Preparation method of halide solid electrolyte, preparation method of solid-state battery pole piece and solid-state battery
By using a liquid-phase preparation method of halide solid electrolytes in lithium batteries, the safety issues of the lithium metal deposition process and the complexity of solid electrolyte synthesis in lithium batteries are solved, and solid-state batteries with high energy density and safety are realized and simplified Simplify the preparation process and improve electrochemical performance.
Patent Information
- Application Number
- CN202310315358.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
The unstable deposition process and dendrite growth of lithium metal in traditional lithium batteries lead to safety issues, and the existing solid electrolyte synthesis methods are complex and have low connection strength, making it difficult to ensure the high energy density and safety of the battery.
The liquid-phase preparation method of halide solid electrolytes is adopted, by mixing transition metals or rare earth elements and halogens in organic solvents to form a reaction solution and drying, to obtain a solid electrolyte with uniform particle size and high ionic conductivity, and in the solid-state battery electrode The solid electrolyte layer is formed in situ on the chip, which simplifies the preparation process and improves the mechanical properties.
It achieves the safety and high energy density of lithium batteries, simplifies the battery pole piece preparation process, reduces energy consumption, and improves the electrochemical performance and industrial production potential of solid-state batteries.
Smart Images

Figure BDA0004151100910000091 
Figure BDA0004151100910000101 
Figure BDA0004151100910000111
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a liquid phase preparation method of a halide solid electrolyte, a solid-state battery pole piece preparation method and a solid-state battery. Background Art
[0002] With the rapid development of electric vehicles, high-energy-density lithium metal batteries have attracted increasing attention. However, the unstable deposition process and dendrite growth of lithium metal in traditional liquid electrolytes can cause a series of safety issues, which seriously hinders the development of lithium metal anodes.
[0003] Compared with liquid electrolytes, the non-flammability of solid electrolytes can perfectly solve the safety problems of lithium batteries, and can match lithium metal negative electrodes with high-voltage positive electrodes to make all-solid-state lithium batteries (ASSLBs) with higher energy density. The development of solid electrolytes is one of the most critical steps for ASSLBS.
[0004] Conventional solid electrolyte synthesis methods include high-energy ball milling and aqueous phase synthesis. Among them, the high-energy ball milling method is simple, but the reaction degree cannot be quantified, and there may be unreacted reactants that affect the battery ion conductivity; the aqueous phase method uses ammonium chloride to form a complex with chloride, mixes the reactants in the aqueous phase, and then dries and calcines, but the calcination process is prone to cause changes in the crystal form.
[0005] A major problem facing all-solid-state batteries is the preparation process of the battery solid electrolyte layer. The existing slurry method requires transfer printing or coating a layer of solid electrolyte on the surface of the electrode, which is a complicated process and has low connection strength. The powder compaction method has problems such as difficulty in ensuring strength. Summary of the invention
[0006] In view of this, one of the technical problems to be solved by the present invention is to provide a liquid phase preparation method of a halide solid electrolyte, wherein the halide solid electrolyte obtained by the method has uniform particle size and high ionic conductivity.
[0007] The second technical problem to be solved by the present invention is to provide a solid-state battery pole piece, a preparation method thereof and a solid-state battery. The preparation method of the solid-state battery pole piece is simple and has good mechanical properties.
[0008] The present invention provides a liquid phase preparation method of a halide solid electrolyte, comprising:
[0009] S1) MX a mixing with a first organic solvent to obtain a first reaction solution;
[0010] mixing LiX with a second organic solvent to obtain a second reaction solution;
[0011] M is selected from transition metal elements or rare earth elements; X is a halogen; a is a coordination valence;
[0012] S2) mixing the first reaction solution and the second reaction solution, and drying to obtain a halide solid electrolyte.
[0013] Preferably, the M is selected from one or more of Sc, Y, In, Ga, La, Zr and Ti; the X is selected from one or more of F, Cl, Br and I; the first organic solvent and the second organic solvent are each independently selected from one or more of dimethyl sulfoxide, tetrahydropyran, tetrahydrofuran, anisole, amino ethers, halogenated ethers, hydroxy ethers, 2,3-dimethyltetrahydrofuran, 2,5-dimethyltetrahydrofuran and fluorinated tetrahydropyran, toluene, xylene, carbon tetrachloride, and ethyl acetate.
[0014] Preferably, the MX a The molar ratio of LiX to the first organic solvent is 1:(15-25); the molar ratio of LiX to the second organic solvent is 1:(7-15);
[0015] The mass ratio of the first reaction solution to the second reaction solution is 1:(1-5).
[0016] Preferably, the mixing in step S2) is stirring mixing, and the mixing speed is 100 to 1000 r / min;
[0017] The drying temperature is 50° C. to 300° C.; the drying time is 0.5 to 5 hours.
[0018] The present invention also provides a halide solid electrolyte prepared by the above preparation method.
[0019] The present invention also provides a method for preparing a solid-state battery electrode, comprising the following steps:
[0020] A1) MX a mixing with a first organic solvent to obtain a first reaction solution;
[0021] Mixing LiX with a second organic solvent to obtain a second reaction solution; M is selected from transition metal elements or rare earth elements; X is a halogen; a is a coordination valence;
[0022] Mixing the positive electrode material, the conductive agent and the binder in a third organic solvent to obtain a positive electrode slurry;
[0023] Applying the positive electrode slurry on the positive electrode current collector to obtain a positive electrode sheet;
[0024] A2) After mixing the first reaction solution and the second reaction solution, immersing the mixture into a positive electrode plate, taking it out and drying it to obtain a solid-state battery plate.
[0025] Preferably, the positive electrode material is selected from one or more of nickel-cobalt-manganese ternary positive electrode materials, lithium iron phosphate, lithium-rich manganese-based materials and lithium cobalt oxide;
[0026] The conductive agent is selected from one or more of conductive carbon black, nanocarbon fiber and Ketjen black;
[0027] The binder is selected from one or more of styrene-butadiene rubber, tetrafluoroethylene rubber and silicone rubber;
[0028] The positive electrode current collector is selected from aluminum foil, carbon-coated aluminum foil or microporous aluminum foil;
[0029] The third organic solvent is selected from N-methylpyrrolidone and / or dimethyl sulfoxide;
[0030] The molar ratio of the positive electrode material to the third organic solvent in the positive electrode slurry is 1:(10-25);
[0031] The positive electrode slurry is coated to a thickness of 5 to 500 μm.
[0032] Preferably, the mixing in step A2) is stirring mixing, and the mixing speed is 100-1000 r / min; the immersion time is 0.1-120 min; the drying temperature is 50° C.-150° C.;
[0033] The immersing and drying steps in step A2) are repeated 1 to 10 times, and the solid-state battery electrode is obtained after being taken out and dried.
[0034] The present invention also provides a solid-state battery electrode prepared by the above preparation method.
[0035] The present invention also provides a solid-state battery, comprising a solid-state battery pole piece prepared by the above preparation method;
[0036] Also includes a negative electrode plate;
[0037] The negative electrode plate comprises a negative electrode active material and a negative electrode current collector;
[0038] The negative electrode active material is selected from any one of metallic lithium, pure silicon negative electrode material, silicon-carbon negative electrode material, and silicon-oxygen negative electrode material;
[0039] The negative electrode current collector is selected from copper foil, carbon-coated copper foil or microporous copper foil.
[0040] The present invention provides a liquid phase preparation method of a halide solid electrolyte, comprising: S1) preparing MN xMix with a first organic solvent to obtain a first reaction solution; mix LiN with a second organic solvent to obtain a second reaction solution; M is selected from transition metal elements or rare earth elements; N is a halogen; a is a coordination valence; S2) After the first reaction solution and the second reaction solution are mixed, they are dried to obtain a halide solid electrolyte. The present invention uses a weak polar solvent to form a reaction solution with a lithium salt and a halide respectively, and then mixes them under liquid phase conditions for complexation, and dries to obtain a solid electrolyte. Compared with the prior art, the electrolyte prepared by this method has uniform particle size, high ionic conductivity, and does not require ball milling after being applied to the battery, which reduces energy consumption and can be mass-produced industrially.
[0041] The present invention also provides a method for preparing a solid-state battery electrode, comprising the following steps: A1) a Mixing with a first organic solvent to obtain a first reaction solution; mixing LiN with a second organic solvent to obtain a second reaction solution; M is selected from transition metal elements or rare earth elements; X is a halogen; a is a coordination valence; mixing the positive electrode material, the conductive agent and the binder in a third organic solvent to obtain a positive electrode slurry; coating the positive electrode slurry on the positive electrode collector to obtain a positive electrode plate; A2) mixing the first reaction solution with the second reaction solution, immersing the positive electrode plate, taking out and drying to obtain a solid-state battery plate. Compared with the prior art, the method for preparing the plate of the present invention does not require the addition of a solid electrolyte. After mixing the two reaction solutions, immersing the positive electrode plate, and forming a solid electrolyte layer in situ on the surface of the original plate layer through reaction, so that the interface of the obtained solid-state battery plate is more solid. DETAILED DESCRIPTION
[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0043] The present invention provides a liquid phase preparation method of a halide solid electrolyte, comprising: S1) preparing MX a Mixing with a first organic solvent to obtain a first reaction solution; mixing LiX with a second organic solvent to obtain a second reaction solution; M is selected from transition metal elements or rare earth elements; X is a halogen; a is a coordination valence; S2) After mixing the first reaction solution and the second reaction solution, drying them to obtain a halide solid electrolyte.
[0044] The present invention has no particular limitation on the sources of all raw materials, and any raw materials available on the market can be used.
[0045] MX aand a first organic solvent to obtain a first reaction solution; the M is preferably one or more of Sc, Y, In, Ga, La, Zr and Ti; the X is preferably one or more of F, Cl, Br and I; a is a coordination valence; the first organic solvent is preferably one or more of dimethyl sulfoxide, tetrahydropyran, tetrahydrofuran, anisole, amino ethers, halogenated ethers, hydroxy ethers, 2,3-dimethyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, fluorinated tetrahydropyran, toluene, xylene, carbon tetrachloride, ethyl acetate; the MX a The molar ratio to the first organic solvent is preferably 1:(15-25), more preferably 1:(18-22), and even more preferably 1:20.
[0046] LiX is mixed with a second organic solvent to obtain a second reaction solution; the second organic solvent is preferably one or more of dimethyl sulfoxide, tetrahydropyran, tetrahydrofuran, anisole, amino ethers, halogenated ethers, hydroxy ethers, 2,3-dimethyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, fluorinated tetrahydropyran, toluene, xylene, carbon tetrachloride, and ethyl acetate; the molar ratio of LiX to the second organic solvent is preferably 1:(7-15), more preferably 1:(8-12), more preferably 1:(9-11), and most preferably 1:10.
[0047] The solvent has a great influence on the synthesis process of solid electrolytes and the microstructure of solid electrolytes. The solid electrolyte (SA) prepared with acetone and acetonitrile as a mixed solvent has a dense surface and the lowest crystallinity, while the solid electrolyte (SN) prepared with N-methylpyrrolidone (NMP) and acetonitrile as a mixed solvent has the highest crystallinity. The microstructure of the solid electrolyte directly determines its mechanical and electrochemical properties. The type of solvent affects the surface flatness and structural uniformity of the solid electrolyte. The selection of solvents for dissolving solid electrolytes should be comprehensively considered from the perspectives of solubility, viscosity, evaporation rate, safety of the solvent, and side reactions. For example, if NMP, water, etc. are used for sulfide solid electrolytes, serious side reactions will occur, and the conductivity will drop by several orders of magnitude. The use of low-polarity solvents cannot dissolve binders such as PVDF and PAA. The use of high-polarity solvents such as aqueous solvents is unstable with solid electrolytes. Low-polarity solvents can only dissolve very few low-molecular-weight binders. Borohydride solid electrolytes contain LiBH4, which is easily decomposed when exposed to water, so they cannot be dissolved in water and the water content in the solvent must be strictly controlled.
[0048] The first reaction solution is mixed with the second reaction solution; the mass ratio of the first reaction solution to the second reaction solution is preferably 1:(1-5), more preferably 1:(1.5-3), further preferably 1:(1.5-2.5), and most preferably 1:(1.7-2.5); in the embodiments provided by the present invention, the mass ratio of the first reaction solution to the second reaction solution is specifically 1:1.7, 1:1.72, 1:1.9, 1:2.5 or 1:2.4; the mixing rotation speed is preferably 100-1000r / min.
[0049] After mixing, drying is performed to obtain a halide solid electrolyte; the drying temperature is preferably 50°C to 300°C, more preferably 60°C to 250°C, and more preferably 60°C to 200°C; in the embodiment provided by the present invention, the drying temperature is specifically 60°C, 100°C, 200°C or 150°C; the drying time is preferably 0.5 to 5h. The lower drying temperature of the solid electrolyte has little effect on the product performance, but the product is sintered when it is greater than 200°C, and the sintering has a greater impact on the product. The solvent evaporates at a higher temperature, which will produce side reactions and solvent foaming, and the solid electrolyte cannot be precipitated uniformly and densely. At different sintering temperatures, the ionic conductivity of the solid electrolyte is different. The closer to the glass transition temperature of the solid electrolyte, the more amorphous areas in the electrolyte increase, which can provide channels for the movement of lithium ions, so that the conductivity of the solid electrolyte increases sharply.
[0050] The present invention adopts a solid electrolyte that can be complexed with halides to prepare the solid electrolyte under liquid phase conditions. The electrolyte prepared by the method has uniform particle size and high ionic conductivity, and does not require ball milling after being applied to batteries, thereby reducing energy consumption.
[0051] The present invention also provides a halide solid electrolyte prepared by the method.
[0052] The present invention also provides a method for preparing a solid-state battery electrode, comprising the following steps: A1) a A2) mixing LiX with a first organic solvent to obtain a first reaction solution; mixing LiX with a second organic solvent to obtain a second reaction solution; M is selected from transition metal elements or rare earth elements; X is a halogen; a is a coordination valence; mixing the positive electrode material, the conductive agent and the binder in a third organic solvent to obtain a positive electrode slurry; coating the positive electrode slurry on the positive electrode collector to obtain a positive electrode plate; A3) mixing the first reaction solution with the second reaction solution, immersing the positive electrode plate, taking out and drying to obtain a solid-state battery plate.
[0053] The preparation of the first reaction solution and the second reaction solution are the same as described above and will not be repeated here.
[0054] The positive electrode material, the conductive agent and the binder are mixed in a third organic solvent to obtain a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector to obtain a positive electrode plate; the positive electrode material is preferably one or more of a nickel-cobalt-manganese ternary positive electrode material, lithium iron phosphate, a lithium-rich manganese-based material and lithium cobalt oxide; the nickel-cobalt-manganese ternary positive electrode material is preferably one or more of ternary 622, ternary Ni83 and ternary Ni90; the conductive agent is preferably one or more of conductive carbon black, nano-carbon fiber and Ketjen black; the binder is preferably one or more of styrene-butadiene rubber, tetrapropylene rubber and silicone rubber; the third organic solvent is preferably N-methylpyrrolidone and / or dimethyl sulfoxide; the molar ratio of the positive electrode material to the third organic solvent in the positive electrode slurry is preferably 1: (10-25); in the positive electrode slurry, excluding the third organic solvent, the mass ratio of the positive electrode material is preferably greater than 80%, the mass ratio of the conductive agent is preferably less than 10%, and the mass ratio of the binder is preferably less than 10%.
[0055] The positive electrode slurry is coated on the positive electrode collector to obtain a positive electrode sheet; the positive electrode collector can be a collector well known to those skilled in the art without any special restrictions, and is preferably aluminum foil, carbon-coated aluminum foil or microporous aluminum foil in the present invention; the thickness of the positive electrode slurry coating is preferably 5 to 500 μm, more preferably 20 to 400 μm, more preferably 50 to 300 μm, and most preferably 100 to 200 μm; in the embodiment provided by the present invention, the thickness of the positive electrode slurry coating is specifically 175 μm.
[0056] After the first reaction solution and the second reaction solution are mixed, they are immersed in the positive electrode plate and dried; the mass ratio of the first reaction solution to the second reaction solution is preferably 1: (1-5), more preferably 1: (1.5-3), more preferably 1: (1.5-2.5), and most preferably 1: (1.7-2.5); the mixing speed is preferably 100-1000 r / min; the immersion time is preferably 0.1-120 min, more preferably 5-100 min, more preferably 10-60 min, and most preferably 30-40 min; the drying temperature is preferably 50°C-150°C, more preferably 60°C-250°C, and more preferably 60°C-200°C.
[0057] In the present invention, a solid-state battery electrode can be obtained directly after drying, and the immersion and drying steps can be repeated 1 to 10 times as needed, preferably 2 to 8 times, more preferably 3 to 6 times, and most preferably 4 to 5 times, and a solid-state battery electrode can be obtained after taking out and drying.
[0058] The method for preparing solid-state battery pole pieces of the present invention does not require the addition of solid electrolytes. The two reaction solutions react to obtain a halide solid electrolyte solution, and a solid electrolyte is formed on the surface of the original pole piece layer through the reaction, which is equivalent to forming a solid electrolyte layer in situ, thereby making the obtained solid-state battery pole piece interface more solid.
[0059] The present invention also provides a solid-state battery electrode prepared by the above method.
[0060] The present invention also provides a solid-state battery, comprising the above-mentioned solid-state battery pole piece.
[0061] The present invention also provides a method for preparing a solid-state battery, comprising: laminating the solid-state battery pole piece prepared by the above method with the negative pole piece, and pressurizing and assembling them into a solid-state battery.
[0062] The negative electrode sheet includes a negative electrode active material and a negative electrode current collector; the negative electrode active material is preferably any one of metal lithium, pure silicon negative electrode material, silicon carbon negative electrode material, and silicon oxygen negative electrode material; the negative electrode current collector is preferably copper foil, carbon coated copper foil, microporous copper foil, etc.; preferably, the negative electrode sheet preferably also includes a negative electrode conductive agent; the negative electrode conductive agent is preferably one or more of conductive carbon black, nano carbon fiber, Ketjen black, carbon nanotube, and graphene; preferably, the negative electrode sheet preferably also includes a negative electrode binder; the negative electrode binder is preferably one or more of sodium carboxymethyl cellulose, styrene butadiene rubber, polyacrylic acid, and polyacrylamide. In the negative electrode sheet, in addition to the negative electrode current collector, the mass ratio of the negative electrode active material is preferably greater than 80%, the mass ratio of the negative electrode conductive agent is preferably less than 10%, and the mass ratio of the negative electrode binder is preferably less than 10%.
[0063] The pressurized pressure is preferably 10 to 370 MPa.
[0064] In order to further illustrate the present invention, the technical solution provided by the present invention is described in detail below in conjunction with embodiments.
[0065] The reagents used in the following examples are all commercially available.
[0066] Example 1
[0067] Weigh 1 g of ScCl3 using an analytical balance and dissolve it in 9.53 g of tetrahydrofuran to obtain solution A;
[0068] Use an analytical balance to weigh 1 g of LiCl and dissolve it in 17 g of tetrahydrofuran to obtain solution B;
[0069] Solution A and solution B are mixed to obtain solution C;
[0070] Solution C was placed in an oven at 60° C. and dried to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0071] Example 2
[0072] Weigh 1 g of ScCl3 on an analytical balance and dissolve it in 9.53 g of tetrahydrofuran to obtain solution A;
[0073] Use an analytical balance to weigh 1g of LiCl and dissolve it in 17g of tetrahydrofuran to obtain solution B.
[0074] Solution A and solution B are mixed to obtain solution C;
[0075] Solution C was placed in an oven at 100° C. to dry to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0076] Example 3
[0077] Weigh 1 g of ScCl3 on an analytical balance and dissolve it in 9.53 g of tetrahydrofuran to obtain solution A;
[0078] Use an analytical balance to weigh 1 g of LiCl and dissolve it in 17 g of tetrahydrofuran to obtain solution B;
[0079] Solution A and solution B are mixed to obtain solution C;
[0080] Solution C was placed in an oven at 200° C. to dry to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0081] Example 4
[0082] Weigh 1 g of ScCl3 on an analytical balance and dissolve it in 12.18 g of toluene to obtain solution A;
[0083] Use an analytical balance to weigh 1 g of LiCl and dissolve it in 21.74 g of toluene to obtain solution B;
[0084] Solution A and solution B are mixed to obtain solution C;
[0085] Solution C was placed in an oven at 100° C. to dry to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0086] Example 5
[0087] Weigh 1 g of ScCl3 on an analytical balance and dissolve it in 14.03 g of xylene to obtain solution A;
[0088] Use an analytical balance to weigh 1 g of LiCl and dissolve it in 25.06 g of xylene to obtain solution B;
[0089] Solution A and solution B are mixed to obtain solution C;
[0090] Solution C was placed in an oven at 150° C. and dried to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0091] Example 6
[0092] Weigh 1 g of ScCl3 on an analytical balance and dissolve it in 11.65 g of ethyl acetate to obtain solution A;
[0093] Use an analytical balance to weigh 1 g of LiCl and dissolve it in 20.79 g of ethyl acetate to obtain solution B;
[0094] Solution A and solution B are mixed to obtain solution C;
[0095] Solution C was placed in an oven at 100° C. to dry to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0096] Example 7
[0097] 1 g of ScCl3 was weighed on an analytical balance and dissolved in 6.09 g of ethanol-water solution to obtain solution A;
[0098] Use an analytical balance to weigh 1 g of LiCl and dissolve it in 17 g of ethanol water to obtain solution B;
[0099] The ethanol aqueous solution is a 95% ethanol aqueous solution;
[0100] Solution A and solution B are mixed to obtain solution C;
[0101] Solution C was placed in an oven at 100° C. to dry to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0102] Example 8
[0103] 1 g of GaCl3 was weighed on an analytical balance and dissolved in 8.19 g of tetrahydrofuran to obtain solution A;
[0104] Use an analytical balance to weigh 1 g of LiCl and dissolve it in 17 g of tetrahydrofuran to obtain solution B;
[0105] Solution A and solution B are mixed to obtain solution C;
[0106] Solution C was placed in an oven at 100° C. to dry to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0107] Example 9
[0108] Analytical balance weighs 1 g of InCl3 and dissolves it in 6.52 g of tetrahydrofuran to obtain solution A;
[0109] Use an analytical balance to weigh 1 g of LiCl and dissolve it in 17 g of tetrahydrofuran to obtain solution B;
[0110] Solution A and solution B are mixed to obtain solution C;
[0111] Solution C was placed in an oven at 100° C. to dry to obtain a halide solid electrolyte. The ionic conductivity of the solid electrolyte was tested, and the results are shown in Table 1.
[0112] Ionic conductivity detection method:
[0113] (1) Add 100 mg of solid electrolyte powder into a 10 mm (10 mm diameter of the sheet after mold pressing) polyetheretherketone (PEEK) mold, apply a pressure of 350 MPa for 180 s to form a sheet;
[0114] (2) Attach 50 mm thick stainless steel sheets to both sides of the thin sheet and pressurize at 20 MPa for 5 seconds to obtain a component with electrodes blocked at both ends.
[0115] (3) Assembling the components into batteries, and conducting electrochemical impedance spectroscopy (EIS) tests at a frequency range of 1 MHz to 100 MHz and a scan rate of 5 mV / s;
[0116] (4) Calculate the ionic conductivity according to the formula shown in formula (I), where d is the sample thickness (cm), Re is the body impedance of the sample under test (ohm), which can be obtained from the intersection of the semicircle arc and the oblique line in the Nyquist plot of the electrochemical impedance spectroscopy; S is the effective area of the electrode (cm 2 ).
[0117] σ=d / Re×S Formula (I)
[0118] Table 1 Preparation conditions and ionic conductivity test results of halide solid electrolytes in Examples 1 to 9
[0119]
[0120]
[0121] From the data of Examples 1 to 3 in the table, it can be seen that when the metal halide is ScCl3 and the organic solvent is tetrahydrofuran, the highest conductivity that can be obtained at a drying temperature of 200°C is 2.24 mS / cm;
[0122] It can be seen from the data of Examples 3 to 7 that the conductivity obtained by using different solvents is also different, and the conductivity obtained by using ethanol aqueous solution is the lowest.
[0123] It can be seen from the data of Example 2, Example 8 and Example 9 that the use of different metal halides will also affect the conductivity.
[0124] Example 10
[0125] (1) Positive electrode:
[0126] The positive electrode plate includes a positive electrode current collector (a bare aluminum foil with a thickness of 12 μm) and a positive electrode coating, wherein the positive electrode coating includes ternary Ni83 (a nickel-cobalt-manganese ternary positive electrode material with a nickel molar content of 83%), conductive carbon black (SP) and polyvinylidene fluoride (PVDF), wherein the mass ratio of ternary Ni83, SP and PVDF is 95%:2%:3%, which are added to the solvent NMP and mixed evenly to form a positive electrode coating, wherein the solid content of the positive electrode coating is 50%; the positive electrode coating is evenly coated on the surface of the 12 μm positive electrode current collector, the coating thickness is 175 μm, and the positive electrode plate is obtained after drying. Solution A and solution B are prepared according to the method of Example 1, and a mixed solution C is obtained after solution A and solution B are mixed, and the prepared positive electrode plate is immersed in the mixed solution C for about 30 minutes, and then taken out and dried in a vacuum oven at 100°C, and the operation is repeated 5 times to obtain a solid-state battery plate having a solid electrolyte on the surface.
[0127] (2) Negative electrode
[0128] The metal lithium negative electrode sheet is a negative electrode current collector (copper foil with a thickness of 6 μm) and a lithium foil (lithium foil with a thickness of 100 μm) which are composited and pressed by a roller press to obtain a metal lithium negative electrode sheet with a thickness of 105 μm.
[0129] (3) Preparation of battery cells
[0130] The solid-state battery electrode and negative electrode prepared by (1) and (2) were assembled into a solid-state battery under pressure of 50 MPa. The electrical properties were tested and the results are shown in Table 2.
[0131] Electrical performance test method:
[0132] Test assembled solid-state battery: test temperature 60℃, 0.1C constant current charge to 4.5V, stand for 30min, 0.1C constant current discharge to 2.5V.
[0133] Embodiment 11
[0134] The difference between Example 11 and Example 10 is that the mixed solution C is prepared according to Example 8.
[0135] Example 12
[0136] The difference between Example 12 and Example 10 is that the mixed solution C is prepared according to Example 9.
[0137] Embodiment 13
[0138] The difference between Example 13 and Example 10 is that the negative electrode plate is a silicon negative electrode plate prepared by the following method.
[0139] Silicon negative electrode sheet preparation:
[0140] The silicon negative electrode sheet includes a negative electrode current collector (copper foil with a thickness of 6 μm) and a negative electrode coating, wherein the negative electrode coating includes micron silicon, polyvinylidene fluoride and carbon nanotubes, wherein the mass ratio of micron silicon, polyvinylidene fluoride and carbon nanotubes is 90%:5%:5%, and the micron silicon, polyvinylidene fluoride and carbon nanotubes are added into a solvent deionized water and mixed evenly to form a negative electrode coating, wherein the solid content of the negative electrode coating is 45%; the negative electrode coating is evenly coated on a 6 μm copper foil with a coating thickness of 50 μm, and then dried at a temperature of 110° C., rolled, and cut into strips to form a negative electrode sheet.
[0141] Embodiment 14
[0142] The difference between Example 14 and Example 13 is that the mixed solution C is prepared according to Example 8.
[0143] Embodiment 15
[0144] The difference between Example 15 and Example 13 is that the mixed solution C is prepared according to Example 9.
[0145] Table 2 Electrical performance test results of solid-state batteries prepared in Examples 10 to 15
[0146]
[0147]
[0148] The solid-state battery pole piece prepared by the method of the present invention has a metal lithium negative electrode as the negative electrode. The solid-state battery is made and the electrical performance is tested. Its first-cycle discharge capacity is greater than 225mAh / g, and its first efficiency is higher than 92%. When a silicon negative electrode is used, the first-cycle discharge capacity is greater than 214mAh / g, and the first efficiency is higher than 86%. Whether it is a metal lithium negative electrode or a silicon negative electrode, its efficiency is relatively high. This method can be applied to solid-state batteries, greatly improving the efficiency of solid-state batteries.
Claims
1. A liquid phase preparation method of a halide solid electrolyte, characterized in that: include: S1) MX a mixing with a first organic solvent to obtain a first reaction solution; mixing LiX with a second organic solvent to obtain a second reaction solution; M is selected from transition metal elements or rare earth elements; X is a halogen; a is a coordination valence; S2) mixing the first reaction solution and the second reaction solution, and drying to obtain a halide solid electrolyte.
2. The preparation method according to claim 1, characterized in that: The M is selected from one or more of Sc, Y, In, Ga, La, Zr and Ti; the X is selected from one or more of F, Cl, Br and I; the first organic solvent and the second organic solvent are each independently selected from one or more of dimethyl sulfoxide, tetrahydropyran, tetrahydrofuran, anisole, amino ethers, halogenated ethers, hydroxy ethers, 2,3-dimethyltetrahydrofuran, 2,5-dimethyltetrahydrofuran and fluorinated tetrahydropyran, toluene, xylene, carbon tetrachloride, and ethyl acetate.
3. The preparation method according to claim 1, characterized in that: The MX a The molar ratio of LiX to the first organic solvent is 1:(15-25); the molar ratio of LiX to the second organic solvent is 1:(7-15); The mass ratio of the first reaction solution to the second reaction solution is 1:(1-5).
4. The preparation method according to claim 1, characterized in that: The mixing in step S2) is stirring mixing, and the mixing speed is 100-1000r / min; The drying temperature is 50° C. to 300° C.; the drying time is 0.5 to 5 hours.
5. A halide solid electrolyte prepared by the preparation method according to any one of claims 1 to 4.
6. A method for preparing a solid-state battery electrode, characterized in that: The following steps are involved: A1) MX a mixing with a first organic solvent to obtain a first reaction solution; Mixing LiX with a second organic solvent to obtain a second reaction solution; M is selected from transition metal elements or rare earth elements; X is a halogen; a is a coordination valence; Mixing the positive electrode material, the conductive agent and the binder in a third organic solvent to obtain a positive electrode slurry; Applying the positive electrode slurry on the positive electrode current collector to obtain a positive electrode sheet; A2) After mixing the first reaction solution and the second reaction solution, immersing the mixture into a positive electrode plate, taking it out and drying it to obtain a solid-state battery plate.
7. The preparation method according to claim 6, characterized in that: The positive electrode material is selected from one or more of nickel-cobalt-manganese ternary positive electrode materials, lithium iron phosphate, lithium-rich manganese-based materials and lithium cobalt oxide; The conductive agent is selected from one or more of conductive carbon black, nanocarbon fiber and Ketjen black; The binder is selected from one or more of styrene-butadiene rubber, tetrafluoroethylene rubber and silicone rubber; The positive electrode current collector is selected from aluminum foil, carbon-coated aluminum foil or microporous aluminum foil; The third organic solvent is selected from N-methylpyrrolidone and / or dimethyl sulfoxide; The molar ratio of the positive electrode material to the third organic solvent in the positive electrode slurry is 1:(10-25); The positive electrode slurry is coated to a thickness of 5 to 500 μm.
8. The preparation method according to claim 6, characterized in that: The mixing in step A2) is stirring mixing, and the mixing speed is 100-1000 r / min; the immersion time is 0.1-120 min; the drying temperature is 50° C.-150° C.; The immersing and drying steps in step A2) are repeated 1 to 10 times, and the solid-state battery electrode is obtained after being taken out and dried.
9. A solid-state battery electrode prepared by the preparation method according to any one of claims 6 to 8.
10. A solid-state battery, characterized in that: A solid-state battery electrode prepared by any one of claims 6 to 8; Also includes a negative electrode plate; The negative electrode plate comprises a negative electrode active material and a negative electrode current collector; The negative electrode active material is selected from any one of metallic lithium, pure silicon negative electrode material, silicon-carbon negative electrode material, and silicon-oxygen negative electrode material; The negative electrode current collector is selected from copper foil, carbon-coated copper foil or microporous copper foil.
Citation Information
Cited By
Electrode plate, preparation method thereof and battery
CN121215663A
Oxidation halide solid electrolyte material and preparation method and application thereof
CN122010565A
Halide solid electrolyte and preparation method therefor, solid electrolyte membrane, solid-state battery and electrical device
WO2026184258A1