Preparation method of nano-silver transparent conductive film

By combining ultraviolet irradiation and hot air drying technology, rapid curing and drying of nano-silver transparent conductive films is achieved, which solves the problems of long curing time and high cost in the existing technology, and improves conductivity and preparation efficiency.

CN118737571APending Publication Date: 2024-10-01TIANJIN BAOXINGWEI TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075267.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the curing and drying process of the existing nano-silver transparent conductive film, the ultraviolet light curing efficiency is low, resulting in a long curing time, and two sets of curing and drying equipment are required, which increases production costs and preparation time.

Method used

Rapid curing and drying is carried out by combining ultraviolet irradiation from a light-curing lamp and hot air from the drying head. Simultaneous curing and drying of the substrates on both sides is achieved by rotating the mounting base. The coating pause time is used for timely curing, reducing production costs and preparation time.

Benefits of technology

The conductivity and stability of nanosilver particles are improved, the preparation time is shortened, the production cost is reduced, and the preparation efficiency and stability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737571A_ABST
    Figure CN118737571A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a nano-silver transparent conductive film and relates to the field of preparation of nano-silver transparent conductive films, in particular to preparation equipment of the nano-silver transparent conductive film in the preparation process of the nano-silver transparent conductive film, and the preparation equipment comprises a conveying table composed of a left conveying face, a right conveying face and a fixing part. A portal frame is erected at the upper ends of the left and right fixed parts of the conveying table, and a curing and drying unit is arranged below the horizontal section of the portal frame. One curing and drying unit is used for rapidly completing curing and drying of the coated substrates on the two production lines, the production cost is effectively reduced, meanwhile, the coated substrates are timely cured and dried according to the coating pause time, the coated substrates do not need to be independently cured and dried, and the production efficiency is improved. And the preparation time of the nano-silver transparent conductive film is effectively shortened, so that the preparation efficiency of the nano-silver transparent conductive film is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of nano silver transparent conductive films, in particular to a method for preparing nano silver transparent conductive films. Background Art

[0002] Nanosilver transparent conductive film is a thin film composed of nano-scale silver particles, which has good transparency and conductivity. It is usually used in various electronic products such as liquid crystal displays, touch screens, solar cells, etc. to provide conductivity while maintaining high transparency. The preparation of nanosilver transparent conductive film usually includes the steps of preparing the substrate, solution preparation, surface coating, curing and drying, and optical inspection. Curing and drying is one of the most important steps in the preparation of nanosilver transparent conductive film. Curing and drying refers to conveying the coated substrate into the rapid curing and drying equipment for curing and drying operations to promote the combination of silver nanoparticles and the formation of a conductive film.

[0003] However, the following problems exist in the curing and drying process of the coated substrate: 1. The coated substrate is usually cured and dried by complete ultraviolet irradiation, but the single ultraviolet light curing efficiency is low and the curing and drying time is long, which leads to low curing and drying efficiency.

[0004] 2. When two production lines are used to prepare nanosilver transparent conductive film at the same time, two sets of curing and drying equipment are required to cure and dry the substrates coated on different production lines, which results in high production costs. In addition, the coating and curing and drying are carried out separately, which results in a longer overall preparation time for the nanosilver transparent conductive film, thereby reducing the preparation efficiency of the nanosilver transparent conductive film.

[0005] Therefore, in order to solve the problems existing in the curing and drying process of the coated substrate, the present invention provides a method for preparing a nano silver transparent conductive film. Summary of the invention

[0006] The present invention provides a method for preparing a nano silver transparent conductive film, and the method for preparing the nano silver transparent conductive film specifically comprises the following steps:

[0007] S1. Prepare the substrate: Select a suitable substrate material, usually a glass substrate, and clean the substrate surface using existing cleaning equipment to ensure that its surface is smooth and clean.

[0008] S2. Solution preparation: Prepare a nanosilver solution, suspend the nanosilver particles in a solvent according to a specific formula under laboratory conditions, and fully stir and mix the solution to ensure uniform dispersion of the nanosilver particles.

[0009] S3. Coating the surface: The substrate is transported to the coating area, and then the prepared nanosilver particle solution can be evenly coated on the substrate surface using spin coating or spray coating in the prior art to form a uniform nanosilver film, ensuring uniform coating and moderate coating thickness.

[0010] S4, curing and drying: while the substrate is being coated, the coated substrate transported to the curing and drying area is rapidly cured and dried by the curing and drying unit to promote the combination of nanosilver particles and the formation of a conductive film, thereby improving the conductivity and stability of the film.

[0011] S5. Optical inspection: Use existing inspection equipment to conduct optical inspection on the prepared nanosilver transparent conductive film, and evaluate the performance of the conductive film by inspecting indicators such as light transmittance, conductivity, and surface uniformity to ensure that the transparency and conductivity of the nanosilver transparent conductive film meet the requirements.

[0012] The method for preparing a nanosilver transparent conductive film using the above steps S1-S5 also specifically involves a nanosilver transparent conductive film preparation device in the process of preparing the nanosilver transparent conductive film, including a conveying table composed of two left and right conveying surfaces and a fixed part, a gantry is set on the upper ends of the left and right fixed parts of the conveying table, and a curing and drying unit is set below the horizontal section of the gantry; the curing and drying unit includes a rotating shaft rotatably installed between the middle fixed part of the conveying table and the horizontal section of the gantry, a movable plate is slidably sleeved on the outside of the rotating shaft, a mounting seat is installed on the right end of the movable plate, and light curing lamps arranged in a matrix are arranged at the lower end of the mounting seat, and drying heads evenly arranged on the left and right are arranged between the front and rear adjacent light curing lamps, and the curing and drying unit is installed. The upper end of the mounting seat is respectively provided with a light-curing device and a drying device for controlling the light-curing lamp and the drying head, a limit assembly is provided at the right end of the mounting seat, a control assembly for controlling the left and right movement and the front and back swing of the drying head is provided at the upper end of the mounting seat, and a driving assembly for driving the rotating shaft to rotate and the mounting seat to move downward is provided on the horizontal section of the gantry; the limit assembly includes a limit plate installed at the right end of the mounting seat, and limit columns are installed at the upper ends of the left and right fixed parts of the conveying platform, and semicircular grooves that can cooperate with the limit columns are provided on the front and rear sides of the limit plate, and alignment columns that are symmetrical about the semicircular grooves are installed on the front and rear ends of the limit plate, and a matching block is installed on the rear side of the limit column for sliding up and down, and an alignment hole is provided on the matching block for plugging and cooperating with the corresponding alignment column.

[0013] In one embodiment, the driving assembly includes a gear fixedly mounted on the upper end of the rotating shaft, a rack meshing on the rear side of the gear and connected to the horizontal section of the gantry for sliding left and right, the left end of the rack being connected to the pushing end of the cylinder, the cylinder being installed at the lower end of the horizontal end of the gantry, a connecting piece being arranged between the left and right matching blocks and the movable plate, and a hydraulic cylinder installed on the horizontal section of the gantry being arranged at the upper end of the connecting piece.

[0014] In one of the embodiments, the connecting member includes a semicircular groove plate arranged between the left and right limit columns, and the left and right ends of the semicircular groove plate are respectively equipped with connecting plates that are slidably connected to the corresponding limit columns up and down, and the lower end of the rear side of the connecting plate is equipped with a connecting column 1 that is fixedly connected to a matching block, and the inner ring surface of the middle section of the semicircular groove plate is equipped with a control plate sleeved on the rotating shaft, and the pushing end of the hydraulic cylinder slides through the horizontal section of the gantry and is connected to the control plate, and the lower end of the control plate is equipped with a connecting column 2 that is symmetrical on the left and right and rotatably connected to the moving plate, and the upper end of the mounting seat is equipped with a support frame, and the upper end of the support frame is equipped with a support rod that is slidably connected to the semicircular groove plate.

[0015] In one embodiment, the control component includes a front-to-back symmetrical cross bar, and the drying heads evenly arranged on the left and right are installed at the lower end of the same cross bar. A connecting groove rotatably connected to the cross bar is provided on the mounting seat, and a horizontal column with No. 1 threads on both ends is rotatably installed between the left and right groove walls of the connecting groove. The cross bar is slidably installed on the outside of the horizontal column, and a left-right symmetrical inverted shaped plate is slidably installed on the upper end of the mounting seat. The vertical section of the inverted shaped plate slides left and right and passes through the mounting seat and is threadedly connected to the corresponding horizontal column. The cross bar is rotatably installed between the vertical sections of the left and right inverted shaped plates, and a fixed column slidably connected to the horizontal sections of the left and right inverted shaped plates is installed on the upper end of the mounting seat.

[0016] In one of the embodiments, a rectangular plate is installed at the upper end of the horizontal section of the inverted shaped plate on the left side, and a connecting rod is hinged on the upper end of the rectangular plate. The other end of the connecting rod is hinged on a sliding rod through a pin shaft, and a driven pulley is provided at the lower end of the sliding rod. The sliding rod is slidably connected to a guide frame installed on the upper end of the driven pulley, and an elliptical groove slidably connected to the pin shaft is provided at the upper end of the driven pulley. A mounting frame rotatably connected to the lower end of the driven pulley is installed at the upper end of the mounting seat, and a driving pulley rotatably installed on the upper end of the mounting seat is provided on the front side of the driven pulley. The driving pulley and the driven pulley are connected by a belt drive, and the upper end of the driving pulley is connected to the output shaft of the motor, and the motor is installed on the upper end of the mounting seat through a bracket.

[0017] In one of the embodiments, the outer side of the alignment column is provided with an installation hole which is symmetrical up and down, a push rod is installed in the installation hole for vertical sliding, a telescopic spring is connected between the push rod and the wall of the installation hole, and the wall of the alignment hole is provided with auxiliary holes which are symmetrical up and down and are slidably connected to the corresponding push rod.

[0018] In one of the embodiments, the left and right limit posts and the lower end of the rotating shaft are both provided with No. 2 threads, and the left and right limit posts and the rotating shaft are both threadedly installed with limit rings.

[0019] In one of the embodiments, a protective cover is fixedly mounted on the outside of the mounting seat, and the protective cover is fixedly connected to the movable plate and the limiting plate.

[0020] In summary, the present invention includes at least one of the following beneficial effects:

[0021] 1. The present invention provides a method for preparing a nanosilver transparent conductive film, which first uses ultraviolet light from a light curing lamp to provide sufficient energy to fully cure a nanosilver particle solution, and then uses hot air from a drying head to quickly and effectively dry the pre-cured substrate. The hot air can further completely sinter the nanosilver particles to each other, thereby improving the conductivity and stability of the film, accelerating the curing and drying efficiency, and thus improving the preparation efficiency of the nanosilver conductive film.

[0022] 2. The present invention provides a method for preparing a nano silver transparent conductive film. By rotating the mounting seat, the curing and drying unit can complete the curing and drying of the substrates on the left and right conveying surfaces side by side. One curing and drying unit can quickly complete the curing and drying of the coated substrates on two production lines, effectively reducing the production cost. At the same time, the coating pause time is used to timely cure and dry the coated substrates, and there is no need to cure and dry the coated substrates separately, which greatly improves the curing and drying speed of the substrate, effectively shortens the preparation time of the nano silver transparent conductive film, and thus improves the preparation efficiency of the nano silver transparent conductive film.

[0023] 3. The present invention provides a method for preparing a nano silver transparent conductive film. Through the cooperation between the matching blocks and the limiting plates on the left and right sides, the mounting seat can be limited in rotation before and after rotation. At the same time, a stable rectangular drying structure is formed between the rotating shaft, the mounting seat, the limiting plate, the movable plate, the limiting column and the corresponding matching blocks, which can further improve the stability of the mounting seat during rapid rotation and the curing and drying process.

[0024] In addition to the technical problems solved by the embodiments of the present invention described above, the technical features that constitute the technical solutions, and the beneficial effects brought about by the technical features of these technical solutions, other technical problems that can be solved by a method for preparing a nanosilver transparent conductive film provided by an embodiment of the present application, other technical features included in the technical solutions, and the beneficial effects brought about by these technical features will be further described in detail in the specific implementation manner. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0026] Figure 1 The present invention is a flow chart of a method for preparing a nano silver transparent conductive film.

[0027] Figure 2It is a schematic diagram of the main three-dimensional structure of a preparation device for a nano silver transparent conductive film of the present invention.

[0028] Figure 3 It is a schematic diagram of the three-dimensional structure of the curing and drying unit of the present invention.

[0029] Figure 4 It is a schematic diagram of the three-dimensional structure of the driving assembly and the connecting member of the present invention.

[0030] Figure 5 It is a schematic diagram of the three-dimensional structure of the limiting component of the present invention.

[0031] Figure 6 It is a schematic diagram of the three-dimensional structure of the mounting base and the control assembly of the present invention.

[0032] Figure 7 It is a schematic diagram of the three-dimensional structure of the horizontal column, the cross bar and the inverted profile plate of the present invention.

[0033] Figure 8 It is a schematic diagram of the three-dimensional structure of the light curing lamp and the drying head of the present invention.

[0034] Reference numerals: 1, conveying platform; 11, conveying surface; 2, gantry; 21, curing and drying unit; 211, rotating shaft; 212, moving plate; 213, mounting seat; 214, light curing lamp; 215, drying head; 216, light curing device; 217, drying device; 218, limiting plate; 219, limiting column; 220, alignment column; 221, matching block; 223, alignment hole; 224, gear; 225, rack; 226, cylinder; 227, hydraulic cylinder; 228, semicircular groove plate; 229, connecting plate; 230. Connecting column one; 231. Control board; 232. Connecting column two; 233. Support rod; 234. Cross bar; 235. Horizontal column; 236. Inverted plate; 237. Fixed column; 238. Connecting rod; 239. Sliding rod; 240. Driven pulley; 241. Guide frame; 242. Oval groove; 243. Driving pulley; 244. Belt; 245. Motor; 246. Mounting frame; 247. Retaining rod; 248. Telescopic spring; 249. Auxiliary hole; 250. Limiting ring; 251. Protective cover. DETAILED DESCRIPTION

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0036] See also Figure 1 A method for preparing a nano silver transparent conductive film, the method for preparing the nano silver transparent conductive film specifically comprises the following steps:

[0037] S1. Prepare the substrate: Select a suitable substrate material, usually a glass substrate, and clean the substrate surface using existing cleaning equipment to ensure that its surface is smooth and clean.

[0038] S2. Solution preparation: Prepare a nanosilver solution, suspend the nanosilver particles in a solvent according to a specific formula under laboratory conditions, and fully stir and mix the solution to ensure uniform dispersion of the nanosilver particles.

[0039] S3. Coating the surface: The substrate is transported to the coating area, and then the prepared nanosilver particle solution can be evenly coated on the substrate surface using spin coating or spray coating in the prior art to form a uniform nanosilver film, ensuring uniform coating and moderate coating thickness.

[0040] S4, curing and drying: while the substrate is being coated, the coated substrate transported to the curing and drying area is rapidly cured and dried by the curing and drying unit 21 to promote the combination of nanosilver particles and the formation of a conductive film, thereby improving the conductivity and stability of the film.

[0041] S5. Optical inspection: Use existing inspection equipment to conduct optical inspection on the prepared nanosilver transparent conductive film, and evaluate the performance of the conductive film by inspecting indicators such as light transmittance, conductivity, and surface uniformity to ensure that the transparency and conductivity of the nanosilver transparent conductive film meet the requirements.

[0042] See also Figure 1 The method for preparing a nanosilver transparent conductive film using the above steps S1-S5 also specifically involves a nanosilver transparent conductive film preparation device in the process of preparing the nanosilver transparent conductive film, including a conveying platform 1 composed of two left and right conveying surfaces 11 and a fixed part, a gantry 2 is set on the upper ends of the left and right fixed parts of the conveying platform 1, and a curing and drying unit 21 is set below the horizontal section of the gantry 2; the conveying platform 1 drives the two conveying surfaces 11 to convey the substrate at the same time through a driving source, and a coating device for uniformly coating the nanosilver particle solution on the surface of the substrate is set on the front side of the conveying platform 1, and the driving source and the coating device are both existing devices, which are not shown in the figure.

[0043] See also Figure 1 , Figure 2 , Figure 3 , Figure 5 and Figure 7The curing and drying unit 21 includes a rotating shaft 211 rotatably installed between the middle fixed part of the conveying platform 1 and the horizontal section of the gantry 2, a movable plate 212 is slidably mounted on the outside of the rotating shaft 211 up and down, a mounting seat 213 is installed on the right end of the movable plate 212, and light curing lamps 214 arranged in a matrix are arranged at the lower end of the mounting seat 213, and drying heads 215 evenly arranged on the left and right are arranged between the front and rear adjacent light curing lamps 214, and light curing devices 216 and drying devices 217 for controlling the light curing lamps 214 and the drying heads 215 are respectively arranged on the upper end of the mounting seat 213, a limiting component is arranged on the right end of the mounting seat 213, and a control component for controlling the left and right movement and front and back swing of the drying head 215 is arranged on the upper end of the mounting seat 213, and a driving component for driving the rotating shaft 211 to rotate and the mounting seat 213 to move downward is arranged on the horizontal section of the gantry 2.

[0044] See also Figure 2 , Figure 3 and Figure 4 The limiting assembly includes a limiting plate 218 installed on the right end of the mounting seat 213, and limiting posts 219 are installed on the upper ends of the left and right fixed parts of the conveyor platform 1. Semicircular grooves that can cooperate with the limiting posts 219 are opened on the front and rear sides of the limiting plate 218, and alignment posts 220 that are symmetrical about the semicircular grooves are installed on the front and rear ends of the limiting plate 218. A matching block 221 is installed on the rear side of the limiting post 219 for sliding up and down, and an alignment hole 223 is opened on the matching block 221 for plugging and cooperating with the corresponding alignment post 220.

[0045] See also Figure 2 and Figure 3 The driving assembly includes a gear 224 fixedly mounted on the upper end of the rotating shaft 211, and a rack 225 is meshed with the rear side of the gear 224 and is slidably connected to the horizontal section of the gantry 2. The left end of the rack 225 is connected to the pushing end of the cylinder 226, and the cylinder 226 is installed at the lower end of the horizontal end of the gantry 2. A connecting piece is arranged between the left and right matching blocks 221 and the movable plate 212, and a hydraulic cylinder 227 installed on the horizontal section of the gantry 2 is arranged at the upper end of the connecting piece.

[0046] See also Figure 2 and Figure 3The connecting member includes a semicircular groove plate 228 arranged between the left and right limit columns 219, and the left and right ends of the semicircular groove plate 228 are respectively installed with connecting plates 229 corresponding to the limit columns 219 for sliding up and down connection, and the lower end of the rear side of the connecting plate 229 is installed with a connecting column 230 fixedly connected to the matching block 221, and the inner ring surface of the middle section of the semicircular groove plate 228 is installed with a control plate 231 sleeved on the rotating shaft 211, and the pushing end of the hydraulic cylinder 227 slides through the horizontal section of the gantry 2 and is connected to the control plate 231, and the lower end of the control plate 231 is installed with a connecting column 232 that is symmetrical on the left and right and rotatably connected to the moving plate 212, and a support frame is installed on the upper end of the mounting seat 213, and a support rod 233 slidably connected to the semicircular groove plate 228 is installed on the upper end of the support frame.

[0047] In the process of preparing nanosilver transparent conductive film, the first step is to select a suitable substrate material, usually a glass substrate, and clean the substrate surface with existing cleaning equipment to ensure that its surface is smooth and clean.

[0048] Step 2: Prepare the nanosilver solution, suspend the nanosilver particles in the solvent according to a specific formula under laboratory conditions, and fully stir and mix it to ensure the uniform dispersion of the nanosilver particles.

[0049] Step 3: The substrates placed on the left and right conveying surfaces 11 are conveyed to the coating area at the same time by the conveying table 1, and then the nanosilver particle solution is evenly coated on the surface of the substrate by the existing coating device. During this process, in order to ensure that the nanosilver particle solution is fully and effectively coated on the surface of the substrate, the conveying surface 11 needs to be suspended, and the static substrate can better complete the coating. After the coating is completed, the substrate will continue to be conveyed to the next process, and the conveying surface 11 is controlled by the conveying table 1 to intermittently convey the substrate to the coating area and coat it section by section until the coating of all substrates is completed.

[0050] Step 4: During the coating process of the coating device on the substrate surface, the conveying surface 11 and the substrate are both in a stationary state. At this time, the coated substrate is just transported to the location of the curing and drying unit 21. Then, the control plate 231 can be quickly pushed downward by the hydraulic cylinder 227 to slide downward along the rotating shaft 211. The control plate 231 drives the semicircular groove plate 228 and the connecting plates 229 at both ends to move downward synchronously. At the same time, the connecting plate 229 pushes the corresponding matching block 221 along the limit block 211 through the connecting column 230. The positioning column 219 slides downward, and the control board 231 pushes the movable plate 212 to slide downward along the rotating shaft 211 through the left and right connecting columns 232. At this time, the limiting plate 218 and the matching block 221 on the right side form a whole through the matching between the positioning column 220 and the positioning hole 223. The limiting plate 218 and the movable plate 212 can drive the mounting seat 213 to move downward synchronously with the matching block 221 and the control board 231, and the mounting seat 213 drives the light fixing device 216, the light fixing lamp 214, and the drying device 217 to move downward synchronously with the drying device 217. The head 215 is synchronously moved down to a position close to the substrate, and then the light curing lamp 214 can be controlled by the light curing device 216 to irradiate the coated substrate with ultraviolet light. Ultraviolet light has a high energy density and can provide sufficient energy to fully cure the nanosilver particle solution. The light curing lamps 214 arranged in a matrix can further accelerate the curing of the coated substrate until the nanosilver particle solution on the substrate is cured on the surface of the substrate, but the nanosilver particle solution at this time is not completely dry. Then, the drying head 215 can be controlled by the drying device 217 to quickly and effectively dry the cured substrate. At this time, the nanosilver particle solution will not be deformed by the drying hot air. The hot air can further make the nanosilver particles completely sintered with each other, thereby improving the conductivity and stability of the film. The method of curing first and then drying is different from the traditional method of completely using light to dry. The drying speed of the nanosilver particle solution is greatly increased by using drying hot air to assist ultraviolet light, thereby improving the preparation efficiency of the nanosilver conductive film.

[0051] After the substrate on the right conveying surface 11 is cured and dried, the cylinder 226 can quickly push the rack 225 to slide to the right along the horizontal section of the gantry 2. The rack 225 moves to the right and drives the gear 224 to rotate half a circle clockwise. The gear 224 drives the moving plate 212, the mounting seat 213 and the limit plate 218 to rotate half a circle clockwise through the rotating shaft 211. The light curing device 216, the light curing lamp 214, the drying device 217 and the drying head 215 rotate synchronously with the mounting seat 213. After half a circle of clockwise rotation, the mounting plate 212, the mounting seat 213 and the limit plate 218 rotate clockwise. The seat 213 is located just above the left base, and the limiting plate 218 gradually cooperates with the alignment hole 223 and the limiting column 219 on the matching block 221 through the alignment column 220 on its front side and the semicircular groove. At this time, the limiting plate 218 and the left matching block 221 also form a whole through the cooperation of the alignment column 220 and the alignment hole 223. The cooperation between the alignment hole 223 and the alignment column 220 can also ensure the accurate and stable docking between the limiting plate 218 and the matching block 221. In this process, the support frame is connected along the semicircular groove through the support rod 233. The circular groove plate 228 synchronously slides from the right end of the semicircular groove plate 228 to the left end. Through the cooperation between the semicircular groove plate 228 and the support rod 233, not only the rapid rotation of the mounting base 213 is guided and limited, but also the mounting base 213 is supported, thereby improving the stability of the mounting base 213 during the overall rotation. At this time, the light curing lamp 214 and the drying head 215 are just located at the curing and drying position above the left substrate, and then the light curing device 216 and the drying device 217 are used to control the light curing lamp 214 and the drying head 215 to cure the left substrate. The nanosilver particle solution is first photocured and then dried until the left substrate is also completely cured and dried. Through the cooperation between the matching blocks 221 and the limiting plates 218 on the left and right sides, the mounting seat 213 before and after rotation can be limited in rotation. At the same time, a stable rectangular drying structure is formed between the rotating shaft 211, the mounting seat 213, the limiting plates 218, the moving plate 212, the limiting columns 219 and the corresponding matching blocks 221, which can further improve the stability of the mounting seat 213 during rapid rotation as a whole and during the curing and drying process.

[0052] As the curing and drying of the left substrate is completed, the substrate in the coating area gradually completes the coating of the nanosilver particle solution, and then the conveying platform 1 conveys the substrate to be coated to the coating area again through the conveying surface 11, and the substrate after coating is correspondingly moved again to the area where the curing and drying unit 21 is located, and the nanosilver transparent conductive film after curing and drying is correspondingly conveyed backward, and then the left substrate can be cured and dried in the same way as above, and the mounting seat 213 can be rotated to the top of the right substrate in the same way as above and the right substrate can be cured and dried. Similarly, the left and right substrates that are subsequently transported to the curing and drying area at the same time can be cured and dried. The same curing and drying operation is performed, and the curing and drying of the substrates on the left and right conveying surfaces 11 can be completed side by side through the rotating mounting seat 213. The curing and drying of the coated substrates on the two production lines can be quickly completed by using one curing and drying unit 21. There is no need to use two curing and drying devices 217 to work at the same time, which is beneficial to reducing production costs. The coated substrates can be cured and dried in time during the coating pause time, and there is no need to cure and dry the coated substrates separately, which greatly improves the curing and drying speed of the coated substrates, effectively shortens the preparation time of the nanosilver transparent conductive film, and thus improves the preparation efficiency of the nanosilver transparent conductive film.

[0053] After the nano silver transparent conductive film is cured and dried, the control board 231, the semicircular groove plate 228 and the connecting plate 229 can be driven by the hydraulic cylinder 227 to move up and reset synchronously. The connecting plate 229 and the control board 231 respectively drive the matching block 221 and the movable plate 212 to move up and reset synchronously through the connecting column 230 and the connecting column. At this time, the mounting seat 213 moves upward and away from the conveying platform 1 synchronously with the movable plate 212, the limit plate 218 and the matching block 221, and the drying head 215 and the light curing lamp 214 as a whole move away from the conveying platform 1 synchronously. After the curing is completed, the substrate continues to be transported to the subsequent optical detection area.

[0054] Step 5: Then the prepared nanosilver transparent conductive film can be optically inspected by existing testing equipment, and the performance of the conductive film can be evaluated by testing indicators such as light transmittance, conductivity and surface uniformity to ensure that the transparency and conductivity of the nanosilver transparent conductive film can meet the requirements. Finally, the nanosilver transparent conductive films that meet the requirements can be collected uniformly.

[0055] See also Figure 5 and Figure 6The control component includes a front-to-back symmetrical cross bar 234, and the drying heads 215 evenly arranged on the left and right are installed at the lower end of the same cross bar 234. A connecting groove rotatably connected to the cross bar 234 is provided on the mounting seat 213. A horizontal column 235 with No. 1 threads on both ends is rotatably installed between the left and right groove walls of the connecting groove. The cross bar 234 is slidably installed on the outside of the horizontal column 235. A left-right symmetrical inverted plate 236 is slidably installed on the upper end of the mounting seat 213. The vertical section of the inverted plate 236 slides left and right through the mounting seat 213 and is threadedly connected to the corresponding horizontal column 235. The cross bar 234 is rotatably installed between the vertical sections of the left and right inverted plates 236. A fixed column 237 slidably connected to the horizontal sections of the left and right inverted plates 236 is installed on the upper end of the mounting seat 213.

[0056] See also Figure 5 and Figure 6 A rectangular plate is installed at the upper end of the horizontal section of the inverted shaped plate 236 on the left side, and a connecting rod 238 is hinged on the upper end of the rectangular plate. A sliding rod 239 is hinged on the other end of the connecting rod 238 through a pin shaft. A driven pulley 240 is arranged at the lower end of the sliding rod 239. The sliding rod 239 is slidably connected to a guide frame 241 installed at the upper end of the driven pulley 240. An elliptical groove 242 slidably connected to the pin shaft is opened at the upper end of the driven pulley 240. A mounting frame 246 rotatably connected to the lower end of the driven pulley 240 is installed at the upper end of the mounting seat 213. A driving pulley 243 rotatably installed at the upper end of the mounting seat 213 is arranged on the front side of the driven pulley 240. The driving pulley 243 and the driven pulley 240 are connected through a belt 244. The upper end of the driving pulley 243 is connected to the output shaft of the motor 245, and the motor 245 is installed at the upper end of the mounting seat 213 through a bracket.

[0057] During the process of curing and drying the nano silver particle solution, the active pulley 243 can be driven to rotate by the motor 245, and the active pulley 243 drives the driven pulley 240 to rotate synchronously through the belt 244, and the driven pulley 240 drives the sliding rod 239 to rotate synchronously through the cooperation between the pin shaft and the elliptical groove 242. In this process, the sliding rod 239 slides accordingly along the guide frame 241, and at the same time, the sliding rod 239 drives the rectangular plate to reciprocate left and right through the connecting rod 238, and the inverted plate 236 on the left side reciprocates left and right along the mounting seat 213 and the fixed rod synchronously with the rectangular plate. Since the vertical sections of the inverted plate 236 on the left and right sides are threadedly connected with the No. 1 thread on the horizontal column 235, the inverted plate 236 on the right side reciprocates synchronously with the inverted plate 236 on the left side through the horizontal column 235, and the inverted plate 236 on the left and right sides are The horizontal column 235 rotates with the reciprocating movement of the inverted plate 236. The horizontal column 235 drives the cross bar 234 to swing back and forth along the connecting groove while rotating, and the drying head 215 on the cross bar 234 swings back and forth synchronously. In addition, since the vertical section of the inverted plate 236 is rotatably connected with the cross bar 234, the cross bar 234 can drive the drying head 215 to reciprocate left and right synchronously with the inverted plate 236. Through the cooperation between the inverted plate 236, the horizontal column 235 and the cross bar 234, the drying head 215 moves left and right while swinging back and forth, thereby expanding the drying range of the drying head 215 drying the nano silver particle solution, and making the hot air evenly sprayed on the substrate surface, thereby increasing the drying speed, improving the drying efficiency and the drying effect.

[0058] See also Figure 4 The outside of the alignment column 220 is provided with mounting holes which are symmetrical up and down, and a push rod 247 is slidably installed in the mounting hole, and a telescopic spring 248 is connected between the push rod 247 and the wall of the mounting hole. The wall of the alignment hole 223 is provided with auxiliary holes 249 which are symmetrical up and down and slidably connected to the corresponding push rod 247.

[0059] In the process of docking and mating between the limit plate 218 and the matching block 221, the alignment post 220 on the limit plate 218 is gradually inserted into the alignment hole 223 on the matching block 221. At this time, the push rod 247 is resisted by the alignment hole 223 and compresses the telescopic spring 248 along the installation hole and approaches the horizontal axis direction of the alignment post 220. As the alignment post 220 goes deeper, the push rod 247 is acted upon by the telescopic spring 248 to slide in the direction of the auxiliary hole 249, and finally presses against the auxiliary hole 249. In the process of the limit plate 218 leaving the matching block 221, the push rod 247 is subjected to the tension and compressed and the telescopic spring 248 is pressed against the auxiliary hole 249. The compression spring 248 allows the support rod 247 to smoothly disengage from the auxiliary hole 249, and allows the alignment column 220 to smoothly leave the alignment hole 223. The cooperation between the support rod 247, the expansion spring 248 and the auxiliary hole 249 can assist the cooperation between the limit plate 218 and the matching block 221, strengthen the connection between the alignment column 220 and the alignment hole 223, and prevent the limit plate 218 and the matching block 221 from loosening due to external factors, thereby affecting the smooth progress of subsequent curing and drying. At the same time, it can also ensure the smooth rotation and up and down movement of the mounting seat 213, thereby improving the stability during curing and drying.

[0060] See also Figure 2 and Figure 3 The left and right limit posts 219 and the lower ends of the rotating shaft 211 are both provided with No. 2 threads, and the left and right limit posts 219 and the rotating shaft 211 are both threadedly installed with limit rings 250.

[0061] Before the mounting seat 213 drives the light curing lamp 214 and the drying head 215 to move downward, the limiting ring 250 can be rotated to cooperate between the No. 2 thread and the limiting ring 250 to move the limiting column 219 and the limiting ring 250 on the rotating shaft 211 to appropriate positions respectively. In the subsequent downward movement of the movable plate 212 and the connecting plate 229, they gradually conflict with the limiting ring 250. The limiting ring 250 is used to limit the downward movement of the movable plate 212 and the connecting plate 229 to ensure that the light curing lamp 214, the drying head 215 and the substrate always maintain a suitable distance, so that the light curing lamp 214 and the drying head 215 can play their role to the greatest extent, thereby improving the curing and drying effect. In addition, the limiting ring 250 can be flexibly rotated to change the limiting position of the limiting ring 250 on the movable plate 212 and the connecting plate 229 according to the concentration and amount of the nanosilver particle solution on the substrate.

[0062] See also Figure 1 , Figure 2 and Figure 3 The mounting seat 213 is externally fixed with a protective cover 251 , and the protective cover 251 is fixedly connected to the movable plate 212 and the limiting plate 218 .

[0063] When the mounting base 213 moves downward, the protective cover 251 moves downward synchronously therewith. During the process of curing and drying the substrate by the light curing lamp 214 and the drying head 215, the curing and drying area can be limited by the protective cover 251, and the ultraviolet light generated by the light curing lamp 214 and the hot air generated by the drying head 215 can be confined within the protective cover 251, so that the ultraviolet light and the drying hot air can completely act on the surface of the substrate within the curing and drying area, thereby increasing the utilization rate of the ultraviolet light and the drying hot air, avoiding the heat of curing and drying from dissipating outward and affecting the drying efficiency and drying effect, and further improving the efficiency of curing and drying.

[0064] In the description of the present invention, it is necessary to understand that the orientations or positional relationships indicated by terms such as “middle”, “upper”, “lower”, “front”, “back”, “left”, “right”, “top” and “bottom” are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0065] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "connect", "install", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection, a sliding connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0066] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, all equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a nano silver transparent conductive film, characterized in that: The preparation method of the nano silver transparent conductive film specifically comprises the following steps: S1. Prepare the substrate: Select a suitable substrate material, usually a glass substrate, and clean the substrate surface using existing cleaning equipment to ensure that the surface is smooth and clean; S2. Solution preparation: preparing a nanosilver solution, suspending the nanosilver particles in a solvent according to a specific formula under laboratory conditions, and fully stirring and mixing the solution to ensure uniform dispersion of the nanosilver particles; S3, coating the surface: transporting the substrate to the coating area, and then using spin coating or spray coating in the prior art to evenly coat the prepared nanosilver particle solution on the substrate surface to form a uniform nanosilver film, ensuring uniform coating and moderate coating thickness; S4, curing and drying: while the substrate is being coated, the substrate that has been coated and transported to the curing and drying area is rapidly cured and dried by the curing and drying unit (21) to promote the combination of nano silver particles and the formation of a conductive film, thereby improving the conductivity and stability of the film; S5. Optical testing: Use existing testing equipment to perform optical testing on the prepared nanosilver transparent conductive film, and evaluate the performance of the conductive film by testing indicators such as light transmittance, conductivity, and surface uniformity to ensure that the transparency and conductivity of the nanosilver transparent conductive film meet the requirements; A method for preparing a nanosilver transparent conductive film using the above steps S1-S5 also specifically involves a nanosilver transparent conductive film preparation device in the process of preparing the nanosilver transparent conductive film, comprising a conveying platform (1) consisting of two left and right conveying surfaces (11) and a fixed part, a gantry (2) is arranged on the upper ends of the left and right fixed parts of the conveying platform (1), and a curing and drying unit (21) is arranged below the horizontal section of the gantry (2); The curing and drying unit (21) comprises a rotating shaft (211) rotatably mounted between a fixed portion in the middle of the conveying platform (1) and a horizontal section of the gantry (2); a movable plate (212) is mounted on the outer portion of the rotating shaft (211) for sliding upward and downward movement; a mounting seat (213) is mounted on the right end of the movable plate (212); a light curing lamp (214) arranged in a matrix is ​​disposed at the lower end of the mounting seat (213); and drying heads (215) evenly arranged on the left and right are disposed between the light curing lamps (214) adjacent to each other in front and behind. ), a light fixing device (216) and a drying device (217) for controlling a light fixing lamp (214) and a drying head (215) are respectively arranged at the upper end of the mounting seat (213), a limit position component is arranged at the right end of the mounting seat (213), a control component for controlling the left and right movement and the front and back swing of the drying head (215) is arranged at the upper end of the mounting seat (213), and a driving component for driving the rotating shaft (211) to rotate and the mounting seat (213) to move downward is arranged on the horizontal section of the gantry (2); The limiting assembly comprises a limiting plate (218) mounted on the right end of the mounting seat (213); limiting posts (219) are mounted on the upper ends of the left and right fixed parts of the conveying platform (1); semicircular grooves that can be matched with the limiting posts (219) are provided on the front and rear sides of the limiting plate (218); alignment posts (220) that are symmetrical about the semicircular grooves are mounted on the front and rear ends of the limiting plate (218); a matching block (221) is mounted on the rear side of the limiting post (219) so as to slide up and down; and an alignment hole (223) that is plugged and matched with the corresponding alignment post (220) is provided on the matching block (221).

2. The method for preparing a nano silver transparent conductive film according to claim 1, characterized in that: The driving assembly comprises a gear (224) fixedly mounted on the upper end of the rotating shaft (211); a rack (225) meshing with the rear side of the gear (224) and connected to the horizontal section of the gantry (2) in a left-right sliding manner; the left end of the rack (225) is connected to the pushing end of a cylinder (226); the cylinder (226) is mounted on the lower end of the horizontal end of the gantry (2); a connecting piece is arranged between the left and right matching blocks (221) and the movable plate (212); and a hydraulic cylinder (227) mounted on the horizontal section of the gantry (2) is arranged on the upper end of the connecting piece.

3. The method for preparing a nano silver transparent conductive film according to claim 2, characterized in that: The connecting member comprises a semicircular groove plate (228) arranged between left and right limit columns (219), the left and right ends of the semicircular groove plate (228) are respectively provided with connecting plates (229) connected to the corresponding limit columns (219) in an upward and downward sliding manner, the lower end of the rear side of the connecting plate (229) is provided with a connecting column (230) fixedly connected to the matching block (221), the inner ring surface of the middle section of the semicircular groove plate (228) is provided with a control plate (231) sleeved on the rotating shaft (211), the pushing end of the hydraulic cylinder (227) slides through the horizontal section of the gantry (2) and is connected to the control plate (231), the lower end of the control plate (231) is provided with a connecting column (232) which is symmetrical and rotatably connected to the moving plate (212), the upper end of the mounting seat (213) is provided with a support frame, and the upper end of the support frame is provided with a support rod (233) slidably connected to the semicircular groove plate (228).

4. The method for preparing a nano silver transparent conductive film according to claim 1, characterized in that: The control assembly comprises a front-to-rear symmetrical cross bar (234), the drying heads (215) evenly arranged on the left and right are mounted on the lower end of the same cross bar (234), a connecting groove rotatably connected to the cross bar (234) is provided on the mounting seat (213), a horizontal column (235) with No. 1 threads on both the left and right ends is rotatably mounted between the left and right groove walls of the connecting groove, the cross bar (234) is slidably mounted on the outside of the horizontal column (235), a left-right symmetrical inverted plate (236) is slidably mounted on the upper end of the mounting seat (213), the vertical section of the inverted plate (236) slides left and right through the mounting seat (213) and is threadedly connected to the corresponding horizontal column (235), the cross bar (234) is rotatably mounted between the vertical sections of the left and right inverted plates (236), and a fixed column (237) slidably connected to the horizontal sections of the left and right inverted plates (236) is installed on the upper end of the mounting seat (213).

5. The method for preparing a nano silver transparent conductive film according to claim 4, characterized in that: A rectangular plate is installed at the upper end of the horizontal section of the inverted plate (236) on the left side, a connecting rod (238) is hinged at the upper end of the rectangular plate, a sliding rod (239) is hinged at the other end of the connecting rod (238) through a pin shaft, a driven pulley (240) is arranged at the lower end of the sliding rod (239), the sliding rod (239) is slidably connected to a guide frame (241) installed at the upper end of the driven pulley (240), an elliptical groove (242) slidably connected to the pin shaft is opened at the upper end of the driven pulley (240), and the driven pulley (240) is provided with a plurality of guide frames (241) installed at the upper end of the driven pulley (240). The upper end of the mounting seat (213) is provided with a mounting frame (246) rotatably connected to the lower end of the driven pulley (240); the front side of the driven pulley (240) is provided with a driving pulley (243) rotatably mounted on the upper end of the mounting seat (213); the driving pulley (243) and the driven pulley (240) are connected to each other through a belt (244); the upper end of the driving pulley (243) is connected to the output shaft of the motor (245); and the motor (245) is mounted on the upper end of the mounting seat (213) through a bracket.

6. The method for preparing a nano silver transparent conductive film according to claim 1, characterized in that: The alignment posts (220) are provided with vertically symmetrical mounting holes on their exteriors, abutment rods (247) are slidably mounted in the mounting holes, a telescopic spring (248) is connected between the abutment rods (247) and the wall of the mounting holes, and the walls of the alignment holes (223) are provided with vertically symmetrical auxiliary holes (249) that are slidably connected to the corresponding abutment rods (247).

7. The method for preparing a nano silver transparent conductive film according to claim 1, characterized in that: The lower ends of the left and right limit posts (219) and the rotating shaft (211) are both provided with No. 2 threads, and the left and right limit posts (219) and the rotating shaft (211) are both threadedly mounted with limit rings (250).

8. The method for preparing a nano silver transparent conductive film according to claim 1, characterized in that: The mounting seat (213) is externally fixedly sleeved with a protective cover (251), and the protective cover (251) is fixedly connected to the movable plate (212) and the limiting plate (218).