Nitride LED epitaxial wafer and preparation method and application thereof

By using a composite buffer layer structure to adjust lattice mismatch and stress in nitride LED epitaxial wafers, the efficiency and life problems caused by dislocations and defects in group III nitride semiconductor materials in heteroepitaxial wafers are solved, and efficient Luminous performance and long life.

CN118738243AActive Publication Date: 2024-10-01JIANGSU INST OF ADVANCED SEMICON CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411072780.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-01
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Dislocations or defects caused by lattice constants and thermal mismatch in Group III nitride semiconductor materials during the heteroepitaxial process affect device efficiency and life, limiting their application in the field of semiconductor electronics.

Method used

Adopting a composite buffer layer structure, including a nitride front layer, a composite structural layer, a nitride back layer and a nitride covering layer, the lattice mismatch is adjusted through the patterning effect of the composite structural layer, reducing stress and improving the crystal quality of the nitride light-emitting layer. quality and luminous efficiency.

Benefits of technology

Through full diversion of dislocations and stress relief, the crystal quality and luminous efficiency of nitride LED epitaxial wafers are improved, the device life is extended, and its reliability in semiconductor applications is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738243A_ABST
    Figure CN118738243A_ABST
Patent Text Reader

Abstract

The invention provides a nitride LED epitaxial wafer and a preparation method and application thereof. The nitride LED epitaxial wafer comprises a substrate, a composite buffer layer, a nitride buffer layer, a first nitride layer, a nitride light-emitting layer and a second nitride layer which are arranged in a stacked mode. Wherein the composite buffer layer comprises a nitride front layer, a composite structure layer, a nitride rear layer and a nitride covering layer which are stacked, and the nitride front layer is arranged on the surface of the substrate; and the composite structure layer has a nano pattern structure and is used for adjusting lattice mismatch between the nitride front layer and the nitride rear layer. By adopting the scheme provided by the invention, the problem of dislocation or defects caused by lattice constant and thermal mismatch can be solved, and multifunctional buffer technology development is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor optoelectronic devices and relates to a nitride LED epitaxial wafer, and in particular to a nitride LED epitaxial wafer and a preparation method and application thereof. Background Art

[0002] III-V nitride semiconductor materials are widely used in optoelectronic devices, optoelectronic integration, ultra-high-speed microelectronic devices, and ultra-high-frequency microwave devices and circuits, and have broad application prospects.

[0003] Since III-nitrides are generally grown heteroepitaxially on heterogeneous substrates such as sapphire or SiC, the lattice constants and thermal mismatches between different materials will produce dislocations or defects, which extend upward as the epitaxial layer grows. These dislocations or defects appear as non-radiative recombination centers when the device is working, affecting the device efficiency. At the same time, they act as leakage channels, causing the leakage current to increase and causing the device to age rapidly, thereby affecting the device's working efficiency and life, restricting its promotion and application in the field of semiconductor electronics. Summary of the invention

[0004] The purpose of the present invention is to provide a nitride LED epitaxial wafer and a preparation method and application thereof. By adopting the solution provided by the present invention, the dislocation or defect problems caused by lattice constant and thermal mismatch can be overcome, and the development of multifunctional buffer technology can be realized.

[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a nitride LED epitaxial wafer, wherein the nitride LED epitaxial wafer comprises a stacked substrate, a composite buffer layer, a nitride buffer layer, a first nitride layer, a nitride light-emitting layer and a second nitride layer.

[0007] Among them, the composite buffer layer includes a stacked nitride front layer, a composite structure layer, a nitride rear layer and a nitride covering layer, and the nitride front layer is arranged on the surface of the substrate; the composite structure layer has a nano-pattern structure for adjusting the lattice mismatch between the nitride front layer and the nitride rear layer.

[0008] On the one hand, the present invention promotes the full redirection of dislocations in the growth process of the epitaxial wafer through the graphic effect of the composite structure layer, thereby improving the crystal quality, and at the same time, intensifies the reflection of light in the nitride light-emitting layer toward the substrate, thereby improving the light extraction efficiency. On the other hand, the composite structure layer adjusts the lattice mismatch between the nitride front layer and the nitride rear layer, relieves the stress caused by the nitride graphic structure, reduces the stress in the nitride light-emitting layer, relieves the stress pulling effect caused by the component difference in the nitride light-emitting layer, improves the component incorporation in the nitride light-emitting layer, and can grow the nitride light-emitting layer at a relatively high temperature, thereby improving the crystal quality of the nitride light-emitting layer, and improving the light-emitting efficiency and brightness of the epitaxial wafer.

[0009] Preferably, the composite structural layer is an AlSiN composite structural layer, comprising a SiN structural layer, an AlN structural layer, and AlN microstructural units and SiN microstructural units that are arranged opposite to each other.

[0010] Among them, the AlN structural layer is arranged between the SiN structural layer and the nitride front layer; the AlN structural layer is at least partially embedded in the nitride front layer; the AlN microstructure unit presents a convex structure and is embedded in the SiN structural layer; the SiN microstructure unit presents a concave structure and is embedded in the AlN structural layer.

[0011] Preferably, the longitudinal heights of the AlN microstructure unit and the SiN microstructure unit are respectively 1-20 nm.

[0012] Preferably, radial dimensions of the AlN microstructure unit and the SiN microstructure unit are 5-150 nm respectively.

[0013] Preferably, the nitride front layer is penetrated by nanopores.

[0014] Preferably, the AlSiN composite structure layer includes at least two first AlSiN composite units arranged in the nanopore, the first AlSiN composite unit includes a SiN structure layer, an AlN structure layer, and relatively arranged AlN microstructure units and SiN microstructure units, and the height of the first AlSiN composite unit is less than or equal to the depth of the nanopore.

[0015] Alternatively, the AlSiN composite structure layer includes at least two second AlSiN composite units disposed in the nanopores and a SiN structure layer disposed on the second AlSiN composite unit, and the second AlSiN composite unit includes an AlN structure layer and relatively disposed AlN microstructure units and SiN microstructure units.

[0016] Preferably, the pore size of the nanopore is 5-150 nm.

[0017] In a second aspect, the present invention provides a method for preparing the nitride LED epitaxial wafer as described in the first aspect, the preparation method comprising:

[0018] providing a substrate;

[0019] Depositing a nitride front layer, a composite structure layer, a nitride rear layer and a nitride capping layer in sequence on the surface of the substrate to form a composite buffer layer;

[0020] A nitride buffer layer, a first nitride layer, a nitride light-emitting layer and a second nitride layer are sequentially deposited on the surface of the composite buffer layer to obtain the nitride LED epitaxial wafer.

[0021] Preferably, the deposition of the composite structure layer comprises:

[0022] S11, in an inert gas atmosphere, introducing an Al source for surface pretreatment, wherein the flow rate of the Al source is 100-300 sccm and the introduction time is 2-15 s;

[0023] S12, in an inert gas atmosphere, introducing a Si source for surface pretreatment, wherein the flow rate of the Si source is 10-300 sccm and the introduction time is 5-20 s;

[0024] S13, in an inert gas atmosphere, introducing a N source for surface pretreatment, wherein the flow rate of the N source is 1-25 slm and the introduction time is 10-30 s;

[0025] S14, alternately and repeatedly executing steps S11 to S13 to obtain the composite structure layer.

[0026] Wherein, the number of repetitions of step S11 to step S13 is 1-50 times, and the thickness of the composite structure layer is 2-100 nm.

[0027] Preferably, the deposition of the nitride rear layer comprises:

[0028] S21, under the second setting condition, introducing a first flow rate of Al source for surface treatment, wherein the first flow rate is 100-300 sccm, and the introduction time of the first flow rate of Al source is 2-10 s;

[0029] S22, under the second setting condition, introducing a second flow rate of Al source for surface treatment, wherein the second flow rate is 5-100 sccm, and the introduction time of the second flow rate of Al source is 5-20 s;

[0030] S23. Under the second setting condition, a N source is introduced for surface treatment, wherein the flow rate of the N source is 5-50 slm and the introduction time is 5-20 s.

[0031] The second setting conditions include a temperature of 650-950° C., a pressure of 50-500 torr, and a growth thickness of 10-50 nm.

[0032] Preferably, the nitride front layer is a SiN pattern structure layer, and the deposition of the nitride front layer includes:

[0033] Under the first set conditions, Si source and N source are introduced to grow the SiN graphic structure layer on the surface of the substrate; wherein the first set conditions include a temperature of 1000-1200°C, a pressure of 50-500torr, a flow rate of the Si source of 10-300sccm, a flow rate of the N source of 1-100slm, and a growth thickness of 5-50nm.

[0034] Preferably, the deposition of the nitride capping layer comprises:

[0035] Under the third setting condition, the nitride capping layer is grown on the surface of the nitride rear layer; wherein the third setting condition includes a temperature of 1050-1250° C., a pressure of 100-500 torr, and a growth thickness of 20-100 nm.

[0036] And / or, the deposition of the nitride buffer layer comprises:

[0037] Under the fourth setting condition, the nitride buffer layer is grown on the surface of the nitride capping layer; wherein the fourth setting condition includes a temperature of 1050-1150° C., a pressure of 100-500 torr, and a growth thickness of 0.1-3 μm.

[0038] And / or, the depositing of the first nitride layer comprises:

[0039] Under the fifth setting condition, the first nitride layer is grown on the surface of the nitride buffer layer; wherein the fifth setting condition includes a temperature of 1000-1100° C., a pressure of 100-500 torr, a growth thickness of 0.5-10 μm, and a doping concentration of (1-8)×10 18 cm -3 .

[0040] Preferably, the deposition of the nitride light emitting layer comprises:

[0041] Under the sixth setting condition, a nitride quantum well layer and a nitride quantum barrier layer are periodically grown on the surface of the first nitride layer to form the nitride light-emitting layer; wherein the sixth setting condition includes a temperature of 700-1200° C. and a pressure of 100-500 torr.

[0042] Preferably, the growth conditions of the nitride quantum well layer include a temperature of 700-1150° C., a pressure of 100-500 torr, and a growth thickness of 1-6 nm.

[0043] Preferably, the growth conditions of the nitride quantum barrier layer include a temperature of 750-1200° C., a pressure of 100-500 torr, and a growth thickness of 3-15 nm.

[0044] Preferably, the number of stacked groups of the nitride quantum well layer and the nitride quantum barrier layer is 2-15 groups.

[0045] And / or, the depositing of the second nitride layer comprises:

[0046] Under the seventh setting condition, the second nitride layer is grown on the surface of the nitride light-emitting layer; wherein the seventh setting condition includes a temperature of 900-1100° C., a pressure of 100-500 torr, a growth thickness of 0.02-0.3 μm, and a doping concentration of (0.1-10)×10 20 cm -3 .

[0047] In a third aspect, the present invention provides an application of the nitride LED epitaxial wafer as described in the first aspect, wherein the nitride LED epitaxial wafer is used for manufacturing semiconductor devices.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] (1) The present invention promotes the full redirection of dislocations in the growth process of the epitaxial wafer through the patterning effect of the composite structure layer, thereby improving the crystal quality. At the same time, it intensifies the reflection of light in the nitride light-emitting layer toward the substrate, thereby improving the light extraction efficiency.

[0050] (2) The composite structure layer adjusts the lattice mismatch between the nitride front layer and the nitride back layer, relieves the epitaxial wafer stress caused by the nitride graphic structure, reduces the stress in the nitride light-emitting layer, relieves the stress pulling effect caused by the component difference in the nitride light-emitting layer, and improves the component incorporation in the nitride light-emitting layer. The nitride light-emitting layer can be grown at a relatively high temperature, thereby improving the crystal quality of the nitride light-emitting layer, and improving the luminescence efficiency and brightness of the epitaxial wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a schematic diagram of the structure of the nitride LED epitaxial wafer provided by the present invention;

[0052] Figure 2 is a schematic diagram of the composite structure layer in the nitride LED epitaxial wafer provided in Example 1;

[0053] Figure 3is a schematic diagram of the composite structure layer in the nitride LED epitaxial wafer provided in Example 2;

[0054] Figure 4 This is a schematic diagram of the composite structure layer in the nitride LED epitaxial wafer provided in Example 3.

[0055] Among them: 10-substrate; 20-composite buffer layer; 21-nitride front layer; 22-composite structural layer; 23-nitride rear layer; 24-nitride covering layer; 25-nanopore; 26-SiN structural layer; 27-AlN structural layer; 28-SiN microstructure unit; 29-AlN microstructure unit; 30-nitride buffer layer; 31-first AlSiN composite unit; 32-second AlSiN composite unit; 41-first nitride layer; 42-second nitride layer; 50-nitride light-emitting layer. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0057] The invention provides a nitride LED epitaxial wafer, which comprises a stacked substrate, a composite buffer layer, a nitride buffer layer, a first nitride layer, a nitride light-emitting layer and a second nitride layer.

[0058] Furthermore, the composite buffer layer includes a stacked nitride front layer, a composite structural layer, a nitride rear layer and a nitride covering layer, and the nitride front layer is arranged on the surface of the substrate; the composite structural layer has a nano-pattern structure for adjusting the lattice mismatch between the nitride front layer and the nitride rear layer.

[0059] On the one hand, the present invention promotes the full redirection of dislocations in the growth process of the epitaxial wafer through the graphic effect of the composite structure layer, thereby improving the crystal quality, and at the same time, intensifies the reflection of light in the nitride light-emitting layer toward the substrate, thereby improving the light extraction efficiency. On the other hand, the composite structure layer adjusts the lattice mismatch between the nitride front layer and the nitride rear layer, relieves the stress caused by the nitride graphic structure, reduces the stress in the nitride light-emitting layer, relieves the stress pulling effect caused by the component difference in the nitride light-emitting layer, improves the component incorporation in the nitride light-emitting layer, and can grow the nitride light-emitting layer at a relatively high temperature, thereby improving the crystal quality of the nitride light-emitting layer, and improving the light-emitting efficiency and brightness of the epitaxial wafer.

[0060] In some embodiments, the composite structure layer is an AlSiN composite structure layer, including a SiN structure layer, an AlN structure layer, and AlN microstructure units and SiN microstructure units that are relatively arranged.

[0061] Furthermore, the AlN structural layer is arranged between the SiN structural layer and the nitride front layer; the AlN structural layer is at least partially embedded in the nitride front layer; the AlN microstructure unit presents a convex structure and is embedded in the SiN structural layer; the SiN microstructure unit presents a concave structure and is embedded in the AlN structural layer.

[0062] In some embodiments, the longitudinal heights of the AlN microstructure unit and the SiN microstructure unit are respectively 1-20 nm, for example, 1 nm, 2 nm, 4 nm, 6 nm, 8 nm, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm or 20 nm, but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] In some embodiments, the radial dimensions of the AlN microstructure unit and the SiN microstructure unit are respectively 5-150nm, for example, 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm or 150nm, but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0064] In some embodiments, the nitride front layer has nanopores extending therethrough.

[0065] In some embodiments, the AlSiN composite structure layer includes at least two first AlSiN composite units disposed in the nanopore, the first AlSiN composite unit includes a SiN structure layer, an AlN structure layer, and relatively disposed AlN microstructure units and SiN microstructure units, and the height of the first AlSiN composite unit is less than or equal to the depth of the nanopore.

[0066] In some embodiments, the AlSiN composite structure layer includes at least two second AlSiN composite units disposed in the nanopores and a SiN structure layer disposed on the second AlSiN composite unit, and the second AlSiN composite unit includes an AlN structure layer and relatively disposed AlN microstructure units and SiN microstructure units.

[0067] In some embodiments, the pore size of the nanopore is 5-150nm, for example, it can be 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm or 150nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0068] In the present invention, the nitride rear layer is an AlN layer, which provides a lattice transition for the nitride capping layer, reduces stress in the epitaxial wafer, improves the crystal quality of the epitaxial wafer, reduces crack defects on the surface of the epitaxial wafer, and thus improves the yield of the epitaxial wafer.

[0069] A certain embodiment of the present invention provides a method for preparing a nitride LED epitaxial wafer, the method comprising:

[0070] D1. Provide a substrate.

[0071] The substrate provides a support surface for the growth of nitride LED epitaxial wafers.

[0072] D2. A nitride front layer, a composite structure layer, a nitride rear layer and a nitride covering layer are sequentially deposited on the surface of the substrate to form a composite buffer layer.

[0073] D3. A nitride buffer layer, a first nitride layer, a nitride light-emitting layer and a second nitride layer are sequentially deposited on the surface of the composite buffer layer to obtain a nitride LED epitaxial wafer.

[0074] In some embodiments, the nitride front layer is a SiN graphic structure layer, and the deposition of the nitride front layer includes: introducing a Si source and an N source under a first set condition to grow the SiN graphic structure layer on the surface of the substrate.

[0075] Furthermore, the first setting conditions include a temperature of 1000-1200° C., a pressure of 50-500 torr, a flow rate of the Si source of 10-300 sccm, a flow rate of the N source of 1-100 slm, and a growth thickness of the SiN graphic structure layer of 5-50 nm. For example, the temperature may be 1000°C, 1020°C, 1040°C, 1060°C, 1080°C, 1100°C, 1120°C, 1140°C, 1160°C, 1180°C or 1200°C, but is not limited to the values ​​listed, and other values ​​not listed within the numerical range are equally applicable; the pressure may be 50 torr, 100 torr, 150 torr, 200 torr, 250 torr, 300 torr, 350 torr, 400 torr, 450 torr or 500 torr, but is not limited to the values ​​listed, and other values ​​not listed within the numerical range are equally applicable; the flow rate of the Si source may be 10 sccm, 50 sccm, 100 sccm, 150 sccm, 200 sccm, 250 sccm or 300 sccm, but is not limited to the values ​​listed. numerical values, and other unlisted numerical values ​​within the numerical range are also applicable; the flow rate of the N source can be 1slm, 5slm, 10slm, 15slm, 20slm, 25slm, 30slm, 35slm, 40slm, 45slm, 50slm, 55slm, 60slm, 65slm, 70slm, 75slm, 80slm, 85slm, 90slm, 95slm or 100slm, but is not limited to the listed numerical values, and other unlisted numerical values ​​within the numerical range are also applicable; the growth thickness of the SiN graphic structure layer is 5-50nm, for example, it can be 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm or 50nm, but is not limited to the listed numerical values, and other unlisted numerical values ​​within the numerical range are also applicable.

[0076] In certain embodiments, depositing the composite structural layer includes:

[0077] S11. In an inert gas atmosphere, introduce an Al source for surface pretreatment.

[0078] The flow rate of the Al source is 100-300 sccm, for example, it can be 100 sccm, 120 sccm, 140 sccm, 160 sccm, 180 sccm, 200 sccm, 220 sccm, 240 sccm, 260 sccm, 280 sccm or 300 sccm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0079] The introduction time of the Al source is 2-15s, for example, it can be 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s, 10s, 11s, 12s, 13s, 14s or 15s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0080] S12. In an inert gas atmosphere, introduce a Si source for surface pretreatment.

[0081] The inert gas may be N2, the Si source may be SiH4, and the flow rate of the Si source may be 10-300sccm, for example, 10sccm, 50sccm, 100sccm, 150sccm, 200sccm, 250sccm or 300sccm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0082] The Si source is introduced for 5-20 s, for example, it can be 5s, 6s, 7s, 8s, 9s, 10s, 11s, 12s, 13s, 14s, 15s, 16s, 17s, 18s, 19s or 20s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0083] S13. In an inert gas atmosphere, introduce a N source for surface pretreatment.

[0084] The N source may be NH3, and the flow rate of the N source may be 1-25slm, for example, 1slm, 2slm, 4slm, 6slm, 8slm, 10slm, 12slm, 14slm, 16slm, 18slm, 20slm, 22slm, 24slm or 25slm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0085] The N source is introduced for 10-30 s, for example, 10 s, 12 s, 14 s, 16 s, 18 s, 20 s, 22 s, 24 s, 26 s, 28 s or 30 s, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0086] In the present invention, the surface pretreatment of step S13 can also play the role of heat treatment of steps S11 and S12. By utilizing the mutual dissolution of Si and Al, the Al atoms distributed on the surface of the Al deposition layer formed in step S11 and the Si deposition layer in step S12 form a Si-rich deposition and diffuse with each other. The Si atoms diffuse into the Al deposition layer, and at the same time, the Al atoms diffuse into the Si deposition layer. Due to the poor surface migration activity and low mobility of Al atoms, the Al atoms in step S11 are aggregated in the area with high surface activity, while Al atoms are dispersed in the area with low surface activity. More Al atoms are spatially distributed in the Al atom aggregation area to form a diffusion extension area, and more Al atoms diffuse into the Si deposition layer. At the same time, since the diffusion rate of atoms close to the interface is faster than that of atoms far from the interface, the Si atoms and Al atoms diffuse slowly as they are far away from the interface, resulting in non-uniform diffusion of atoms on both sides of the interface. As the diffusion terminates, AlN microstructure units with convex structures and SiN microstructure units with concave structures are finally formed in the Si deposition layer and the Al deposition layer.

[0087] S14, alternately and repeatedly executing steps S11 to S13 to obtain a composite structure layer.

[0088] In some embodiments, steps S11 to S13 are repeated 1-50 times, for example, 1 time, 5 times, 10 times, 15 times, 20 times, 25 times, 30 times, 35 times, 40 times, 45 times or 50 times, but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0089] In some embodiments, the thickness of the composite structure layer is 2-100nm, for example, it can be 2nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0090] In some embodiments, the material of the nitride rear layer is AlN, and the deposition of the nitride rear layer includes:

[0091] S21. Under the second set condition, introduce a first flow rate of Al source for surface treatment.

[0092] The first flow rate is 100-300 sccm, for example, it can be 100 sccm, 120 sccm, 140 sccm, 160 sccm, 180 sccm, 200 sccm, 220 sccm, 240 sccm, 260 sccm, 280 sccm or 300 sccm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0093] The introduction time of the Al source is 2-10s, for example, it can be 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s or 10s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0094] In the present invention, high flow rate (flow rate value is 100-300sccm) Al source surface treatment can form a metal layer distribution with a thickness of 1-5nm on the surface of the composite structure layer. This high flow condition can quickly distribute the nanoscale metal layer on the surface of the composite structure layer, limit the movement of Al atoms on the surface of the composite structure layer, avoid uneven distribution of metal components due to surface potential energy differences of the composite structure layer, thereby shielding surface defects and further improving the uniformity of the metal layer distribution on the surface of the composite structure layer.

[0095] S22. Under the second set condition, introduce a second flow rate of Al source for surface treatment.

[0096] The second flow rate is 5-100sccm, for example, it can be 5sccm, 10sccm, 15sccm, 20sccm, 25sccm, 30sccm, 35sccm, 40sccm, 45sccm, 50sccm, 55sccm, 60sccm, 65sccm, 70sccm, 75sccm, 80sccm, 85sccm, 90sccm, 95sccm or 100sccm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0097] The introduction time of the Al source is 5-20s, for example, it can be 5s, 6s, 7s, 8s, 9s, 10s, 11s, 12s, 13s, 14s, 15s, 16s, 17s, 18s, 19s or 20s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0098] In the present invention, a low flow rate (flow rate value is 5-100sccm) of Al source can fully diffuse Al atoms, improve the consistency of potential energy of Al atoms distributed on the surface, alleviate the concentrated distribution of surface defects, reduce the probability of surface defects being amplified, and avoid surface defects from diffusing in the thickness direction and entering the nitride light-emitting layer, thereby preventing them from forming non-radiative recombination centers and leakage channel extensions where leakage channels are concentrated.

[0099] S23. Under the second set condition, introduce N source to perform surface treatment.

[0100] The flow rate of the N source is 5-50slm, for example, it can be 5slm, 10slm, 15slm, 20slm, 25slm, 30slm, 35slm, 40slm, 45slm or 50slm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0101] The N source is introduced for 5-20 s, for example, it can be 5s, 6s, 7s, 8s, 9s, 10s, 11s, 12s, 13s, 14s, 15s, 16s, 17s, 18s, 19s or 20s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0102] In the present invention, under the surface treatment of the N source, the low-flow metal layer is nitrided to form a metal nitride layer, which reduces nitrogen vacancy defects in the metal nitride layer, avoids leakage channels caused by defects, and improves the leakage performance of the epitaxial wafer.

[0103] Furthermore, the second setting conditions include an inert gas atmosphere, a temperature of 650-950° C., a pressure of 50-500 torr, and a growth thickness of the nitride rear layer of 10-50 nm. For example, the temperature may be 650°C, 675°C, 700°C, 725°C, 750°C, 775°C, 800°C, 825°C, 850°C, 875°C, 900°C, 925°C or 950°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable; the pressure may be 50 torr, 100 torr, 150 torr, 200 torr, 250 torr, 300 torr, 350 torr, 400 torr, 450 torr or 500 torr, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable; the growth thickness of the nitride rear layer is 10-50 nm, for example, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm or 50 nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0104] In the present invention, the lattices of the nitride rear layer and the composite structure layer match each other, and the lower growth temperature can release the stress inside the nitride rear layer through the dislocation effect, providing a low-stress growth template for the growth of the nitride cover layer.

[0105] In some embodiments, the depositing of the nitride capping layer includes: growing the nitride capping layer on the surface of the nitride rear layer under a third setting condition.

[0106] Further, the third setting condition includes a temperature of 1050-1250°C, a pressure of 100-500 torr, and a growth thickness of the nitride capping layer of 20-100 nm. For example, the temperature may be 1050°C, 1060°C, 1070°C, 1080°C, 1090°C, 1100°C, 1110°C, 1120°C, 1130°C, 1140°C, 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C or 1250°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the pressure may be 100 torr, 150 torr, 200 torr, 250 torr, 300 torr, 400 torr, 500 torr, 600 torr, 700 torr, 800 torr, 900 torr, 1000 torr, 1100 torr, 1200 torr, 1300 torr, 1300 torr, 1400 torr, 1500 torr, 1600 torr, 1700 torr, 1800 torr, 1900 torr, 2000 torr, 2100 torr, 2200 torr, 2300 torr, 2400 torr, 2500 torr, 2600 torr, 2700 torr, 2800 torr, 3000 torr, 3100 to The growth thickness of the nitride capping layer can be 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm or 100nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0107] Compared with the nitride back layer, the growth temperature of the nitride capping layer is higher, which can reduce the impurity defects in the nitride capping layer, improve the crystal quality of the nitride capping layer, and provide a lattice-matched low-defect growth template.

[0108] In some embodiments, depositing the nitride buffer layer includes:

[0109] Under the fourth setting condition, a nitride buffer layer is grown on the surface of the nitride cap layer.

[0110] Further, the fourth setting condition includes a temperature of 1050-1150°C, a pressure of 100-500 torr, and a growth thickness of the nitride buffer layer of 0.1-3 μm. For example, the temperature may be 1050°C, 1060°C, 1070°C, 1080°C, 1090°C, 1100°C, 1110°C, 1120°C, 1130°C, 1140°C, or 1150°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the pressure may be 100 torr, 150 torr, 200 torr, 250 torr, 300 torr, 350 torr, 400 torr, 450 torr, or 500 torr. rr, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the growth thickness of the nitride buffer layer is 0.1-3μm, for example, it can be 0.1μm, 0.2μm, 0.4μm, 0.6μm, 0.8μm, 1μm, 1.2μm, 1.4μm, 1.6μm, 1.8μm, 2μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm or 3μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0111] In some embodiments, depositing the first nitride layer includes: growing the first nitride layer on a surface of the nitride buffer layer under a fifth setting condition.

[0112] Further, the doping element in the first nitride layer may be Si, and the fifth setting condition includes a temperature of 1000-1100° C., a pressure of 100-500 torr, a growth thickness of the first nitride layer of 0.5-10 μm, and a doping concentration of the first nitride layer of (1-8)×10 18 cm -3For example, the temperature may be 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, 1050°C, 1060°C, 1070°C, 1080°C, 1090°C or 1100°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the pressure may be 100 torr, 150 torr, 200 torr, 250 torr, 300 torr, 350 torr, 400 torr, 450 torr or 500 torr, but is not limited to the listed values, Other values ​​not listed in the numerical range are also applicable; the growth thickness of the first nitride layer is 0.5-10 μm, for example, it can be 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm or 10 μm, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; the doping concentration of the first nitride layer can be 1×10 18 cm -3 , 2×10 18 cm -3 , 3×10 18 cm -3 , 4×10 18 cm -3 , 5×10 18 cm -3 , 6×10 18 cm -3 ,7×10 18 cm -3 or 8×10 18 cm -3 , but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0113] In some embodiments, the deposition of the nitride light emitting layer includes: under a sixth setting condition, periodically growing a nitride quantum well layer and a nitride quantum barrier layer on the surface of the first nitride layer to form the nitride light emitting layer.

[0114] Further, the sixth setting condition includes a temperature of 700-1200° C. and a pressure of 100-500 torr. For example, the temperature may be 700° C., 750° C., 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C., 1100° C., 1150° C. or 1200° C., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the pressure may be 100 torr, 150 torr, 200 torr, 250 torr, 300 torr, 350 torr, 400 torr, 450 torr or 500 torr, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0115] In some embodiments, the number of stacked groups of nitride quantum well layers and nitride quantum barrier layers is 2-15 groups, for example, it can be 2 groups, 3 groups, 4 groups, 5 groups, 6 groups, 7 groups, 8 groups, 9 groups, 10 groups, 11 groups, 12 groups, 13 groups, 14 groups or 15 groups.

[0116] In some embodiments, the growth conditions of the nitride quantum well layer include a temperature of 700-1150° C., a pressure of 100-500 torr, and a growth thickness of the nitride quantum well layer of 1-6 nm. For example, the temperature can be 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C or 1150°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable; the pressure can be 100torr, 150torr, 200torr, 250torr, 300torr, 350torr, 400torr, 450torr or 500torr, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable; the growth thickness of the nitride quantum well layer can be 1nm, 1.5nm, 2nm, 2.5nm, 3nm, 3.5nm, 4nm, 4.5nm, 5nm, 5.5nm or 6nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0117] In some embodiments, the growth conditions of the nitride quantum barrier layer include a temperature of 750-1200° C., a pressure of 100-500 torr, and a growth thickness of 3-15 nm. For example, the temperature can be 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable; the pressure can be 100torr, 150torr, 200torr, 250torr, 300torr, 350torr, 400torr, 450torr or 500torr, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable; the growth thickness of the nitride quantum barrier layer can be 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm or 15nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0118] In some embodiments, depositing the second nitride layer includes: growing the second nitride layer on the surface of the nitride light emitting layer under a seventh setting condition.

[0119] Further, the doping element in the second nitride layer may be Mg, and the seventh setting condition includes a temperature of 900-1100° C., a pressure of 100-500 torr, a growth thickness of the second nitride layer of 0.02-0.3 μm, and a doping concentration of (0.1-10)×10 20 cm -3 For example, the temperature may be 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, 1020°C, 1040°C, 1060°C, 1080°C or 1100°C, but is not limited to the values ​​listed, and other values ​​not listed within the numerical range are also applicable; the pressure may be 100 torr, 150 torr, 200 torr, 250 torr, 300 torr, 350 torr, 400 torr, 450 torr or 500 torr, but is not limited to the values ​​listed. The growth thickness of the second nitride layer can be 0.02 μm, 0.04 μm, 0.06 μm, 0.08 μm, 0.1 μm, 0.12 μm, 0.14 μm, 0.16 μm, 0.18 μm, 0.2 μm, 0.22 μm, 0.24 μm, 0.26 μm, 0.28 μm or 0.3 μm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; the doping concentration of the second nitride layer can be 0.1×10 20 cm -3 , 1×

[0120] 10 20 cm -3 , 2×10 20 cm -3 , 3×10 20 cm -3 , 4×10 20 cm -3 , 5×10 20 cm -3 , 6×10 20 cm -3 ,7×10 20 cm -3 , 8×10 20 cm -3 ,9×10 20 cm -3 or 10×10 20 cm -3 , but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0121] A certain embodiment of the present invention provides an application of a nitride LED epitaxial wafer, where the nitride LED epitaxial wafer is used to manufacture a semiconductor device.

[0122] Example 1

[0123] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. Figure 1 As shown, the nitride LED epitaxial wafer includes a stacked substrate 10, a composite buffer layer 20, a nitride buffer layer 30, a first nitride layer 41, a nitride light-emitting layer 50, and a second nitride layer 42. The composite buffer layer 20 includes a stacked nitride front layer 21, a composite structure layer 22, a nitride back layer 23, and a nitride capping layer 24, and the nitride front layer 21 is arranged on the surface of the substrate 10; the composite structure layer 22 has a nano-pattern structure for adjusting the lattice mismatch between the nitride front layer 21 and the nitride back layer 23.

[0124] The nitride front layer 21 is a SiN pattern structure layer. The composite structure layer 22 is an AlSiN composite structure layer, such as Figure 2As shown, the AlSiN composite structure layer includes a SiN structure layer 26, an AlN structure layer 27, and an AlN microstructure unit 29 and a SiN microstructure unit 28 that are arranged oppositely. Specifically, the AlN structure layer 27 is arranged between the SiN structure layer 26 and the nitride front layer 21; the AlN structure layer 27 is partially embedded in the nitride front layer 21; the SiN microstructure unit 28 presents a concave structure and is embedded in the AlN structure layer 27; the AlN microstructure unit 29 presents a convex structure and is embedded in the SiN structure layer 26. The longitudinal heights of the AlN microstructure unit 29 and the SiN microstructure unit 28 are 10 nm, respectively, and the radial dimensions are 5 nm, respectively.

[0125] In this embodiment, the nitride front layer 21 is penetrated by a nanopore 25, and the pore size of the nanopore 25 is 10 nm; the AlSiN composite structure layer includes a plurality of first AlSiN composite units 31 arranged in the nanopore 25, the first AlSiN composite unit 31 includes a SiN structure layer 26, an AlN structure layer 27, and relatively arranged AlN microstructure units 29 and SiN microstructure units 28, and the height of the first AlSiN composite unit 31 is less than the depth of the nanopore 25.

[0126] In this embodiment, the method for preparing the above-mentioned nitride LED epitaxial wafer includes the following steps:

[0127] D11. Provide a 4-inch sapphire substrate 10.

[0128] D12. Under the conditions of a temperature of 1115°C and a pressure of 200 torr, SiH4 with a flow rate of 200 sccm and NH3 with a flow rate of 50 slm are introduced to grow a SiN graphic structure layer with a thickness of 10 nm on the surface of the substrate 10 as a nitride prelayer 21.

[0129] D13 . Depositing a composite structure layer 22 on the nitride front layer 21 .

[0130] The deposition of the composite structure layer 22 comprises the following steps:

[0131] S11. In N2 atmosphere, TMAl was introduced at a flow rate of 150 sccm for 8 s for surface pretreatment.

[0132] S12. In N2 atmosphere, SiH4 is introduced at a flow rate of 200 sccm for surface pretreatment for 10 s.

[0133] S13. In N2 atmosphere, NH3 was introduced at a flow rate of 15 slm for surface pretreatment for 20 s.

[0134] S14, alternately repeating step S11 to step S13 20 times in total to obtain a composite structure layer 22 with a thickness of 10 nm.

[0135] D14. Under the conditions of a temperature of 850° C. and a pressure of 100 torr, a nitride rear layer 23 with a thickness of 30 nm is grown on the composite structure layer 22 .

[0136] The deposition of the nitride rear layer 23 comprises the following steps:

[0137] S21. In N2 atmosphere, TMAl with a flow rate of 240 sccm is introduced for surface treatment. The introduction time is 8 s, and an Al metal layer with a thickness of 3 nm is formed on the surface of the composite structure layer 22.

[0138] S22. Under N2 atmosphere, TMAl was introduced with a flow rate of 20 sccm for 18 s for surface treatment.

[0139] S23. Under N2 atmosphere, NH3 was introduced at a flow rate of 20 slm for surface treatment, and the introduction time was 10 s.

[0140] D15. Under the conditions of a temperature of 1125° C. and a pressure of 200 torr, a nitride capping layer 24 with a thickness of 70 nm and made of GaN is grown on the surface of the nitride rear layer 23 .

[0141] It is worth noting that, after steps D12 to D15 , a composite buffer layer 20 can be prepared.

[0142] D16. Under the conditions of a temperature of 1115° C. and a pressure of 150 torr, a nitride buffer layer 30 with a thickness of 2.5 μm and made of GaN is grown on the surface of the nitride cap layer 24 .

[0143] D17, under the conditions of temperature of 1050°C and pressure of 200 torr, a 2.5 μm thick GaN with Si doping concentration of 5×10 18 cm -3 The first nitride layer 41 is formed.

[0144] D18. Periodically grow a nitride quantum well layer and a nitride quantum barrier layer (not shown in the figure) on the surface of the first nitride layer 41 to form a nitride light emitting layer 50.

[0145] The material of the nitride quantum well layer is InGaN, and the growth conditions include temperature of 760°C, pressure of 300torr, and growth thickness of 3nm; the material of the nitride quantum barrier layer is GaN, and the growth conditions include temperature of 910°C, pressure of 300torr, and growth thickness of 9nm; the number of stacking groups of nitride quantum well layers and nitride quantum barrier layers is 10.

[0146] D19, under the conditions of temperature of 975°C and pressure of 200 torr, a 0.12 μm thick GaN material with a Mg doping concentration of 5×10 19 cm -3 The second nitride layer 42 is formed.

[0147] It is worth noting that, after steps D16-D19, a nitride LED epitaxial wafer can be prepared.

[0148] Example 2

[0149] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. Figure 1 As shown, the nitride LED epitaxial wafer includes a stacked substrate 10, a composite buffer layer 20, a nitride buffer layer 30, a first nitride layer 41, a nitride light-emitting layer 50, and a second nitride layer 42. The composite buffer layer 20 includes a stacked nitride front layer 21, a composite structure layer 22, a nitride back layer 23, and a nitride capping layer 24, and the nitride front layer 21 is disposed on the surface of the substrate 10; the composite structure layer 22 has a nano-pattern structure for adjusting the lattice mismatch between the nitride front layer 21 and the nitride back layer 23.

[0150] The nitride front layer 21 is a SiN pattern structure layer. The composite structure layer 22 is an AlSiN composite structure layer, such as Figure 3 As shown, the AlSiN composite structure layer includes a SiN structure layer 26, an AlN structure layer 27, and an AlN microstructure unit 29 and a SiN microstructure unit 28 that are arranged oppositely. Specifically, the AlN structure layer 27 is arranged between the SiN structure layer 26 and the nitride front layer 21; the AlN structure layer 27 is partially embedded in the nitride front layer 21; the SiN microstructure unit 28 presents a concave structure and is embedded in the AlN structure layer 27; the AlN microstructure unit 29 presents a convex structure and is embedded in the SiN structure layer 26. The longitudinal heights of the AlN microstructure unit 29 and the SiN microstructure unit 28 are 1 nm, respectively, and the radial dimensions are 20 nm, respectively.

[0151] In this embodiment, the nitride front layer 21 is penetrated by a nanopore 25, and the pore size of the nanopore 25 is 50 nm; the AlSiN composite structure layer includes a plurality of first AlSiN composite units 31 arranged in the nanopore 25, the first AlSiN composite unit 31 includes a SiN structure layer 26, an AlN structure layer 27, and relatively arranged AlN microstructure units 29 and SiN microstructure units 28, and the height of the first AlSiN composite unit 31 is equal to the depth of the nanopore 25.

[0152] In this embodiment, the method for preparing the above-mentioned nitride LED epitaxial wafer includes the following steps:

[0153] D11. Provide a 4-inch sapphire substrate 10.

[0154] D12. Under the conditions of a temperature of 1000°C and a pressure of 50 torr, SiH4 with a flow rate of 10 sccm and NH3 with a flow rate of 1 slm are introduced to grow a SiN graphic structure layer with a thickness of 5 nm on the surface of the substrate 10 as a nitride prelayer 21.

[0155] D13 . Depositing a composite structure layer 22 on the nitride front layer 21 .

[0156] The deposition of the composite structure layer 22 comprises the following steps:

[0157] S11. In N2 atmosphere, TMAl is introduced at a flow rate of 100 sccm for 2 s for surface pretreatment.

[0158] S12. In N2 atmosphere, SiH4 was introduced at a flow rate of 10 sccm for surface pretreatment for 5 s.

[0159] S13. In N2 atmosphere, NH3 with a flow rate of 1 slm was introduced for surface pretreatment, and the introduction time was 10 s.

[0160] S14, alternately repeating step S11 to step S13 once in total, to obtain a composite structure layer 22 with a thickness of 2 nm.

[0161] D14. Under the conditions of a temperature of 650° C. and a pressure of 50 torr, a nitride rear layer 23 with a thickness of 10 nm is grown on the composite structure layer 22 .

[0162] The deposition of the nitride rear layer 23 comprises:

[0163] S21. In N2 atmosphere, TMAl is introduced at a flow rate of 100 sccm for surface treatment for 2 seconds to form an Al metal layer with a thickness of 2 nm on the surface of the composite structure layer 22.

[0164] S22. In N2 atmosphere, TMAl is introduced at a flow rate of 5 sccm for surface treatment for 5 s.

[0165] S23. Under N2 atmosphere, NH3 with a flow rate of 5 slm is introduced for surface treatment, and the introduction time is 5 s.

[0166] D15. Under the conditions of a temperature of 1050° C. and a pressure of 100 torr, a nitride capping layer 24 with a thickness of 20 nm and made of GaN is grown on the surface of the nitride rear layer 23 .

[0167] It is worth noting that, after steps D12 to D15 , a composite buffer layer 20 can be prepared.

[0168] D16. Under the conditions of a temperature of 1050° C. and a pressure of 100 torr, a nitride buffer layer 30 with a thickness of 0.1 μm and made of GaN is grown on the surface of the nitride cap layer 24 .

[0169] D17, under the conditions of temperature of 1000°C and pressure of 100 torr, a 0.5 μm thick GaN material with Si doping concentration of 1×10 18 cm -3 The first nitride layer 41 is formed.

[0170] D18. Periodically grow a nitride quantum well layer and a nitride quantum barrier layer (not shown in the figure) on the surface of the first nitride layer 41 to form a nitride light emitting layer 50.

[0171] The material of the nitride quantum well layer is InGaN, and the growth conditions include a temperature of 700°C, a pressure of 100torr, and a growth thickness of 1nm; the material of the nitride quantum barrier layer is GaN, and the growth conditions include a temperature of 750°C, a pressure of 100torr, and a growth thickness of 3nm; the number of stacked groups of nitride quantum well layers and nitride quantum barrier layers is 15.

[0172] D19, under the conditions of temperature of 900°C and pressure of 100 torr, a 0.02 μm thick GaN material with a Mg doping concentration of 0.1×10 20 cm -3 The second nitride layer 42 is formed.

[0173] It is worth noting that, after steps D16-D19, a nitride LED epitaxial wafer can be prepared.

[0174] Example 3

[0175] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. Figure 1As shown, the nitride LED epitaxial wafer includes a stacked substrate 10, a composite buffer layer 20, a nitride buffer layer 30, a first nitride layer 41, a nitride light-emitting layer 50, and a second nitride layer 42. The composite buffer layer 20 includes a stacked nitride front layer 21, a composite structure layer 22, a nitride back layer 23, and a nitride capping layer 24, and the nitride front layer 21 is disposed on the surface of the substrate 10; the composite structure layer 22 has a nano-pattern structure for adjusting the lattice mismatch between the nitride front layer 21 and the nitride back layer 23.

[0176] The nitride front layer 21 is a SiN pattern structure layer. The composite structure layer 22 is an AlSiN composite structure layer, such as Figure 4 As shown, the AlSiN composite structure layer includes a SiN structure layer 26, an AlN structure layer 27, and an AlN microstructure unit 29 and a SiN microstructure unit 28 that are arranged oppositely. Specifically, the AlN structure layer 27 is arranged between the SiN structure layer 26 and the nitride front layer 21; the AlN structure layer 27 is partially embedded in the nitride front layer 21; the SiN microstructure unit 28 presents a concave structure and is embedded in the AlN structure layer 27; the AlN microstructure unit 29 presents a convex structure and is embedded in the SiN structure layer 26. The longitudinal heights of the AlN microstructure unit 29 and the SiN microstructure unit 28 are 20 nm, respectively, and the radial dimensions are 120 nm, respectively.

[0177] In this embodiment, the nitride front layer 21 is penetrated by a nanopore 25, and the pore size of the nanopore 25 is 150 nm; the AlSiN composite structure layer includes a plurality of second AlSiN composite units 32 arranged in the nanopore 25 and a SiN structure layer 26 arranged on the second AlSiN composite unit 32, and the second AlSiN composite unit 32 includes an AlN structure layer 27 and relatively arranged AlN microstructure units 29 and SiN microstructure units 28.

[0178] In this embodiment, the method for preparing the above-mentioned nitride LED epitaxial wafer includes the following steps:

[0179] D11. Provide a 4-inch sapphire substrate 10.

[0180] D12. Under the conditions of a temperature of 1200° C. and a pressure of 500 torr, SiH 4 with a flow rate of 300 sccm and NH 3 with a flow rate of 100 slm are introduced to grow a SiN graphic structure layer with a thickness of 15 nm on the surface of the substrate 10 .

[0181] D13 . Depositing a composite structure layer 22 on the nitride front layer 21 .

[0182] The deposition of the composite structure layer 22 comprises the following steps:

[0183] S11. In N2 atmosphere, TMAl was introduced at a flow rate of 300 sccm for 15 s for surface pretreatment.

[0184] S12. In N2 atmosphere, SiH4 is introduced at a flow rate of 300 sccm for 20 s for surface pretreatment.

[0185] S13. In N2 atmosphere, NH3 is introduced at a flow rate of 25 slm for surface pretreatment, and the introduction time is 30 s.

[0186] S14, alternately repeating step S11 to step S13 for 50 times in total, to obtain a composite structure layer 22 with a thickness of 200 nm.

[0187] D14. Under the conditions of a temperature of 950° C. and a pressure of 500 torr, a nitride rear layer 23 with a thickness of 200 nm is grown on the composite structure layer 22 .

[0188] The deposition of the nitride rear layer 23 comprises:

[0189] S21. In N2 atmosphere, TMAl is introduced at a flow rate of 300 sccm for surface treatment for 10 s to form an Al metal layer with a thickness of 50 nm on the surface of the composite structure layer 22.

[0190] S22. In N2 atmosphere, TMAl is introduced at a flow rate of 100 sccm for surface treatment for 20 s.

[0191] S23. Under N2 atmosphere, NH3 with a flow rate of 50 slm is introduced for surface treatment, and the introduction time is 20 s.

[0192] D15. Under the conditions of a temperature of 1250° C. and a pressure of 500 torr, a nitride capping layer 24 with a thickness of 100 nm and made of GaN is grown on the surface of the nitride rear layer 23 .

[0193] It is worth noting that, after steps D12 to D15 , a composite buffer layer 20 can be prepared.

[0194] D16. Under the conditions of a temperature of 1150° C. and a pressure of 500 torr, a nitride buffer layer 30 with a thickness of 3 μm and made of GaN is grown on the surface of the nitride cap layer 24 .

[0195] D17, under the conditions of temperature of 1100°C and pressure of 500 torr, a 10 μm thick GaN-doped Si layer 30 is grown on the surface of the nitride buffer layer 30. 18 cm -3 The first nitride layer 41 is formed.

[0196] D18. Periodically grow a nitride quantum well layer and a nitride quantum barrier layer (not shown in the figure) on the surface of the first nitride layer 41 to form a nitride light emitting layer 50.

[0197] The material of the nitride quantum well layer is InGaN, and the growth conditions include temperature of 1150°C, pressure of 500torr, and growth thickness of 6nm; the material of the nitride quantum barrier layer is GaN, and the growth conditions include temperature of 1200°C, pressure of 500torr, and growth thickness of 15nm; the number of stacking groups of nitride quantum well layer and nitride quantum barrier layer is 2.

[0198] D19, under the conditions of temperature of 1100°C and pressure of 500 torr, a 0.3 μm thick GaN material with Mg doping concentration of 10×10 20 cm -3 The second nitride layer 42 is formed.

[0199] It is worth noting that, after steps D16-D19, a nitride LED epitaxial wafer can be prepared.

[0200] Example 4

[0201] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. In addition to controlling the growth conditions of the composite structure layer 22 to change the longitudinal heights of the AlN microstructure unit 29 and the SiN microstructure unit 28 to 0.5 nm respectively, the remaining steps and conditions are the same as those in Embodiment 1 and will not be described in detail here.

[0202] Example 5

[0203] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. In addition to controlling the growth conditions of the composite structure layer 22 and changing the longitudinal heights of the AlN microstructure unit 29 and the SiN microstructure unit 28 to 25 nm respectively, the remaining steps and conditions are the same as those in Embodiment 1 and are not described in detail here.

[0204] Example 6

[0205] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. In addition to controlling the growth conditions of the composite structure layer 22 to change the radial dimensions of the AlN microstructure unit 29 and the SiN microstructure unit 28 to 2 nm, the remaining steps and conditions are the same as those in Embodiment 1 and will not be described in detail herein.

[0206] Example 7

[0207] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. In addition to controlling the growth conditions of the composite structure layer 22 to change the radial dimensions of the AlN microstructure unit 29 and the SiN microstructure unit 28 to 160 nm respectively, the remaining steps and conditions are the same as those in Embodiment 1 and are not described in detail here.

[0208] Example 8

[0209] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. Except for controlling the growth conditions of the nitride front layer 21 and the composite structure layer 22 to remove the nanopores 25, the remaining steps and conditions are the same as those in Embodiment 1 and are not described in detail here.

[0210] Example 9

[0211] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. Except that the number of repetitions of step S11 to step S13 is changed to 1, the remaining steps and conditions are the same as those in embodiment 1, and thus will not be described in detail here.

[0212] Comparative Example 1

[0213] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. Except for removing the composite structure layer 22, that is, directly setting the nitride rear layer 23 on the surface of the nitride front layer 21, the remaining steps and conditions are the same as those in Example 1, so they are not repeated here.

[0214] Comparative Example 2

[0215] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. Except for removing the nitride front layer 21 and the nitride rear layer 23, that is, only a composite structure layer 22 is provided between the substrate 10 and the nitride covering layer 24, the remaining steps and conditions are the same as those in Embodiment 1, and thus are not described in detail here.

[0216] Comparative Example 3

[0217] This embodiment provides a nitride LED epitaxial wafer and a method for preparing the same. Except for removing the nitride capping layer 24, that is, directly setting a nitride buffer layer 30 on the surface of the nitride rear layer 23, the remaining steps and conditions are the same as those in Embodiment 1, so they are not described here in detail.

[0218] Performance Testing

[0219] The nitride LED epitaxial wafers obtained in Examples 1-9 and Comparative Examples 1-3 were tested for luminous performance at a wavelength of 460±1 nm, and the uniformity of the wavelength of the nitride LED epitaxial wafer was tested by photoluminescence spectrum scanning and recorded as std, and the half-peak width of the (102) crystal plane diffraction peak was tested by an X-ray diffractometer and recorded as Y1 / 2, and then a chip with a size of 3mil×5mil was prepared, and the brightness, luminous efficiency and leakage performance were tested by a chip spot tester. The relevant test results are shown in Table 1 below.

[0220] Table 1

[0221]

[0222]

[0223] From Table 1, we can see that:

[0224] 1) The nitride LED epitaxial wafers obtained in Examples 1-3 have excellent wavelength uniformity, lower (102) crystal plane half-width, higher leakage yield and luminous efficiency, indicating that the present invention utilizes the patterning effect of the composite structure layer to promote the full redirection of dislocations in the epitaxial wafer during the growth process, thereby improving the crystal quality, while enhancing the reflection of light in the nitride light-emitting layer toward the substrate, thereby improving the light extraction efficiency. In addition, the composite structure layer adjusts the lattice mismatch between the nitride front layer and the nitride back layer, thereby alleviating the epitaxial wafer stress caused by the nitride graphic structure, reducing the stress in the nitride light-emitting layer, alleviating the stress-pulling effect caused by the component differences in the nitride light-emitting layer, and improving the component incorporation and distribution uniformity in the nitride light-emitting layer.

[0225] 2) The wavelength uniformity of the nitride LEDs obtained in Example 4 and Example 6 deteriorates slightly, and the half-width of the (102) crystal plane also tends to increase. The leakage yield performance and the luminous efficiency are reduced to a certain extent, indicating that the longitudinal height of the AlN microstructure unit and the SiN microstructure unit is too low or the radial size is too small, and it is difficult to relax the stress well through the interaction between the microstructure units. Therefore, the effect of promoting the full rotation of dislocations in the growth process of the epitaxial wafer is also weakened to a certain extent.

[0226] 3) The wavelength uniformity of the nitride LEDs obtained in Examples 5 and 7 deteriorates slightly, and the half-width of the (102) crystal plane also tends to increase. The leakage yield performance and the luminous efficiency are reduced to a certain extent, indicating that the longitudinal height of the AlN microstructure unit and the SiN microstructure unit is too high or the radial size is too large. Due to the interaction between the microstructure units during the process growth, the stress relaxation effect is also insufficient.

[0227] 4) The wavelength uniformity of the nitride LEDs obtained in Examples 8 and 9 deteriorates slightly, and the (102) crystal plane half-width also tends to increase. The leakage yield performance and luminous efficiency are both reduced to a certain extent. The reason is that Example 8 does not set nanopores, and cannot use the nanopores to restrict atoms in the nano-region during the surface treatment of the composite buffer layer, which increases the unevenness of atomic distribution and further causes uneven stress distribution in the epitaxial wafer. In Example 9, the atomic surface treatment in the epitaxial wafer composite structure layer process is all at nanoscale. Due to the cyclic process, the stress can be released through longitudinal relaxation during the cycle, while Example 9 cannot reflect this stress release effect.

[0228] 5) The wavelength uniformity, (102) crystal plane half-width, leakage yield performance and luminous efficiency of the nitride LEDs obtained in Comparative Examples 1-3 are greatly reduced; Comparative Example 1 does not have the patterning effect of the composite structure layer, and Comparative Example 2 does not have a nitride back layer to provide a lattice transition for the nitride covering layer, which also causes an increase in stress in the epitaxial wafer, and Comparative Example 3 does not have a nitride covering layer as a lattice-matched low-defect growth template.

[0229] In summary, the present invention promotes the full redirection of dislocations in the growth process of the epitaxial wafer through the patterning effect of the composite structure layer, thereby improving the crystal quality, and at the same time intensifies the reflection of light in the nitride light-emitting layer toward the substrate, thereby improving the light extraction efficiency.

[0230] In addition, the composite structure layer adjusts the lattice mismatch between the nitride front layer and the nitride back layer, alleviates the epitaxial wafer stress caused by the nitride graphic structure, reduces the stress in the nitride light-emitting layer, alleviates the stress pulling effect caused by the component difference in the nitride light-emitting layer, and improves the component incorporation in the nitride light-emitting layer. The nitride light-emitting layer can be grown at a relatively high temperature, thereby improving the crystal quality of the nitride light-emitting layer, and improving the luminescence efficiency and brightness of the epitaxial wafer.

[0231] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A nitride LED epitaxial wafer, characterized in that: The nitride LED epitaxial wafer comprises a stacked substrate, a composite buffer layer, a nitride buffer layer, a first nitride layer, a nitride light-emitting layer and a second nitride layer; Among them, the composite buffer layer includes a stacked nitride front layer, a composite structure layer, a nitride rear layer and a nitride covering layer, and the nitride front layer is arranged on the surface of the substrate; the composite structure layer has a nano-pattern structure for adjusting the lattice mismatch between the nitride front layer and the nitride rear layer.

2. The nitride LED epitaxial wafer according to claim 1, characterized in that: The composite structure layer is an AlSiN composite structure layer, comprising a SiN structure layer, an AlN structure layer, and AlN microstructure units and SiN microstructure units arranged relatively; Wherein, the AlN structural layer is arranged between the SiN structural layer and the nitride front layer; the AlN structural layer is at least partially embedded in the nitride front layer; the AlN microstructure unit presents a convex structure and is embedded in the SiN structural layer; the SiN microstructure unit presents a concave structure and is embedded in the AlN structural layer; Preferably, the longitudinal heights of the AlN microstructure unit and the SiN microstructure unit are 1-20 nm respectively; Preferably, radial dimensions of the AlN microstructure unit and the SiN microstructure unit are 5-150 nm respectively.

3. The nitride LED epitaxial wafer according to claim 2, characterized in that: The nitride front layer has nanopores running through it; The AlSiN composite structure layer includes at least two first AlSiN composite units disposed in the nanopore, the first AlSiN composite unit includes a SiN structure layer, an AlN structure layer, and an AlN microstructure unit and a SiN microstructure unit disposed oppositely, and the height of the first AlSiN composite unit is less than or equal to the depth of the nanopore; Alternatively, the AlSiN composite structure layer includes at least two second AlSiN composite units disposed in the nanopores and a SiN structure layer disposed on the second AlSiN composite unit, wherein the second AlSiN composite unit includes an AlN structure layer and an AlN microstructure unit and a SiN microstructure unit disposed oppositely; Preferably, the pore size of the nanopore is 5-150 nm.

4. A method for preparing a nitride LED epitaxial wafer according to any one of claims 1 to 3, characterized in that: The preparation method comprises: providing a substrate; Depositing a nitride front layer, a composite structure layer, a nitride rear layer and a nitride capping layer in sequence on the surface of the substrate to form a composite buffer layer; A nitride buffer layer, a first nitride layer, a nitride light-emitting layer and a second nitride layer are sequentially deposited on the surface of the composite buffer layer to obtain the nitride LED epitaxial wafer.

5. The method for preparing a nitride LED epitaxial wafer according to claim 4, characterized in that: The deposition of the composite structure layer comprises: S11, in an inert gas atmosphere, introducing an Al source for surface pretreatment, wherein the flow rate of the Al source is 100-300 sccm and the introduction time is 2-15 s; S12, in an inert gas atmosphere, introducing a Si source for surface pretreatment, wherein the flow rate of the Si source is 10-300 sccm and the introduction time is 5-20 s; S13, in an inert gas atmosphere, introducing a N source for surface pretreatment, wherein the flow rate of the N source is 1-25 slm and the introduction time is 10-30 s; S14, alternately and repeatedly performing steps S11 to S13 to obtain the composite structure layer; Wherein, the number of repetitions of step S11 to step S13 is 1-50 times, and the thickness of the composite structure layer is 2-100 nm.

6. The method for preparing a nitride LED epitaxial wafer according to claim 4, characterized in that: The deposition of the nitride rear layer comprises: S21, under the second setting condition, introducing a first flow rate of Al source for surface treatment, wherein the first flow rate is 100-300 sccm, and the introduction time of the first flow rate of Al source is 2-10 s; S22, under the second setting condition, introducing a second flow rate of Al source for surface treatment, wherein the second flow rate is 5-100 sccm, and the introduction time of the second flow rate of Al source is 5-20 s; S23, under the second setting condition, introducing a N source for surface treatment, wherein the flow rate of the N source is 5-50 slm and the introduction time is 5-20 s; The second setting conditions include a temperature of 650-950° C., a pressure of 50-500 torr, and a growth thickness of 10-50 nm.

7. The method for preparing a nitride LED epitaxial wafer according to claim 4, characterized in that: The nitride front layer is a SiN pattern structure layer, and the deposition of the nitride front layer includes: Under the first set conditions, Si source and N source are introduced to grow the SiN graphic structure layer on the surface of the substrate; wherein the first set conditions include a temperature of 1000-1200°C, a pressure of 50-500torr, a flow rate of the Si source of 10-300sccm, a flow rate of the N source of 1-100slm, and a growth thickness of 5-50nm.

8. The method for preparing a nitride LED epitaxial wafer according to claim 4, characterized in that: The deposition of the nitride capping layer comprises: Under the third setting condition, the nitride capping layer is grown on the surface of the nitride rear layer; wherein the third setting condition includes a temperature of 1050-1250° C., a pressure of 100-500 torr, and a growth thickness of 20-100 nm; And / or, the deposition of the nitride buffer layer comprises: Under the fourth setting condition, the nitride buffer layer is grown on the surface of the nitride capping layer; wherein the fourth setting condition includes a temperature of 1050-1150° C., a pressure of 100-500 torr, and a growth thickness of 0.1-3 μm; And / or, the depositing of the first nitride layer comprises: Under the fifth setting condition, the first nitride layer is grown on the surface of the nitride buffer layer; wherein the fifth setting condition includes a temperature of 1000-1100° C., a pressure of 100-500 torr, a growth thickness of 0.5-10 μm, and a doping concentration of (1-8)×10 18 cm -3 .

9. The method for preparing a nitride LED epitaxial wafer according to claim 4, characterized in that: The deposition of the nitride light emitting layer comprises: Under the sixth setting condition, a nitride quantum well layer and a nitride quantum barrier layer are periodically grown on the surface of the first nitride layer to form the nitride light-emitting layer; wherein the sixth setting condition includes a temperature of 700-1200° C. and a pressure of 100-500 torr; Preferably, the growth conditions of the nitride quantum well layer include a temperature of 700-1150° C., a pressure of 100-500 torr, and a growth thickness of 1-6 nm; Preferably, the growth conditions of the nitride quantum barrier layer include a temperature of 750-1200° C., a pressure of 100-500 torr, and a growth thickness of 3-15 nm; Preferably, the number of stacked groups of the nitride quantum well layer and the nitride quantum barrier layer is 2-15 groups; And / or, the depositing of the second nitride layer comprises: Under the seventh setting condition, the second nitride layer is grown on the surface of the nitride light-emitting layer; wherein the seventh setting condition includes a temperature of 900-1100° C., a pressure of 100-500 torr, a growth thickness of 0.02-0.3 μm, and a doping concentration of (0.1-10)×10 20 cm -3 .

10. An application of the nitride LED epitaxial wafer according to any one of claims 1 to 3, characterized in that: The nitride LED epitaxial wafer is used for manufacturing semiconductor devices.

Citation Information

Patent Citations

  • Epitaxial structure layer, preparation method thereof and LED chip

    CN115000260A

  • Epitaxial wafer and preparation method thereof

    CN117954537A

  • Nitride epitaxial wafer, preparation method thereof and semiconductor device

    CN118173679A

  • Silica -based gallium nitride power device