable compound as a curable compound, a free radical polymerizable adhesive composition containing a free radical polymerizable compound as a curable compound, and a mixed adhesive composition containing both a cationic polymerizable compound and a free radical polymerizable compound as curable compounds.

[0178] The cationically polymerizable compound is a compound or oligomer that is cured by cation polymerization reaction when irradiated with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays or heated, and specific examples thereof include epoxy compounds, oxetane compounds, and vinyl compounds.

[0179] Examples of epoxy compounds include alicyclic epoxy compounds (compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule) such as 3,4-epoxycyclohexanecarboxylic acid 3,4-epoxycyclohexylmethyl ester; aromatic epoxy compounds (compounds having an aromatic ring and an epoxy group in the molecule) such as diglycidyl ether of bisphenol A; and aliphatic epoxy compounds (compounds having at least one oxirane ring bonded to an aliphatic carbon atom in the molecule) such as 2-ethylhexyl glycidyl ether and 1,4-butanediol diglycidyl ether.

[0180] Examples of the oxetane compound include compounds having one or more oxetane rings in the molecule, such as 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.

[0181] The cationic polymerization type adhesive composition preferably contains a cationic polymerization initiator. The cationic polymerization initiator may be a thermal cationic polymerization initiator or a photocationic polymerization initiator. As the cationic polymerization initiator, aromatic diazonium salts such as benzene diazonium hexafluoroantimonate; aromatic iodonium salts such as diphenyl iodonium tetrakis (pentafluorophenyl) borate; aromatic sulfonium salts such as triphenyl sulfonium hexafluorophosphate; iron-arene complexes such as ditoluene-cyclopentadienyl iron (II) hexafluoroantimonate, etc. The content of the cationic polymerization initiator is usually 0.1 to 10 parts by mass relative to 100 parts by mass of the cationic polymerization compound. The cationic polymerization initiator may contain two or more kinds.

[0182] Examples of the cationically polymerizable adhesive composition include cationically polymerizable compositions described in JP-A Nos. 2016-126345 and 2021-113969.

[0183] The free radical polymerizable compound is a compound or oligomer that is cured by free radical polymerization reaction by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, or heating, and specifically, a compound having an ethylenically unsaturated bond can be cited. As the compound having an ethylenically unsaturated bond, a (meth)acrylic compound having one or more (meth)acryloyl groups in the molecule, a vinyl compound having one or more vinyl groups in the molecule, etc. can be cited.

[0184] Examples of the (meth)acrylic compound include (meth)acrylic group-containing compounds such as (meth)acrylic oligomers having at least two (meth)acryloyl groups in a molecule obtained by reacting two or more of a (meth)acrylic ester monomer, a (meth)acrylamide monomer, and a functional group-containing compound having at least one (meth)acryloyloxy group in a molecule.

[0185] The radical polymerization adhesive composition preferably contains a radical polymerization initiator. The radical polymerization initiator may be a thermal radical polymerization initiator or a photoradical polymerization initiator. As the radical polymerization initiator, acetophenone-based initiators such as acetophenone and 3-methylacetophenone; benzophenone-based initiators such as benzophenone, 4-chlorobenzophenone, and 4,4'-diaminobenzophenone; benzoin ether-based initiators such as benzoin propyl ether and benzoin ethyl ether; thioxanthone-based initiators such as 4-isopropylthioxanthone; xanthone, fluorenone, etc. The content of the radical polymerization initiator is usually 0.1 to 10 parts by mass relative to 100 parts by mass of the radical polymerizable compound. The radical polymerization initiator may contain two or more kinds.

[0186] Examples of the radical polymerizable adhesive composition include radical polymerizable compositions described in JP-A-2016-126345, JP-A-2016-153474, and International Publication No. 2017 / 183335.

[0187] The active energy ray-curable adhesive composition may contain additives such as ion trapping agents, antioxidants, chain transfer agents, tackifiers, thermoplastic resins, fillers, flow regulators, plasticizers, defoamers, antistatic agents, leveling agents, and solvents as necessary.

[0188] The bonding of the polarizer and the polyester resin film can be carried out as follows: an adhesive composition is applied to at least one bonding surface selected from the bonding surface of the polarizer and the bonding surface of the polyester resin film, the two are overlapped with the aid of a coating layer of the adhesive composition, and after bonding by pressing from top and bottom using a bonding roller, the adhesive layer is dried, irradiated with active energy rays to cure it, or heated to cure it.

[0189] The coating layer of the adhesive composition can be formed by various coating methods such as a die coater, a comma coater, a gravure coater, a wire bar coater, and a knife coater.

[0190] Alternatively, the adhesive composition may be cast between the polarizer and the polyester resin film while continuously supplying the film so that the bonding surfaces of the polarizer and the polyester resin film face inward.

[0191] Before forming the adhesive layer coating, at least one of the bonding surfaces selected from the bonding surfaces of the polarizer and the polyester resin film may be subjected to an adhesion-facilitating treatment such as saponification treatment, corona treatment, plasma treatment, primer treatment, anchor coating treatment, etc.

[0192] The bonding of the polarizing plate and the acrylic resin film can be performed in the same manner as the bonding of the polarizing plate and the polyester resin film.

[0193] The light irradiation intensity during irradiation with active energy rays is determined according to the composition of the active energy ray-curable adhesive composition and is not particularly limited, but is preferably 10 mW / cm 2 Above and 1,000mW / cm 2 It should be noted that the irradiation intensity is preferably an intensity in the wavelength region effective for the activation of the photocationic polymerization initiator or the photoradical polymerization initiator. The irradiation is performed once or multiple times with such a light irradiation intensity, and the accumulated light amount is preferably set to 10 mJ / cm 2 More preferably, 100 mJ / cm 2 Above and 1,000mJ / cm 2 the following.

[0194] The light source used for polymerizing and curing the active energy ray-curable adhesive composition is not particularly limited, and examples thereof include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.

[0195] When the first adhesive layer and the second adhesive layer are formed of a water-based adhesive composition, the thickness of the first adhesive layer and the second adhesive layer can be, for example, 5 μm or less, preferably 1 μm or less, more preferably 0.5 μm or less, and can be 0.01 μm or more, preferably 0.05 μm or more.

[0196] When the first adhesive layer and the second adhesive layer are formed by a curable adhesive composition (preferably an active energy ray-curable adhesive composition), the thickness of the first adhesive layer and the second adhesive layer can be, for example, 10 μm or less, preferably 5 μm or less, more preferably 3 μm or less, and can be 0.1 μm or more, preferably 0.5 μm or more, more preferably 1 μm or more.

[0197] The first adhesive layer and the second adhesive layer are preferably formed of the same type of adhesive composition.

[0198] It is preferred that the first adhesive layer and the second adhesive layer are each formed of a cationically polymerizable adhesive composition.

[0199] The first adhesive layer and the second adhesive layer may have the same thickness or different thicknesses, but are preferably the same thickness. It should be noted that “the same thickness” also includes an error of about 0.3 μm.

[0200] <Other constituent conditions>

[0201] The polarizing plate of the present invention may further include an optical functional film in order to impart a desired optical function. Examples of the optical functional film include a retardation film, a light-collecting plate, and a brightness-enhancing film.

[0202] The optically functional film is bonded to the polarizing plate via an adhesive layer or a pressure-sensitive adhesive layer. Examples of the adhesive layer and the pressure-sensitive adhesive layer include the same ones as those described above and the pressure-sensitive adhesive layer described below.

[0203] <Polarizing plate with adhesive layer>

[0204] The present invention also relates to a polarizing plate with an adhesive layer comprising the above-mentioned polarizing plate and an adhesive layer. The polarizing plate with an adhesive layer can be applied to a liquid crystal display device, for example. In the liquid crystal display device, the polarizing plate with an adhesive layer is arranged on the viewing side and / or the back side of a liquid crystal unit as an image display element.

[0205] Examples of the layer constitution of the polarizing plate with an adhesive layer of the present invention are shown below. Figure 6 . Figure 6 The polarizing plate 2 with an adhesive layer shown includes a polarizing plate and an adhesive layer 40 , and the polarizing plate includes a light diffusion layer 5 , a polyester resin film 10 , a first adhesive layer 15 , a polarizer 30 , a second adhesive layer 25 , and a (meth)acrylic resin film 20 in this order.

[0206] picture Figure 6 As in the polarizing plate 2 with an adhesive layer shown, the adhesive layer 40 is preferably laminated on the surface of the light diffusion layer 5 on the opposite side to the polarizer 30 .

[0207] The polarizing plate with an adhesive layer can be bonded to a liquid crystal cell via the adhesive layer 40. That is, from the viewpoint of visibility, the polarizing plate of the present invention is preferably arranged so that the light diffusion layer 5 side is the viewing side in a liquid crystal panel or a liquid crystal display device.

[0208] The adhesive layer 40 may be laminated on either the light diffusion layer 5 or the (meth) acrylic resin film 20, but as described above, it is preferably laminated on the (meth) acrylic resin film 20. If the adhesive layer 40 is laminated on the (meth) acrylic resin film, the light diffusion layer 5 is disposed on the side opposite to the image display element (e.g., the observation side). It should be noted that, when an optically functional film is laminated on the side opposite to the side of the polarizer 30 of the (meth) acrylic resin film, the adhesive layer 40 may be further laminated on the side opposite to the (meth) acrylic resin film 20 of the optically functional film.

[0209] Examples of the adhesive composition forming the adhesive layer include adhesive compositions containing (meth)acrylic resins, silicone resins, polyester resins, polyurethane resins, polyether resins, etc. as base polymers. Among them, (meth)acrylic adhesive compositions containing (meth)acrylic resins are preferred from the viewpoints of transparency, adhesive strength, reliability, heat resistance, reworkability, etc.

[0210] The thickness of the pressure-sensitive adhesive layer is determined based on adhesive strength and the like, and is, for example, 1 μm to 50 μm, preferably 2 μm to 40 μm, and more preferably 3 μm to 30 μm.

[0211] Example

[0212] The present invention will be described in further detail below with reference to Examples. "%" and "parts" in the examples are by mass % and by mass parts unless otherwise specified.

[0213] (Manufacturing Example 1: Manufacturing of Polarizing Plate)

[0214] A long polyvinyl alcohol film (average degree of polymerization: about 2400, degree of saponification: 99.9 mol % or more, thickness: 60 μm) is continuously conveyed and immersed in a swelling bath containing pure water at 20°C for a residence time of 31 seconds (swelling process). Then, the film pulled out from the swelling bath is immersed in a dyeing bath containing iodine at 30°C with a potassium iodide / water ratio of 2 / 100 (mass ratio) for a residence time of 122 seconds (dyeing process). Next, the film pulled out from the dyeing bath is immersed in a cross-linking bath at 56°C with a potassium iodide / boric acid / water ratio of 12 / 4.1 / 100 (mass ratio) for a residence time of 70 seconds, and then immersed in a cross-linking bath at 40°C with a potassium iodide / boric acid / water ratio of 9 / 2.9 / 100 (mass ratio) for a residence time of 13 seconds (cross-linking process). In the dyeing process and the cross-linking process, longitudinal uniaxial stretching is performed by stretching between rollers in the bath. The total stretching ratio based on the original film was set to 5.5 times. Next, the film pulled out from the crosslinking bath was immersed in a cleaning bath containing pure water at 5°C for a residence time of 3 seconds (cleaning process), and then introduced into a drying furnace at 80°C for a residence time of 190 seconds for drying (drying process), thereby obtaining a polarizer. The thickness of the polarizer obtained above was 24 μm.

[0215] (Production Example 2: Production of polyethylene terephthalate resin (1))

[0216] While heating the esterification reaction tank to 200°C, 86.4 parts of terephthalic acid and 64.6 parts of ethylene glycol were added to the esterification reaction tank to obtain a mixture. While stirring the obtained mixture, 0.017 parts of antimony trioxide, 0.064 parts of magnesium acetate tetrahydrate, and 0.16 parts of triethylamine were added to the obtained mixture as catalysts. The gauge pressure in the esterification reaction tank was set to 0.34MPa, and after further pressurized esterification reaction at 240°C, the esterification reaction tank was returned to normal pressure and 0.014 parts of phosphoric acid were added. In addition, the temperature was raised to 260°C for 15 minutes, and 0.012 parts of trimethyl phosphate were added to obtain a mixture. The obtained mixture was dispersed with a high-pressure disperser after 15 minutes, and the obtained esterification reaction product was transported to a polycondensation reaction tank after 15 minutes, and a polycondensation reaction was carried out under reduced pressure at 280°C.

[0217] After the polycondensation reaction is completed, the product is filtered using a NASLON filter with a 95% cutoff diameter of 5 μm, extruded from a nozzle into a bundle, cooled and solidified using cooling water that has been previously filtered (pore size: less than 1 μm), and cut into pellets to obtain a polyethylene terephthalate resin (hereinafter referred to as PET (1)).

[0218] (Production Example 3: Production of polyethylene terephthalate resin (2))

[0219] 10 parts of the dried ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) were mixed with 90 parts of PET (1) obtained in Production Example 2, and a polyethylene terephthalate resin (2) (hereinafter referred to as PET (2)) containing an ultraviolet absorber was obtained using a kneading extruder.

[0220] (Production Example 4: Preparation of coating liquid for forming an easily adhesive layer)

[0221] A water-dispersible sulfonic acid metal salt group-containing copolyester resin was prepared by a conventional method by subjecting a dicarboxylic acid component comprising 46 mol % of terephthalic acid, 46 mol % of isophthalic acid and 8 mol % of 5-sodium sulfonate of isophthalic acid (Japanese: 5-sulfonate sodium natrium) and a diol component comprising 50 mol % of ethylene glycol and 50 mol % of neopentyl glycol to an ester exchange reaction and a polycondensation reaction.

[0222] Next, 51.4 parts of water, 38 parts of isopropyl alcohol, 5 parts of n-butyl cellosolve, and 0.06 parts of a nonionic surfactant were mixed to obtain a mixture. While the obtained mixture was heated and stirred to 77° C., 5 parts of the above-mentioned water-dispersible copolyester resin containing a sulfonic acid metal salt group was added, and stirring was continued until the resin was no longer solidified to obtain a resin aqueous dispersion. The obtained resin aqueous dispersion was cooled to 25° C. to obtain a uniform water-dispersible copolyester resin liquid with a solid content concentration of 5.0% by mass.

[0223] 3 parts of agglomerated silica particles were dispersed in 50 parts of water to obtain an aqueous dispersion of agglomerated silica particles. 0.54 parts of the aqueous dispersion of agglomerated silica particles was added to 99.46 parts of the water-dispersible copolyester resin solution, and 20 parts of water was further added while stirring to obtain a coating solution for forming an easily adhesive layer.

[0224] (Manufacturing Example 5: Manufacture of Protective Film 1)

[0225] PET (3) prepared by mixing 90 parts of PET (1) prepared in Production Example 2 and 10 parts of PET (2) prepared in Production Example 3 was dried under reduced pressure at 135°C for 6 hours and then supplied to extruder 2 (for the intermediate layer B layer). PET (1) was dried and then supplied to extruder 1 (for the outer layer A layer and the outer layer C layer). PET (1) supplied to extruder 1 and PET (3) supplied to extruder 2 were melted at 285°C. The two polymers were filtered using a filter material (nominal filtration accuracy 95% cutoff for particles of 10 μm) of a sintered stainless steel body, respectively, and laminated using two types of three-layer confluence blocks, extruded from a pipe head into a sheet, and then wound on a casting drum with a surface temperature of 30°C using an electrostatic casting method, and cooled and solidified to produce an unstretched PET film. At this time, the discharge amount of each extruder was adjusted so that the thickness ratio of the A layer, the B layer, and the C layer became 10:80:10.

[0226] Next, the unstretched PET film was coated on both sides by a reverse roll method in an amount of 0.08 g / m 2 The coating liquid for forming an easily adhesive layer was applied in a manner of , and then dried at 80° C. for 20 seconds.

[0227] The unstretched PET film having the coating layer formed thereon was stretched to 4.0 times in the width direction in a hot air zone at a temperature of 125° C. using a tenter stretching machine while holding the ends of the film with a clamp. Next, the film was treated at a temperature of 225° C. for 10 seconds while maintaining the stretched width in the width direction, and further subjected to a relaxation treatment of 3.0% in the width direction, thereby obtaining a uniaxially stretched PET film having a film thickness of about 80 μm and having an easy-adhesion layer formed thereon. This was referred to as a protective film 1.

[0228] (Manufacturing Example 6: Manufacture of Protective Film 2)

[0229] A mixture of 90 parts of a (meth)acrylic resin having a lactone ring structure and 10 parts of an acrylonitrile-styrene (AS) resin (lactone ring content: 28.5%) was extruded to obtain a 40 μm thick acrylic resin film stretched 2.0 times in the longitudinal direction and 2.4 times in the transverse direction. This was used as protective film 2.

[0230] (Manufacturing Example 7: Manufacture of Light-Diffusion Film 1 with Release Film)

[0231] Relative to 100 parts by mass of an acrylic adhesive having a refractive index of 1.46, 0.16 parts by mass of an isocyanate crosslinking agent (D-101E, manufactured by Mitsui Chemicals) was added, and 58 parts by mass of spherical acrylic particles (MX-1000, manufactured by Soken Chemicals) having an average particle size of 10 μm and a refractive index of 1.49 as a light diffusing agent were mixed, and stirred to prepare an adhesive composition. Then, the adhesive composition was applied to a release sheet having a thickness of 38 μm, dried to form an adhesive layer, and a release sheet was further attached to the adhesive layer, and aged for 10 days at a temperature of 23°C and a relative humidity of 65% to prepare an adhesive sheet. A light diffusing adhesive layer having a thickness of 25 μm and a total haze of 70% of the adhesive layer after drying was obtained.

[0232] After peeling one release film from the light-diffusing adhesive sheet prepared above, a triacetylcellulose (TAC) film was bonded thereto to obtain a release-film-attached light-diffusing film 1. In addition, the total haze of the TAC film can be regarded as zero.

[0233] (Manufacturing Example 8: Manufacture of Light-Diffusion Film 2 with Release Film)

[0234] In the same manner as in the method for obtaining the light-diffusion layer 1 with a release film, 35 parts by mass of a light-diffusion agent was mixed so as to have a desired haze, thereby obtaining the light-diffusion film 2 with a release film having a total haze of 40% in the pressure-sensitive adhesive layer.

[0235] <Example 1>

[0236] Corona treatment is applied to one side of the protective film 1 with light diffusion layer and the protective film 2, respectively, and an epoxy-based ultraviolet curing adhesive is applied to the corona-treated surface using an adhesive coating device. Next, the polarizer obtained in the above-mentioned manufacturing example 1 is overlapped on the coating layer, and then pressed and bonded using a bonding roller, thereby obtaining a polarizing plate precursor. At this time, bonding is performed in a manner such that the stretching direction (width direction) of the protective film 1 (polyester resin film) is orthogonal to the absorption axis direction (stretching direction of the polarizer). For the polarizing plate precursor, an ultraviolet irradiation device with a conveyor belt (the lamp is a metal halide lamp manufactured by EYE GRAPHICS) is used, and the accumulated light amount becomes 200mJ / cm 2 The polarizing plate was obtained by irradiating the protective film 2 (meth) acrylic resin film side with ultraviolet light (UVB) to cure the adhesive. As described above, a polarizing plate having protective film 1 (polyester resin film) / adhesive layer / polarizer / adhesive layer / protective film 2 ((meth) acrylic resin film) was obtained.

[0237] The surface of the polyester resin film of the above-mentioned polarizing plate that is different from the polarizer side is corona treated, and after the release film of the light-diffusing film 1 with a release film prepared in Manufacturing Example 7 is peeled off, a light-diffusing adhesive layer is bonded to the corona-treated surface to obtain a light-diffusing polarizing plate having a laminated structure of light-diffusing layer (triacetylcellulose film / light-diffusing adhesive layer) / protective film 1 (polyester resin film) / adhesive layer / polarizer / adhesive layer / protective film 2 ((meth)acrylic resin film).

[0238] (Preparation of Polarizing Plate with Adhesive Layer)

[0239] Next, an adhesive layer with a release film having a (meth) acrylic adhesive layer (thickness 20 μm) without light diffusion on the release treated surface is prepared. After the surface of the protective film 2 (meth) acrylic resin film is corona treated, the adhesive layer with a release film is laminated on the protective film 2 ((meth) acrylic resin film) side of the above-mentioned light diffusing polarizing plate, thereby obtaining a polarizing plate with an adhesive layer. The polarizing plate with an adhesive layer has a structure of light diffusion layer (triacetylcellulose film / light diffusing adhesive layer) / protective film 1 (polyester resin film) / adhesive layer / polarizer / adhesive layer / protective film 2 ((meth) acrylic resin film) / adhesive layer / release film.

[0240] <Example 2>

[0241] Except having used the light-diffusion film 2 with a release film produced in Production Example 8, it carried out similarly to Example 1, and obtained the polarizing plate with an adhesive layer.

[0242] <Comparative Example 1>

[0243] A pressure-sensitive adhesive layer-attached polarizing plate was obtained in the same manner as in Example 1, except that a polarizing plate was used instead of the light diffusing polarizing plate.

[0244] <Comparative Example 2>

[0245] A protective film of biaxially stretched polyethylene terephthalate (PET) containing a polyester resin having a thickness of 38 μm (manufactured by Mitsubishi Chemical Corporation) was prepared. Table 1 shows the retardation values ​​Re (Re1 to Re4) of the polyester resin film.

[0246] A polarizing plate and a polarizing plate with an adhesive layer were obtained in the same manner as in Comparative Example 1 except that a polyester resin film having a thickness of 38 μm was used as the polyester resin film. It should be noted that the polarizing plate was bonded in the same manner as in Example 1 in such a manner that the stretching direction (width direction) of the protective film of biaxially stretched polyethylene terephthalate was orthogonal to the absorption axis direction of the polarizer (stretching direction of the polarizer). The stretching direction (width direction) of the protective film of biaxially stretched polyethylene terephthalate refers to the width direction when the film is unrolled from the film roll.

[0247] (Measurement of Phase Difference Value of Polyester Resin Film)

[0248] The retardation values ​​Re1 to Re4 of the polyester resin films used in Examples and Comparative Examples were measured at a wavelength of 587 nm using a retardation measuring device (manufactured by Oji Scientific Instruments Co., Ltd., KOBRA-HB-RESPC).

[0249] Re1: A phase difference value measured in a first arrangement in which the polyester resin film is arranged so that the angle between the surface of the polyester resin film and the measurement direction becomes 90°.

[0250] Re2: The phase difference value measured in the second configuration, wherein the polyester resin film in the first configuration is rotated 30° about its fast axis so that the angle between the surface of the polyester resin film and the measuring direction becomes 60°.

[0251] Re3: The phase difference value measured in the third configuration, wherein the polyester resin film in the first configuration is rotated 30° around an axis forming an angle of 45° relative to its fast axis within the surface of the polyester resin film, thereby configuring the polyester resin film in such a way that the angle between the surface of the polyester resin film and the measuring direction becomes 60°.

[0252] Re4: The phase difference value measured in the fourth configuration, wherein the polyester resin film in the first configuration is rotated 30° about its slow axis so that the angle between the surface of the polyester resin film and the measuring direction becomes 60°.

[0253] <Glass transition temperature>

[0254] The glass transition temperature (Tg) of the (meth)acrylic resin film used in Examples and Comparative Examples was determined using a differential scanning calorimeter (EXSTAR6000 manufactured by Seiko Instruments).

[0255] <Measurement of Phase Difference Value in Thickness Direction of (Meth)Acrylic Resin Film>

[0256] The (meth)acrylic resin films used in the examples and comparative examples were measured for the retardation value Rth in the thickness direction at a wavelength of 587 nm using a retardation measuring device (manufactured by Oji Scientific Instruments Co., Ltd., KOBRA-WPR) in a state where the angle between the surface of the (meth)acrylic resin film and the measurement direction was 50°, and the absolute value of the retardation value Rth in the thickness direction was calculated. The results are shown in Table 1.

[0257] <Measurement of Phase Difference Value in Thickness Direction of Polyester Resin Film>

[0258] The phase difference Rth in the thickness direction of the polyester resin film used in the Examples and Comparative Examples was measured at a wavelength of 587 nm using a phase difference measuring device (manufactured by Oji Instruments Co., Ltd., KOBRA-HB-RESPC) with the angle between the surface of the polyester resin film and the measuring direction being 60°. In addition, Re / Rth was calculated from the phase difference Rth in the thickness direction and the phase difference Re. The results are shown in Table 1.

[0259] <Measurement of haze of light diffusion layer>

[0260] After peeling off the release film of the light diffusion film with a release film, the haze was measured using a sample obtained by laminating an adhesive sheet containing an adhesive layer to a glass substrate (thickness 0.7 mm, "Eagle XG" manufactured by Corning). In the measurement of haze, a haze transmittance meter according to JIS K 7136 (manufactured by Murakami Color Research Institute, haze meter "HM-150") was used. It should be noted that the total haze of the glass substrate used can be regarded as 0.

[0261] <Measurement of rainbow pattern>

[0262] After peeling the release film from the pressure-sensitive adhesive layer-attached polarizing plate obtained in Example 1, the pressure-sensitive adhesive layer side was bonded to an alkali-free glass substrate (thickness 0.7 mm, “Eagle XG” manufactured by Corning) to obtain a glass-bonded polarizing plate laminate 1 .

[0263] The glass-laminated polarizing plate laminate 1 was placed in a backlight source such that the glass substrate side served as a light source. The polarizing plate was visually observed in a dark place from the polyester resin film side in an oblique direction to confirm the visibility of rainbow patterns and evaluate according to the following criteria.

[0264] The pressure-sensitive adhesive layer-attached polarizing plates obtained in Example 2, Comparative Example 1, and Comparative Example 2 were evaluated for rainbow streaks in the same manner.

[0265] ◎: Very weak rainbow pattern

[0266] 0:Rainbow pattern is weak

[0267] ×: Strong rainbow pattern

[0268] <Evaluation of visibility (brightness)>

[0269] In order to reproduce the display state of the actual liquid crystal display device, the polarizing plate with an adhesive layer obtained in Comparative Example 1 was sandwiched between the glass substrate and the polarizing plate laminate 1, and the transmission axes of the two polarizing plates were parallel to each other, and the polarizing plate laminate 2 with glass was obtained. For Example 2 and Comparative Example 1, an optical laminate 2 with glass was obtained in the same manner. In addition, for Comparative Example 2, the polarizing plate with an adhesive layer obtained in Comparative Example 2 was sandwiched between the glass substrate and the transmission axes of the two polarizing plates were parallel to each other, and the polarizing plate laminate 2 with glass was obtained. For Example 1 and Example 2, the light diffusion layer was arranged on the backlight source in a manner that the light diffusion layer became the observation side, and for Comparative Example 1 and Comparative Example 2, the polyester resin film was arranged on the backlight source in a manner that the polyester resin film became the observation side. In a dark place, the polarizing plate was visually observed from the observation side of the polarizing plate and tilted from the direction orthogonal to the transmission axis of the polarizing plate to confirm visibility. The results are shown in Table 1.

[0270] 〇: High brightness and good visibility

[0271] ×: Low brightness, poor visibility

[0272] [Table 1]

[0273]

Claims

1. A polarizing plate comprising, in order, a light diffusion layer, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer and a (meth)acrylic resin film, The retardation value Re of the polyester resin film defined by the formula (1) satisfies the following [i] to [iv], Re=(n x -n y )×d (1) [i] the phase difference value Re1 measured in the first configuration, in which the polyester resin film is arranged so that the angle between the surface of the polyester resin film and the measurement direction is 90°, is 6000 nm or more; [ii] the phase difference value Re2 measured in the second configuration is 5000 nm or more, wherein the polyester resin film in the first configuration is rotated 30° about its fast axis so that the angle between the surface of the polyester resin film and the measuring direction becomes 60°, [iii] the phase difference value Re3 measured in the third configuration is 6000 nm or more, wherein the polyester resin film in the first configuration is rotated 30° around an axis forming an angle of 45° with respect to the fast axis in the plane of the polyester resin film so that the angle between the plane of the polyester resin film and the measuring direction becomes 60°, [iv] The phase difference value Re4 measured in the 4th configuration is greater than 7000nm, and in the 4th configuration, the polyester resin film in the 1st configuration is configured in such a way that the angle between the surface of the polyester resin film and the measuring direction becomes 60° by rotating the polyester resin film about its slow axis by 30°.

2. The polarizing plate according to claim 1, wherein The polyester resin film has a thickness of 60 μm or more.

3. The polarizing plate according to claim 1, wherein The ratio of the retardation value Re1 of the polyester resin film to the retardation value Rth in the thickness direction defined by the formula (2) is 0.5 or more. Rth= 〔(n x +n y ) / 2-n z 〕 ×d (2) Where n x Represents the refractive index in the slow axis direction of the film surface, n y Represents the refractive index in the fast axis direction of the film surface, n z represents the refractive index in the thickness direction of the film, and d represents the thickness of the film.

4. The polarizing plate according to claim 1, wherein The light diffusion layer has a total haze of 20% or more.

5. A polarizing plate with an adhesive layer, comprising the polarizing plate according to any one of claims 1 to 4 and an adhesive layer, The pressure-sensitive adhesive layer is laminated on the surface of the (meth)acrylic resin film opposite to the polarizer. 6 . A liquid crystal display device comprising the polarizing plate with an adhesive layer according to claim 5 .