Preparation process of array type flexible touch electronic skin
By using MXene and CNT materials, combined with material self-assembly and screen printing technology, the problems of complex preparation process and insensitive tactile perception of flexible tactile electronic skin are solved, achieving high performance and sensitive tactile sensing capabilities, simplifying the process and Reduced costs.
Patent Information
- Application Number
- CN202410986313.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
AI Technical Summary
The existing flexible tactile electronic skin has complex preparation processes, insensitive tactile perception, and poor tactile area discrimination ability, making it difficult to find a balance between high sensitivity and wide detection range.
New highly conductive two-dimensional materials MXene and CNT are used to prepare array-type flexible tactile electronic skin through material self-assembly, stenciling and screen printing, including wet chemical methods to prepare MXene single-layer dispersion, spin coating and stenciling Method to prepare a flexible substrate with randomly distributed surface microstructure, plasma treatment and screen printing to prepare patterned MXene-CNT electrodes to achieve simple fabrication and high performance.
The mechanical strength and sensing performance of the flexible tactile electronic skin are improved, the sensitive tactile sensing capability is maintained, the preparation process is simplified, the cost is reduced, it is suitable for large-scale manufacturing, and lightweight and micro-miniature design is achieved.
Smart Images

Figure CN118737567A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sensors, and in particular relates to a preparation process of an array-type flexible tactile electronic skin. Background Art
[0002] With the continuous advancement of science and technology, people's demand for high-precision tactile perception and intelligent interactive systems is increasing, which has promoted the development of the field of flexible tactile electronic skin. In these fields, flexible tactile electronic skin has great potential because they can make up for some shortcomings of traditional rigid tactile sensors, such as large size, difficulty in bending, poor portability, and low adaptability when attached to complex surfaces. Tactile electronic skin designed based on flexible materials and micro-nano structures has the advantages of high flexibility, strong stretchability, good mechanical compatibility, etc. It can achieve high-sensitivity detection of tactile signals, has excellent stability and fast response speed, and the manufacturing process is relatively simple, easy to integrate with other electronic systems.
[0003] Flexible tactile electronic skin needs to maintain high sensitivity over a wide range of pressures to meet the needs of a variety of tactile sensing applications, such as robot tactile feedback, prosthetic perception, human-machine interface, and health monitoring. However, existing flexible tactile sensors usually have difficulty finding a balance between high sensitivity and a wide detection range. They may have high sensitivity under small pressures, but their sensitivity decreases significantly over a large pressure range. This is mainly because as the pressure increases, the microstructure compression of the flexible material tends to saturation, resulting in a decrease in the signal change of the sensor per unit pressure, which rapidly reduces the sensitivity of the device. Therefore, maintaining high sensitivity within the working pressure range is of vital importance for the research and development of flexible tactile electronic skin.
[0004] In order to overcome these challenges, the research and development of flexible tactile electronic skin requires innovations in material selection, structural design, and manufacturing processes. Use materials with high conductivity and high mechanical flexibility, such as conductive polymers, nanomaterials, etc., and improve the mechanical and electrical properties of the sensor through material compounding and modification. In terms of structural design, through the innovation of multilayer structure, corrugated structure or other bionic structures, its stretchability and mechanical stability can be enhanced. In terms of manufacturing process, develop low-temperature manufacturing technology to avoid high temperature damage to flexible substrates and functional materials, and explore integration technology with microelectronic devices to realize the multifunctionality of tactile electronic skin. In addition, through surface modification and the use of biomaterials, the biocompatibility and long-term stability of the sensor can be improved, and biological rejection reactions and material degradation during use can be reduced.
[0005] In short, flexible tactile electronic skin has broad application prospects in the fields of intelligent robots, medical rehabilitation, human-computer interaction, etc. Through continuous innovation in materials, structures and processes, high-performance, low-invasive and long-term stable flexible tactile electronic skin can be developed to meet the development needs of future intelligent perception and interaction technologies. Summary of the invention
[0006] The present invention mainly aims at the shortcomings of the existing flexible tactile electronic skin, such as complex preparation process, insensitive tactile perception, and poor tactile area differentiation ability. Based on the new highly conductive two-dimensional materials MXene and CNT, and based on the microstructured flexible substrate, the flexible tactile electronic skin is sensitively responded. The flexible tactile electronic skin is simply made through material self-assembly, template method, screen printing and other methods, and the process is simplified while maintaining the performance of the flexible tactile electronic skin.
[0007] The technical solution adopted by the present invention is a preparation process of an array-type flexible tactile electronic skin, comprising the following steps: Step 1: Prepare MXene monolayer dispersion using LiF and Ti3AlC2 by wet chemical method, and prepare MXene-CNT mixed slurry by self-dispersion; Step 2, preparing a flexible substrate with randomly distributed surface microstructures by spin coating and template method; Step 3, treating the flexible substrate with randomly distributed surface microstructures by plasma treatment; Step 4, preparing a patterned MXene-CNT electrode by screen printing; Step 5: Clean the MXene-CNT electrode obtained in the above step, laminate it vertically in the order of packaging layer - nanosilver conductive film - MXene-CNT electrode - flexible substrate packaging layer, and lead out the wires.
[0008] Furthermore, the preparation method of the MXene-CNT mixed slurry is specifically as follows: 1) The MAX-Ti3AlC2 material is treated by an in-situ etching method. HF is generated by the in-situ reaction of LiF and HCl, and then MAX-Ti3AlC2 is etched to remove the Al element between its layers, thereby forming layered stacked MXene-Ti3C2Tx particles; 2) Disperse the obtained MXene-Ti3C2Tx material into the form of two-dimensional nanosheets through ultrasonic treatment. The application of ultrasound helps to disperse the MXene material into uniform nanosheets, improving its dispersibility and stability in subsequent applications; 3) Then, the ultrasonically treated MXene-Ti3C2Tx nanosheets were mixed with CNT particles in a polar solvent. The addition of CNTs can further enhance the conductivity and mechanical properties of the MXene material. The mixture was stirred for 3 hours to fully disperse the MXene material and allow for self-adsorption. The solvent was concentrated by high-speed centrifugation to form a MXene-CNT slurry.
[0009] Furthermore, the choice of polar solvent is crucial to the formation and stability of MXene-CNT slurry, which can ensure the uniformity and operability of the slurry. Chloroform or tetrahydrofuran can be used.
[0010] Furthermore, the method for preparing the flexible substrate with randomly distributed surface microstructures is specifically as follows: 1) Mix the PDMS prepolymer and curing agent in a mass ratio of 10:1, stir continuously for 10 minutes to ensure uniform mixing, and then use a vacuum below 10Pa to remove the bubbles in the PDMS; 2) Place the template with a hole structure on a flat spin coater stage and spin coat PDMS at 100 rpm; 3) Curing on a hot plate at 100°C for 2 hours to allow the flexible substrate to be cured with a random distribution of surface microstructures.
[0011] Furthermore, the method for preparing the flexible substrate with randomly distributed surface microstructures after plasma treatment is specifically as follows: High-pressure ionized argon / oxygen is used to form plasma to impact a flexible substrate with randomly distributed surface microstructures, thereby increasing the surface roughness of the flexible substrate and reducing the surface energy, thereby improving the wettability of the PDMS surface.
[0012] Furthermore, the method for preparing the patterned MXene-CNT electrode by screen printing is specifically as follows: 1) Process the desired electrode pattern on the surface of the stainless steel mesh so that the pattern is partially hollowed out; 2) The stainless steel mesh is pressed against the surface of the flexible substrate with randomly distributed surface microstructures, and a certain pressure is applied to fix it; 3) Apply the obtained MXene-CNT slurry on the hollow pattern part of the stainless steel mesh, and use a scraper to apply the MXene-CNT slurry at a 45° angle at a uniform speed to fill the hollow pattern part of the stainless steel mesh; 4) Remove the stainless steel mesh vertically and cure the MXene-CNT electrode in a vacuum drying oven at 60 °C.
[0013] Furthermore, the thickness of the stainless steel mesh is 0.5 mm.
[0014] Furthermore, the laminating pressure of the stainless steel mesh is 10 kPa to prevent the stainless steel mesh from shaking during the coating process.
[0015] Furthermore, the flexible tactile electronic skin packaging method is specifically as follows: 1) Cleaning the MXene-CNT@PDMS and nanosilver conductive film obtained above by oxygen plasma in an oxygen plasma cleaning machine to remove surface impurities; 2) Use high conductivity cables to connect to the MXene-CNT electrodes through conductive silver paste, and lead out cables to connect to external circuits; 3) Vertical plane bonding is carried out in the order of encapsulation layer - nanosilver conductive film - MXene-CNT electrode - flexible substrate encapsulation layer.
[0016] Furthermore, the encapsulation layer is a flexible film such as polyimide (PI), polyethylene terephthalate (PET), polydimethylsiloxane (PDMS), etc.
[0017] The purpose of the present invention is to solve the technical problems of complex preparation process of existing flexible tactile electronic skin, insensitive tactile perception, and poor ability to distinguish tactile areas, and to provide a preparation process of array-type flexible tactile electronic skin.
[0018] Compared with the existing achievements, the beneficial effects of the present invention are: 1) The present invention has a simple sensing structure and high stability and reliability through structural innovation. It uses a variety of excellent performance materials such as MXene, CNT, PDMS, etc. to improve the mechanical strength and sensing performance of the flexible tactile electronic skin; 2) At the same time, the randomly distributed sensing structure of the flexible tactile electronic skin microstructure of the present invention can also maintain the sensitive tactile sensing ability of the flexible tactile electronic skin to meet the design requirements of the electronic skin; 4) The use of material self-assembly, template method, screen printing and other processes has achieved the optimization of the preparation process and improved the utilization rate of materials. It has low processing technology requirements and low cost, and is suitable for large-scale manufacturing; 5) The structure is designed in vertical stacking style to achieve the purpose of lightweight and miniaturization.
[0019] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The following is a schematic diagram of the overall structure of the array-type flexible tactile electronic skin of the present invention; Figure 2 : A schematic diagram of the manufacturing process of a flexible substrate with randomly distributed array-type flexible tactile electronic skin microstructures according to the present invention; Figure 3: A schematic diagram of the screen printing process of the array-type flexible tactile electronic skin of the present invention; Figure 4 : A schematic diagram of the current response of the array-type flexible tactile electronic skin press test of the present invention; Figure 5 Schematic diagram of the array-type flexible tactile electronic skin of the present invention attached to a human arm and the current response of a grasping test.
[0021] In the figure: 1-encapsulation layer, 2-nanosilver film, 3-MXene-CNT electrode, 4-flexible substrate, 5-encapsulation layer, 6-microstructure template, 7-stainless steel mesh. DETAILED DESCRIPTION
[0022] The present invention is further explained below in conjunction with the accompanying drawings and embodiments to facilitate understanding by those skilled in the art.
[0023] like Figure 1 As shown, the array-type flexible tactile electronic skin of the present invention is composed of a five-layer structure vertically packaged, which includes a packaging layer 1, a nanosilver film 2, a MXene-CNT electrode 3, a flexible substrate 4 and a packaging layer 5 from top to bottom.
[0024] After the array-type flexible tactile electronic skin is encapsulated, the micro-spine-like protrusions of the flexible substrate of the array-type flexible tactile electronic skin contact the nanosilver film to form a conductive path, which constitutes a primary signal response. When pressure is applied to the structure, the stress on the flexible substrate further causes the microstructure of the MXene-CNT electrode to contact the nanosilver film, and the original micro-spine-like protrusions will further contact, the contact area will expand, and the resistance will decrease under the piezoresistive effect. At the same time, the partially stacked MXene-CNT will further contact, and the overall performance is a high-sensitivity response under pressure. After the load is removed, the deformed structure supported by the PDMS substrate can recover quickly, which improves the overall signal response and force stability of the flexible tactile electronic skin system.
[0025] The following describes the preparation process of the array-type flexible tactile electronic skin of the present invention. Figure 2-3 As shown, the following steps are included: Step 1: Prepare a MXene monolayer dispersion using LiF and Ti3AlC2 by wet chemical method, and prepare a MXene-CNT mixed slurry by self-dispersion: Use an in-situ etching method to treat the MAX-Ti3AlC2 material, generate HF by the in-situ reaction of LiF and HCl, and then etch the MAX-Ti3AlC2 to remove the Al element between its layers, thereby forming layered stacked MXene-Ti3C2Tx particles. Through ultrasonic treatment, the obtained MXene-Ti3C2Tx material is dispersed into the form of two-dimensional nanosheets. The application of ultrasound helps to disperse the MXene material into uniform nanosheets, improving its dispersibility and stability in subsequent applications. Then, the ultrasonically treated MXene-Ti3C2Tx nanosheets are mixed with CNT particles in a polar solvent. The addition of CNT can further enhance the conductivity and mechanical properties of the MXene material. Stirring is continued for 3 hours to fully disperse it and self-adsorb it. The solvent is concentrated by high-speed centrifugation to form a MXene-CNT slurry.
[0026] Furthermore, the choice of polar solvent is crucial to the formation and stability of MXene-CNT slurry, which can ensure the uniformity and operability of the slurry. Chloroform or tetrahydrofuran can be used.
[0027] Step 2, such as Figure 2 As shown, a flexible substrate with randomly distributed surface microstructures is prepared by spin coating and template method: the PDMS prepolymer and curing agent are mixed at a mass ratio of 10:1, and stirred for 10 minutes to ensure uniform mixing, and then the bubbles of the PDMS are removed by vacuum below 10Pa. The template 6 with a hole structure is placed on a flat spin coater stage, and the PDMS is spin coated at a speed of 100 rpm; it is cured on a hot plate at 100°C for 2 hours to solidify the flexible substrate 4 with randomly distributed surface microstructures.
[0028] Step three, such as Figure 2 As shown, a flexible substrate with randomly distributed surface microstructures is treated by plasma: high-voltage ionized argon / oxygen is used to form plasma to impact the flexible substrate with randomly distributed surface microstructures, so that the surface roughness of the flexible substrate is increased and the surface energy is reduced, thereby improving the wettability of the PDMS surface.
[0029] Step 4: Figure 3As shown, a patterned MXene-CNT electrode is prepared by a screen printing process: the desired electrode pattern is processed on the surface of a stainless steel mesh so that the pattern part is hollowed out; the stainless steel mesh is pressed against the surface of a flexible substrate with randomly distributed surface microstructures, and a certain pressure is applied to fix it; the obtained MXene-CNT slurry is applied on the hollowed-out pattern part of the stainless steel mesh, and a scraper is used to scrape the MXene-CNT slurry at a uniform and stable speed at a 45° angle so that it fills the hollowed-out pattern part of the stainless steel mesh; the stainless steel mesh is removed vertically, and the MXene-CNT electrode is cured in a vacuum drying oven at 60°C.
[0030] Furthermore, the thickness of the stainless steel mesh is 0.5 mm, and the laminating pressure of the stainless steel mesh is 10 kPa to prevent the stainless steel mesh from shaking during the coating process.
[0031] Step 5: Clean the MXene-CNT@PDMS and nanosilver conductive film 2 obtained above with oxygen plasma in an oxygen plasma cleaning machine to remove surface impurities. Use a high conductivity cable to connect to the MXene-CNT3 electrode through a conductive silver paste, and lead out the cable to connect to an external circuit; follow the order of encapsulation layer 1-nanosilver conductive film 2-MXene-CNT electrode 3-flexible substrate 4-encapsulation layer 5, and laminate vertically.
[0032] Furthermore, the encapsulation layer is a flexible film such as polyimide (PI), polyethylene terephthalate (PET), polydimethylsiloxane (PDMS), etc.
[0033] Further, the flexible tactile electronic skin was tested, such as Figure 4 As shown, it can clearly detect and record the intensity and time interval of the pressing pressure.
[0034] Further, the flexible tactile electronic skin was tested, such as Figure 5 As shown, attaching it to the surface of a human arm can achieve good adhesion and sense the grip pressure of the palm.
[0035] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. The technical solution adopted by the present invention is a preparation process of an array-type flexible tactile electronic skin, characterized in that: The following steps are involved: Step 1: Prepare MXene monolayer dispersion using LiF and Ti3AlC2 by wet chemical method, and prepare MXene-CNT mixed slurry by self-dispersion; Step 2, preparing a flexible substrate with randomly distributed surface microstructures by spin coating and template method; Step 3, treating the flexible substrate with randomly distributed surface microstructures by plasma treatment; Step 4, preparing a patterned MXene-CNT electrode by screen printing; Step 5: Clean the MXene-CNT electrode obtained in the above step, laminate it vertically in the order of packaging layer - nanosilver conductive film - MXene-CNT electrode - flexible substrate packaging layer, and lead out the wires.
2. The preparation process of the array-type flexible tactile electronic skin according to claim 1, characterized in that: The preparation method of the MXene-CNT mixed slurry is specifically as follows: an in-situ etching method is adopted, LiF and HCl are used to in-situ form HF to etch MAX-Ti3AlC2, Al between MAX-Ti3AlC2 layers is removed to form MXene-Ti3C2Tx, two-dimensional nanosheets are obtained by ultrasound, and CNTs are mixed in a polar solvent to form a MXene-CNT slurry.
3. The preparation process of the array-type flexible tactile electronic skin according to claim 1, characterized in that: The method for preparing the flexible substrate with randomly distributed surface microstructures is specifically as follows: mixing a curing agent and a prepolymer of PDMS, spin coating the mixture on the surface of a prefabricated template of a microstructure, and obtaining the flexible substrate with randomly distributed surface microstructures after curing.
4. The preparation process of the array-type flexible tactile electronic skin according to claim 1, characterized in that: The method for preparing the flexible substrate with randomly distributed surface microstructures by plasma treatment is specifically: using high-pressure ionized argon / oxygen to form plasma to impact the flexible substrate with randomly distributed surface microstructures to perform surface treatment.
5. The preparation process of the array-type flexible tactile electronic skin according to claim 1, characterized in that: The method for preparing the patterned MXene-CNT electrode by screen printing is specifically as follows: attaching a prefabricated patterned stainless steel mesh to a flexible substrate, coating the MXene-CNT slurry on the surface thereof by screen printing, and vacuum drying and curing the MXene-CNT electrode.
6. The preparation process of the array-type flexible tactile electronic skin according to claim 1, characterized in that: The packaging method specifically comprises: cleaning the components obtained above, laminating them vertically in the order of packaging layer - nanosilver conductive film - MXene-CNT electrode - flexible substrate packaging layer, and leading out the wires.