Graphene aluminum alloy conductive wire and hot melting preparation method thereof
By using atomized spraying and high-temperature melting treatment of graphene carbon nanotube dispersion and pure aluminum powder in conductive wires, the existing problem of low conductivity is solved and high-conductivity of high-purity graphene aluminum alloy conductive wires is achieved efficiency and wear resistance, broadening the scope of applications.
Patent Information
- Application Number
- CN202411047606.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-11
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing rare earth graphene aluminum alloy conductive wires have low conductivity, complex processes and high costs, making them unsuitable for large-scale industrial applications.
The graphene carbon nanotube dispersion and pure aluminum powder are atomized and sprayed under a fluorine-containing inert gas atmosphere, deposited layer by layer to form a graphene aluminum alloy master ingot, and then melted, solid solution treated and extruded at high temperatures to form High purity graphene aluminum alloy conductive wire.
Significantly improves the electrical conductivity of graphene aluminum alloy to 66.2% IACS, enhances fatigue performance and wear resistance, and is suitable for fields such as data centers and aerospace.
Smart Images

Figure CN118737569A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of conductive wire preparation, and in particular relates to a graphene aluminum alloy conductive wire and a hot-melt preparation method thereof. Background Art
[0002] Conductive wire is the main raw material for preparing cables, wires, enameled wires, conductor profiles, connection and conversion terminals and other materials. With the rapid development of the electric power industry, infrastructure construction, and household appliances in recent years, the demand and application of conductive wire has become more and more extensive, and the demand for conductive wire has increased and higher requirements have been put forward.
[0003] At present, most of the conductive wires in the industry are made of copper conductive wires, and a few are made of ordinary aluminum alloy or pure aluminum conductive wires. Due to the scarcity of copper resources, the industrial development of copper conductive wires is limited. It is urgent to develop other materials to prepare conductive wires. However, the conductivity of ordinary aluminum alloy or pure aluminum conductive wires currently developed is not as good as that of copper. Graphene aluminum alloys are prone to agglomeration, which affects the effective role of graphene's conductive properties.
[0004] Patent CN103943281A discloses a method for preparing wires and cables with copper-graphene composite conductive cores. This method uses electroplating and then stretching into wires, uses a large amount of chemical reagents such as sulfuric acid and hydrochloric acid, and has many processing steps and a small preparation amount, making it difficult to achieve industrial production.
[0005] Patent CN106636776A discloses a rare earth graphene aluminum alloy conductive wire and a preparation method. The method adopts low-temperature ball milling powder metallurgy to prepare rare earth graphene aluminum alloy. Although it can achieve uniform dispersion of graphene in aluminum and improvement of the graphene / aluminum interface bonding, the method is complex and costly, and is not suitable for large-scale engineering applications in low value-added fields (such as electrical appliances, cables, etc.). Summary of the invention
[0006] The technical problem to be solved by the present invention is that the conductivity of rare earth graphene aluminum alloy conductive wires prepared by existing methods is not high.
[0007] The technical solution of the present invention to solve the above technical problems is: to provide a method for hot-melt preparation of graphene aluminum alloy conductive wire. The method comprises the following steps:
[0008] a. Preparation of graphene carbon nanotube dispersion
[0009] The graphene powder and the carbon nanotube slurry are mixed in a weight ratio of 1 to 3:1, dispersed in alcohol, and ultrasonically stirred to obtain a graphene carbon nanotube dispersion;
[0010] b. Preparation of graphene aluminum alloy master ingot
[0011] The pure aluminum powder and the graphene carbon nanotube dispersion obtained in step a are mixed in a weight ratio of 3 to 5:1, atomized in a fluorine-containing inert gas atmosphere, sprayed on a substrate at 100 to 200° C., and after spraying a layer evenly, compacted with a roller at 20 to 80° C., and the gas containing fluorine and alcohol is recovered; the spraying is repeated, and the graphene aluminum alloy mother ingot is deposited layer by layer;
[0012] c. Graphene aluminum alloy melting
[0013] The graphene aluminum alloy mother ingot is placed in a pure aluminum alloy melt at 700-760°C, fluorine is added in a high-pressure protective nitrogen atmosphere, and stirred for 40-50 minutes. After stirring, the mother ingot is allowed to stand at 660-680°C, and then cast into a graphene aluminum alloy ingot;
[0014] d. Post-processing of graphene aluminum alloy ingot
[0015] The graphene aluminum alloy ingot is solution treated at a temperature of 450 to 550° C. for 3 to 6 hours;
[0016] e. Aluminum rod extrusion and post-processing
[0017] The graphene aluminum alloy ingot after solution treatment is extruded at 380-420° C. to obtain an aluminum rod with a diameter of 9-10 mm, and an aging treatment is performed at a temperature of 210-350° C. for 4-6 hours to obtain a graphene aluminum alloy conductive wire.
[0018] Among them, in the above-mentioned hot-melt preparation method of graphene aluminum alloy conductive wire, the graphene powder described in step a is a graphene powder with a carbon content of 98 to 99 wt%.
[0019] Furthermore, the graphene is one of single-layer graphene, double-layer graphene or multi-layer graphene.
[0020] Among them, in the hot-melt preparation method of the above-mentioned graphene aluminum alloy conductive wire, the carbon nanotube slurry described in step a is a carbon nanotube slurry with a carbon content of ≥98%, an impurity content of 0.1-0.9%, and an alcohol solvent.
[0021] Furthermore, the carbon nanotube slurry has a specific surface area of 160 to 230 m 2 / g, tube diameter 10~25nm, tube length 10~30μm, density 0.1~0.2g / cm 3 .
[0022] Among them, in the hot-melt preparation method of the above-mentioned graphene aluminum alloy conductive wire, the weight ratio of the total amount of graphene powder and carbon nanotube slurry described in step a to alcohol is 1:98-99.
[0023] Among them, in the hot-melt preparation method of the above-mentioned graphene aluminum alloy conductive wire, the speed of the ultrasonic stirring described in step a is 25 to 50 r / min, and the ultrasonic stirring time is 30 to 60 min.
[0024] Among them, in the hot-melt preparation method of the above-mentioned graphene aluminum alloy conductive wire, the iron content in the final aluminum alloy ingot is 0.05-0.5wt%, the carbon content is 0.1-0.5wt%, the copper content is 0.02-0.25wt%, the silicon content is 0.005-0.25wt%, and the balance is aluminum.
[0025] Among them, in the above-mentioned hot-melt preparation method of graphene aluminum alloy conductive wire, the substrate described in step b is an aluminum alloy substrate.
[0026] Among them, in the hot melt preparation method of the above-mentioned graphene aluminum alloy conductive wire, the solution treatment described in step d has a heating rate of 15°C / min when the temperature is between 20 and 350°C; and a heating rate of 10°C / min when the temperature is above 350°C.
[0027] Among them, in the hot-melt preparation method of the above-mentioned graphene aluminum alloy conductive wire, when extruding the aluminum rod in step e, the extrusion speed is 2 to 2.2 mm / s, and the extrusion force is 250 to 300 kN.
[0028] The present invention also provides a graphene aluminum alloy conductive wire prepared by the above method.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention provides a hot-melt preparation method for a graphene aluminum alloy conductive wire, which adopts high-purity graphene powder and carbon nanotube slurry, prepares the graphene powder and the carbon nanotube slurry into a dispersion liquid, and then atomizes and sprays the dispersion liquid onto a substrate. The dispersion effect of graphene and carbon nanotubes in the aluminum alloy is improved, and the conductivity of the graphene aluminum alloy is significantly improved. The conductivity can be increased to 66.2% IACS, and the wire can be widely used in data centers, aerospace and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Shown is a TEM image of a graphene aluminum alloy conductive wire prepared by the method of the present invention;
[0032] Figure 2 Shown is a TEM image of graphene aluminum alloy conductive wire produced by the existing melt addition method. DETAILED DESCRIPTION
[0033] The invention adopts high-purity graphene powder and carbon nanotube slurry. The C content of the graphene powder is 98-99%, and the carbon content of the carbon nanotube slurry is ≥98%. Both contain less impurities, thereby improving the conductivity of the material.
[0034] At the same time, the present invention adopts a method of adding alcohol for dispersion when dispersing graphene and carbon nanotubes. The alcohol can volatilize in the subsequent processing steps. The volatilized alcohol forms a physical barrier, which can reduce the risk of oxidation.
[0035] At the same time, the present invention adopts a method of atomizing aluminum powder and graphene and carbon nanotube dispersion in a fluorine-containing atmosphere and spraying the dispersion on a substrate to prepare the graphene aluminum alloy conductive wire. By spraying and compacting layer by layer, the graphene and carbon nanotubes are prepared into a slurry, which is not easy to agglomerate compared to powders and can be dispersed more evenly, which can further improve the conductivity of the graphene aluminum alloy conductive wire.
[0036] The present invention adopts a fluorine-containing nitrogen atmosphere, which can generate nano fluoride AlF3 and nitride AIN with component elements, thereby improving the fatigue performance and wear resistance of the graphene aluminum alloy conductive wire.
[0037] The conductivity of the graphene aluminum alloy conductive wire obtained by the present invention reaches 66.2% IACS, which is 5.2% IACS higher than that of electrical aluminum.
[0038] Traditional graphene aluminum alloys are prepared by melting. Graphene directly contacts the high-temperature aluminum alloy melt, which may cause burning. In addition, graphene has a low specific gravity and can only be dispersed in the alloy grains to play a role in pinning dislocations and subgrain boundaries. Therefore, the main function of adding graphene in traditional methods is to increase the hardness of the alloy, and there is a lack of research on increasing the conductivity of graphene. In addition, in traditional methods, graphene exists in a dispersed manner. The dispersed graphene may become a particle that scatters electrons, which will reduce the conductivity of the alloy to a certain extent.
[0039] The present invention adopts a special adding method, limits the appropriate ratio of graphene powder, carbon nanotube slurry and aluminum powder, promotes the formation of an amorphous bonding surface through high-temperature sintering, and the graphene + carbon nanotubes overlap inside the alloy to form a second conductive phase. Ultimately, the conductivity of the alloy not only exceeds the 61% IACS of pure aluminum, but also increases by 5.2%, achieving a very significant improvement.
[0040] The specific implementation modes of the present invention will be further explained below in conjunction with examples, but it does not mean that the protection scope of the present invention is limited to the scope described in the examples.
[0041] The graphene used in the embodiment has a composition of 98.3% carbon content, 1.5% sulfur content, and 0.2% other impurities.
[0042] The carbon nanotubes used in the embodiment have the following composition: C content ≥ 99.5%, Co ≤ 650 ppm, Fe ≤ 100 ppm, Cr ≤ 20 ppm, Zn ≤ 20 ppm, Ni ≤ 10 ppm, and Cu ≤ 10 ppm.
[0043] Example 1 Preparation of graphene aluminum alloy conductive wire using the method of the present invention
[0044] The specific experimental steps are as follows:
[0045] a. Preparation of graphene carbon nanotube dispersion
[0046] Weigh 4 g of graphene and 2 g of carbon nanotubes, mix them, add them into 730 ml of alcohol, and stir them ultrasonically at a speed of 50 r / min for 30 min to obtain a graphene carbon nanotube dispersion;
[0047] b. Graphene aluminum alloy master ingot
[0048] Weigh 3000g of pure aluminum powder, mix the pure aluminum powder and graphene carbon nanotube dispersion, atomize in a fluorine-containing inert gas atmosphere, spray on a substrate at 150°C, evenly spray a layer, and then use an 80°C roller to compact, and recover the fluorine and alcohol-containing gas; repeat the spraying, and deposit layer by layer to form a graphene aluminum alloy mother ingot;
[0049] c. Graphene aluminum alloy melting
[0050] The aluminum alloy mother ingot is placed in a 720°C pure aluminum alloy melt, stirred for 1 hour in a high-pressure nitrogen protective atmosphere, and then allowed to stand at 680°C after the stirring, and cast into an aluminum ingot;
[0051] d. Post-processing of aluminum ingots
[0052] The graphene aluminum alloy ingot was solution treated at 550 °C for 4 h, heated to 350 °C at a rate of 15 °C / min, and then heated to 550 °C at a rate of 10 °C / min;
[0053] e. Aluminum rod extrusion and aging treatment
[0054] The graphene aluminum alloy after solution treatment was extruded into an aluminum rod with a diameter of 9.5 mm at 400°C, an extrusion speed of 2.2 mm / s, an extrusion force of 300 kN, and an aging treatment was performed at 230°C for 6 hours to obtain a graphene aluminum alloy conductive wire.
[0055] Example 2 Preparation of graphene aluminum alloy conductive wire using the method of the present invention
[0056] The specific experimental steps are as follows:
[0057] a. Preparation of graphene carbon nanotube dispersion
[0058] Weigh 6 g of graphene and 2 g of carbon nanotubes, mix them, add them into 730 ml of alcohol, and stir them ultrasonically at a speed of 50 r / min for 30 min to obtain a graphene carbon nanotube dispersion;
[0059] b. Graphene aluminum alloy master ingot
[0060] Weigh 3000g of pure aluminum powder, mix the pure aluminum powder and graphene carbon nanotube dispersion, atomize in a fluorine-containing inert gas atmosphere, spray on a substrate at 100°C, evenly spray a layer, and then use an 80°C roller to compact, and recover the fluorine and alcohol-containing gas; repeat the spraying, and deposit layer by layer to form a graphene aluminum alloy mother ingot;
[0061] c. Graphene aluminum alloy melting
[0062] The aluminum alloy mother ingot is placed in a 760°C pure aluminum alloy melt, stirred for 1 hour in a high-pressure nitrogen protective atmosphere, and then allowed to stand at 680°C after the stirring, and cast into an aluminum ingot;
[0063] d. Post-processing of aluminum ingots
[0064] The graphene aluminum alloy ingot was solution treated by heating to 350°C at a rate of 15°C / min, then to 530°C at a rate of 10°C / min, and kept at this temperature for 5h;
[0065] e. Aluminum rod extrusion and aging treatment
[0066] The graphene aluminum alloy after solution treatment was extruded into an aluminum rod with a diameter of 9.5 mm at 400°C, an extrusion speed of 2 mm / s, an extrusion force of 250 kN, and an aging treatment was performed at a temperature of 230°C and a holding time of 6 h to obtain a graphene aluminum alloy conductive wire.
[0067] The specific experimental steps are as follows:
[0068] a. Preparation of graphene dispersion
[0069] Weigh 8 g of graphene and 0 g of carbon nanotubes, mix them, add them into 800 ml of alcohol, and stir them ultrasonically at a speed of 40 r / min for 30 min to obtain a graphene dispersion;
[0070] b. Graphene aluminum alloy master ingot
[0071] Weigh 3000g of pure aluminum powder, mix the pure aluminum powder and graphene dispersion, atomize in an atmosphere of F-containing inert gas, spray on a substrate at 150°C, evenly spray a layer, compact with a 50°C roller, and recover the gas containing F and alcohol; repeat the spraying, and deposit layer by layer to form a graphene aluminum alloy mother ingot;
[0072] c. Graphene aluminum alloy melting
[0073] The aluminum alloy mother ingot is placed in a 720°C pure aluminum alloy melt, stirred for 1 hour in a high-pressure nitrogen protective atmosphere, and then allowed to stand at 680°C after the stirring, and cast into an aluminum ingot;
[0074] d. Post-processing of aluminum ingots
[0075] The graphene aluminum alloy ingot was solution treated by heating to 350°C at a rate of 15°C / min, then to 530°C at a rate of 10°C / min, and kept at this temperature for 5h;
[0076] e. Aluminum rod extrusion and aging treatment
[0077] The graphene aluminum alloy after solution treatment was extruded into an aluminum rod with a diameter of 9.5 mm at 400°C, an extrusion speed of 2 mm / s, an extrusion force of 250 kN, and an aging treatment was performed at a temperature of 230°C and a holding time of 6 h to obtain a graphene aluminum alloy conductive wire.
[0078] The difference from Example 1 is:
[0079] The graphene and carbon nanotubes are not of high purity. The graphene has a carbon content of 80% and an impurity content of 15%, and the carbon nanotubes have a carbon content of 85% and an impurity content of 10%.
[0080] Comparative Example 3: Preparation of graphene aluminum alloy conductive wire without using the method of the present invention
[0081] The difference from Example 1 is that: in step a, 40 g of graphene and 10 g of carbon nanotubes are used, and in step b, 1950 g of pure aluminum powder is used. The ratio of graphene to aluminum powder is more than 2%.
[0082] Comparative Example 4: Preparation of graphene aluminum alloy conductive wire without using the method of the present invention
[0083] The difference from Example 1 is that the atomization and spraying methods are not adopted, but the melt adding method is adopted.
[0084] The specific steps are as follows:
[0085] Under the protection of inert gas, graphene was blown into the aluminum alloy melt with nitrogen, and then cast into aluminum ingots after electromagnetic stirring for 30 minutes. After cooling to 400°C, aluminum alloy wires with a diameter of 9-10 mm were extruded.
[0086] The TEM image of the graphene aluminum alloy conductive wire prepared in this embodiment is as follows: Figure 2 As shown. Figure 2 It can be seen that no graphene was observed in the prepared graphene aluminum alloy.
[0087] Comparative Example 5: Preparation of graphene aluminum alloy conductive wire without using the method of the present invention
[0088] The difference from Example 1 is that no F-containing inert gas is added.
[0089] The conductivity, elongation and fatigue limit tests of the graphene aluminum alloy conductive wires obtained in the embodiments and comparative examples were carried out. The test methods adopted were the methods in GB / T351-2019, GB / T10120-2013 and GB / T15248-2008, respectively. The results are shown in Table 1 below.
[0090] Table 1 Performance of graphene aluminum alloy conductive wires prepared by different methods
[0091] Electrical conductivity (%IACS) Elongation(%) Fatigue limit(MPa) Example 1 66.2 27.4 88 Example 2 65.8 28 89 Comparative Example 1 65.5 30 91 Comparative Example 2 52 21 77 Comparative Example 3 61.7 30 78 Comparative Example 4 60.2 40 92 Comparative Example 5 62.8 28 62
[0092] It can be seen from the embodiments and comparative examples that the method of the present invention can overlap with each other to form a second conductive phase, thereby improving the conductivity of the alloy. The graphene aluminum alloy conductive wire prepared by the present invention reaches 66.2% IACS, which greatly broadens the application scope of the graphene aluminum alloy conductive wire and has a good application prospect.
Claims
1. A method for preparing graphene aluminum alloy conductive wire by hot melting, characterized in that: The following steps are involved: a. Preparation of graphene carbon nanotube dispersion The graphene powder and the carbon nanotube slurry are mixed in a weight ratio of 1 to 3:1, dispersed in alcohol, and ultrasonically stirred to obtain a graphene carbon nanotube dispersion; b. Preparation of graphene aluminum alloy master ingot The pure aluminum powder and the graphene carbon nanotube dispersion obtained in step a are mixed in a weight ratio of 3 to 5:1, atomized in a fluorine-containing inert gas atmosphere, sprayed on a substrate at 100 to 200° C., and after spraying a layer evenly, compacted with a 20 to 80° C. roller, and the fluorine- and alcohol-containing gas is recovered; the spraying is repeated, and the graphene aluminum alloy mother ingot is deposited layer by layer; c. Graphene aluminum alloy melting The graphene aluminum alloy mother ingot is placed in a pure aluminum alloy melt at 700-760°C, fluorine is added in a high-pressure protective nitrogen atmosphere, stirred for 40-50 minutes, and after stirring, allowed to stand at 660-680°C, and cast into a graphene aluminum alloy ingot; d. Post-processing of graphene aluminum alloy ingot The graphene aluminum alloy ingot is solution treated at a temperature of 450 to 550° C. for 3 to 6 hours; e. Aluminum rod extrusion and post-processing The graphene aluminum alloy ingot after solution treatment is extruded at 380-420°C to obtain an aluminum rod with a diameter of 9-10 mm, and then subjected to aging treatment at a temperature of 210-350°C for 4-6 hours to obtain a graphene aluminum alloy conductive wire.
2. The hot-melt preparation method of the graphene aluminum alloy conductive wire according to claim 1, characterized in that: The graphene powder described in step a is a graphene powder with a carbon content of 98 to 99 wt%.
3. The hot-melt preparation method of the graphene aluminum alloy conductive wire according to claim 1, characterized in that: The carbon nanotube slurry described in step a has a carbon content of ≥98%, an impurity content of 0.1-0.9%, and an alcohol solvent.
4. The hot-melt preparation method of the graphene aluminum alloy conductive wire according to claim 3, characterized in that: The specific surface area of the carbon nanotube slurry is 160-230m 2 / g, tube diameter 10~25nm, tube length 10~30μm, density 0.1~0.2g / cm 3 .
5. The hot-melt preparation method of graphene aluminum alloy conductive wire according to claim 1, characterized in that: The weight ratio of the total amount of graphene powder and carbon nanotube slurry to alcohol described in step a is 1:98-99.
6. The hot-melt preparation method of graphene aluminum alloy conductive wire according to claim 1, characterized in that: The speed of the ultrasonic stirring in step a is 25 to 50 r / min, and the ultrasonic stirring time is 30 to 60 min.
7. The hot-melt preparation method of graphene aluminum alloy conductive wire according to claim 1, characterized in that: The substrate described in step b is an aluminum alloy substrate.
8. The hot-melt preparation method of graphene aluminum alloy conductive wire according to claim 1, characterized in that: In the solution treatment described in step d, the heating rate is 15°C / min when the temperature is between 20°C and 350°C; and the heating rate is 10°C / min when the temperature is above 350°C.
9. The hot-melt preparation method of graphene aluminum alloy conductive wire according to claim 1, characterized in that: In step e, when extruding the aluminum rod, the extrusion speed is 2-2.2 mm / s and the extrusion force is 250-300 kN.
10. The graphene aluminum alloy conductive wire prepared by the hot-melt preparation method of the graphene aluminum alloy conductive wire according to any one of claims 1 to 9.
Citation Information
Patent Citations
Graphene and carbon nanotube mixed enhanced metal-matrix composite material and preparation method thereof
CN102719693A
High-conductivity heat-resistance aluminum alloy wire and preparation method thereof
CN104831127A
High-conductivity high-strength rare earth aluminum alloy composite material for splicing fitting and preparation method thereof
CN114703408A
High-conductivity graphene aluminum alloy rod, preparation method thereof and high-conductivity graphene aluminum alloy stranded wire
CN115466883A
Method for preparing graphene-reinforced aluminum matrix composite material powder by means of short flow
WO2021232942A1