Manufacturing method for in-situ generation of multi-morphology silicon carbide nanostructure reinforced carbon foam ultralight electromagnetic absorption material
Through in-situ reaction, various morphologies of silicon carbide nanostructure-reinforced carbon foam are generated, which solves the problems of insufficient preparation process and unutilized performance of silicon carbide nanowires in the existing technology, and achieves efficient electromagnetic wave absorption and heat insulation properties, which is suitable for in the design of composite materials.
Patent Information
- Application Number
- CN202410934335.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology has shortcomings in the preparation and structural design of silicon carbide nanowires. It lacks a detailed introduction to the preparation process of silicon carbide nanowires and fails to fully utilize its thermal insulation and wave absorption properties, which affects the performance of the material in certain application fields. and application scope.
Silicon carbide nanostructures of various shapes are generated through in-situ reaction methods. Polyurethane foam is used as a carbon source, combined with materials such as carbon powder and alumina powder, and the silicon carbide nanostructure reinforced carbon foam is formed through heat treatment by the buried carbon method to form a three-dimensional network. structure to improve the material’s wave absorption and thermal insulation properties.
The preparation of ultra-light thermal insulation materials has been achieved, with good wave absorption performance and mechanical strength. It is suitable for composite electromagnetic wave absorbing materials, has a wide range of applications, and reaches a minimum reflection loss of -59.321dB at a frequency of 11.28GHz. The conductivity is 0.035W/(m·K) and the volume density is 26.3g/m3.
Smart Images

Figure CN118738877A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of manufacturing wave-absorbing composite materials, and in particular to a method for manufacturing an ultralight electromagnetic absorbing material with in-situ generated silicon carbide nanostructures and reinforced carbon foams with various morphologies. Background Art
[0002] At present, with the continuous development of electromagnetic technology, electromagnetic waves have been widely used in various fields such as communications, radar and navigation systems, which obviously puts higher requirements on the working performance of absorbing materials. Therefore, the research and development of high-temperature heat-insulating and absorbing integrated materials with low density, high temperature resistance, oxidation resistance, good heat insulation effect and excellent absorbing performance has important scientific and practical significance.
[0003] The Chinese invention patent with application number 201810591706.8 discloses a CVI-SiC nanowire reinforced composite carbon foam material and its preparation method. The material is composed of a three-dimensional network of carbon foam, and silicon carbide nanowires grow on the surface of the carbon foam. The cross-sectional shape of the carbon foam wall can be circular, elliptical or triangular, with a size between 1 and 10 μm, a porosity of 95 to 99.5%, a pore size between 10 and 50 μm, an aspect ratio of 5 to 20, and a compressive strength between 20 and 50 kPa. The silicon carbide nanowire is a β-SiC nanowire with a metal ball at the tip, a purity of not less than 99%, a diameter range of 10 to 80 nm, and a length range of 0.5 to 50 μm. The advantages of this invention include: (1) low-density reinforced composite carbon foam, with a density of 5 to 20 mg per cubic centimeter, and significantly enhanced compressive resistance; (2) the material can be used in supercapacitors, and the intricate porous structure between its nanowires helps store energy particles and improves energy storage efficiency; (3) due to its ultra-high specific surface area, it can also be used in the field of catalysis. However, this invention also has some shortcomings: (1) the method of directly preparing silicon carbide nanowires on the surface of carbon foam does not bring about obvious performance improvements; (2) there is a lack of detailed introduction to the preparation process and structural design of silicon carbide nanowires; (3) there is no mention of its thermal insulation and wave absorption properties, which are key properties of this material in certain application fields. Therefore, it is necessary to further study and optimize to improve the performance and application range of the material.
[0004] The Chinese invention patent with application number 201911121756.0 relates to a method for preparing a silicon carbide-porous carbon one-dimensional nano-wave absorbing material and its application. The wave absorbing material is composed of silicon carbide nanowires and porous carbon, and is in a gray-black powder form. The porous carbon is located on the surface of the silicon carbide nanowires to form a core-shell structure. The invention uses silicon carbide as the main material, and the final product has stable performance and is easy to mass produce. By controlling the heat treatment time, the microstructure of the porous carbon and the dielectric properties of silicon carbide can be adjusted to improve the wave absorbing performance. When the material is mixed with paraffin, at a certain ratio, when the matching thickness is 2.69mm, the bandwidth of the reflection loss in the frequency range of 2-18GHz is less than -10dB, which can reach 7.16GHz. In addition, when the matching thickness is 2.38mm, the lowest reflection loss occurs at 15.24GHz, reaching -56.34dB. However, the material is a one-dimensional nanostructure, but it does not have the advantages of a three-dimensional spatial network structure.
[0005] The Chinese invention patent application number 202110252587.5 discloses a silicon carbide nano thermal insulation and wave absorbing composite material, which is composed of a carbon foam substrate template, a silicon carbide coating reinforced interface and a silicon carbide nanowire network structure, with a volume density of 15.0-25.0 kg / m 3 , the thermal conductivity at room temperature is 0.030~0.040W / (m·K), and the minimum reflection loss is -40.0~-30.0dB. The advantages of this invention include: (1) The discontinuous and discontinuously distributed silicon carbide coating enhanced interface reduces the overall weight of the material on the one hand, and reduces solid heat transfer on the other hand. (2) The reaction gas is evenly distributed on the silicon carbide coating enhanced interface and grows in a straight line to form a "T"-shaped pinning structure. (3) The silicon carbide nanowire network structure has uniformity and integrity. However, there are still some problems in this invention that can be further improved: (1) The process includes multiple steps and the adjustment of multiple reaction conditions, and it is necessary to accurately control the time, temperature, gas flow rate and other parameters of each step. (2) During the reaction process, impurities or incomplete reaction products may be produced, which may affect the performance and stability of the final product.
[0006] In summary, it is very advantageous to select silicon carbide as the main material for high temperature resistance, heat insulation and wave absorption, but how to use simple process steps to prepare multifunctional silicon carbide materials that take into account both wave absorption and heat insulation is still a problem that needs to be solved urgently. Summary of the invention
[0007] The purpose of the present invention is to provide a method for manufacturing an ultra-light electromagnetic absorption material of carbon foam reinforced with silicon carbide nanostructures in situ to solve the above-mentioned problems in the background technology. The present invention obtains a carbon foam material reinforced with silicon carbide nanostructures in various morphologies through an in-situ reaction method. The material uses porous carbon foam as a skeleton, and the silicon carbide nanostructure is coated and entangled with the internal and external micropores and surface of the carbon foam to form a three-dimensional network structure. The prepared material is ultra-light and heat-insulating, has a certain mechanical strength and good wave-absorbing performance, and provides an effective way to design composite electromagnetic wave-absorbing materials.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] One of the technical solutions of the present invention is to provide a method for preparing in-situ generated silicon carbide nanostructure reinforced carbon foam, characterized in that it comprises the following steps:
[0010] A carbon source, silicon powder and a foaming agent are mixed and foamed to obtain a silicon-containing foam precursor;
[0011] The silicon-containing foam precursor is subjected to high-temperature heat treatment using a carbon embedding method to obtain the in-situ generated silicon carbide nanostructure reinforced carbon foam.
[0012] Preferably, the preparation method comprises the following steps:
[0013] The polyurethane material A, metal silicon powder and polyurethane material B are mixed and reacted to obtain silicon-containing polyurethane foam;
[0014] The silicon-containing polyurethane foam is placed in crucible A, and then crucible A is placed in crucible B with carbon powder on the bottom, and then carbon powder is continued to be added to crucible B until crucible A is completely covered, and then a layer of alumina powder a, a layer of silica powder, and a layer of alumina powder b are laid on the top of the carbon powder in sequence, and then the crucible B is heat-treated to obtain the in-situ generated silicon carbide nanostructure reinforced carbon foam.
[0015] After the foaming treatment, a polyurethane foam containing uniformly dispersed metallic silicon powder can be obtained, which provides a porous structure and is conducive to the subsequent generation of silicon carbide nanostructures.
[0016] During the heat treatment process, which is carried out under normal atmosphere, the carbon embedding method can isolate oxygen in the air, and the polyurethane foam generates carbon, which reacts with silicon powder in situ to generate silicon carbide nanostructures.
[0017] Preferably, the mass ratio of the polyurethane material a, the metal silicon powder and the polyurethane material b is 1:0.5-3:1-1.2.
[0018] Preferably, the reaction is carried out by stirring at a rotation speed of 1000-1500 r / min for 5-10 min and then standing for 2-10 min.
[0019] Preferably, after the reaction is completed, a aging step is further included; the aging temperature is 70-90° C. and the time is 1-2 h.
[0020] Preferably, the morphology of silicon carbide in the in-situ generated silicon carbide nanostructure-enhanced carbon foam is controlled by adjusting the heat treatment temperature, specifically:
[0021] When the heat treatment temperature is 1350-1400° C., the generated silicon carbide nanostructure is spherical in shape;
[0022] When the heat treatment temperature is 1450-1500° C., the generated silicon carbide nanostructure has a bead-like shape;
[0023] When the heat treatment temperature is 1550-1600° C., the generated silicon carbide nanostructure has a bamboo-like shape.
[0024] Preferably, the heat treatment is to heat the temperature to 1400-1600° C. at a heating rate of 5° C. / min and then keep the temperature for 1 hour.
[0025] The present invention can make the generated silicon carbide nanostructure have various morphologies by regulating the heat treatment temperature. As the heat treatment temperature increases from low to high, the morphologies of the generated nanostructures are spherical, chain-beaded and bamboo-jointed in sequence.
[0026] During the reaction process, the decomposition of the polyurethane of the present invention will have the following stages: the polyurethane foam matrix begins to decompose primarily after being heated. This process mainly occurs at a relatively low temperature (about 290°C). At this time, chemical bonds with poor stability begin to break and release some small molecular products. As the temperature rises, the polyurethane foam enters the main decomposition stage. In this stage, the main chain urethane bonds begin to depolymerize to generate products such as isocyanates and polyols; at the same time, a large amount of small molecular gases are generated, such as HCN, NO, CO, etc. When the temperature continues to rise, the residues produced by the decomposition of the polyurethane foam begin to be deeply carbonized. In this process, organic matter is gradually converted into carbonized products such as coke. Under anaerobic conditions, due to the lack of oxygen, the combustion reaction is suppressed, so it is easier to form coke. In this environment, the polyurethane will be cracked into carbon and maintain the original basic foam structure, and then continue to react with silicon powder.
[0027] The second technical solution of the present invention is to provide an in-situ generated silicon carbide nanostructure reinforced carbon foam obtained according to the above preparation method.
[0028] The third technical solution of the present invention is to provide an application of the above-mentioned in-situ generated silicon carbide nanostructure reinforced carbon foam in the field of electromagnetic absorption materials.
[0029] The beneficial technical effects of the present invention are as follows:
[0030] The present invention obtains carbon foam materials reinforced with silicon carbide nanostructures of various morphologies through an in-situ reaction method. The material uses porous carbon foam as a skeleton, and the silicon carbide nanostructures are coated and entangled with the internal and external micropores and surfaces of the carbon foam to form a three-dimensional network structure.
[0031] In the carbon foam reinforced with in-situ generated silicon carbide nanostructures of the present invention, the carbon generated by the polyurethane reaction provides a carbon source for the in-situ generated silicon carbide, wherein the carbon source is not limited to polyurethane foam. The three-dimensional network composed of silicon carbide nanostructures with various morphologies improves the electromagnetic wave absorption performance of the composite material on the one hand, and strengthens the mechanical strength of the carbon foam matrix on the other hand. The obtained composite material is ultra-light and heat-insulating, which can meet the requirements of various working environments and achieve good technical effects. The characteristics of reinforcement, heat insulation, wave absorption, etc. are achieved through the silicon carbide nanostructure network with different morphologies.
[0032] Nanostructures can form strong and hard nanoparticle networks in the foam matrix, and these network structures can significantly enhance the strength and hardness of the matrix. Nanoparticles have a higher surface area and smaller grain size, which can provide more grain boundaries and dislocation barriers, thereby effectively preventing the expansion of cracks. In addition, nanoparticles are dispersed in the foam matrix as a reinforcement phase, forming interfaces between the nanoparticles and the matrix. These interface regions can absorb and disperse stress due to the high strength and high toughness of the nanoparticles, further preventing the expansion of cracks, thereby improving the toughness of the matrix.
[0033] Among them, carbon foam, as a typical conductive electromagnetic absorption material, can allow more electromagnetic waves to enter the material and convert part of the electromagnetic wave energy into heat energy. The silicon carbide nanostructure distributed on the carbon foam is a dielectric loss type electromagnetic absorption material, which can consume the electromagnetic waves entering the material through interface polarization and dipole relaxation polarization. The synergistic effect of the two consumption methods greatly improves the electromagnetic wave loss capacity. At the same time, the micron-scale porous structure formed by the overlapping of silicon carbide nanostructures can effectively inhibit heat conduction and form a good high-temperature thermal insulation effect.
[0034] The synthesis process of the invention is simple, highly repeatable, low-cost, environmentally friendly, and has a wide range of applications. The prepared material is ultra-light and heat-insulating, has a certain mechanical strength and good wave-absorbing performance, and provides an effective way to design composite electromagnetic wave-absorbing materials. The minimum reflection loss of the prepared product at a frequency of 11.28 GHz can reach -59.321 dB, the thermal conductivity at room temperature is 0.035 W / (m·K), and the volume density is 26.3 g / m3 , is an ideal lightweight heat-insulating and wave-absorbing multifunctional material. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 The X-ray diffraction patterns of different products in Effect Example 1. Among them, (a) is the X-ray diffraction pattern of the product obtained at different insulation temperatures when the addition amount of metal silicon powder is 0.5g; (b) is the X-ray diffraction pattern of the product obtained at different insulation temperatures when the addition amount of metal silicon powder is 1.0g; (c) is the X-ray diffraction pattern of the product obtained at different insulation temperatures when the addition amount of metal silicon powder is 2.0g; (d) is the X-ray diffraction pattern of the product obtained at different insulation temperatures when the addition amount of metal silicon powder is 3.0g.
[0037] Figure 2 The following are scanning electron microscope images of different products in Example 2. Among them, (a) and (d) are scanning electron microscope images of products obtained at 1400°C; (b) and (e) are scanning electron microscope images of products obtained at 1500°C; (c) and (f) are scanning electron microscope images of products obtained at 1600°C.
[0038] Figure 3 The microscopic data of the product at a holding temperature of 1400°C in Example 2 are shown in Figure 2. (a) is a diffraction spot diagram; (b) is a transmission electron microscope diagram; (c)-(e) are EDS element spectrum analysis diagrams.
[0039] Figure 4 The microscopic data of the product at a holding temperature of 1500°C in Example 2. (a) and (c) are transmission electron microscope images of different parts; (b) is a local enlarged image of the marked part in (a) and a lattice diffraction fringe image; (d)-(f) are EDS element spectrum analysis images.
[0040] Figure 5 The microscopic data of the product at a holding temperature of 1600°C in Example 2. (a)-(b) are transmission electron microscope images at different magnifications; (c) is a local magnification of the marked part in (b) and a lattice diffraction fringe image; (d)-(f) are EDS element spectrum analysis images. DETAILED DESCRIPTION
[0041] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0042] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0043] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.
[0044] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.
[0045] The specifications of the metallic silicon powder used in the following embodiments and comparative examples of the present invention are ≥800 meshes and the purity is ≥99.89%.
[0046] The polyurethane material a and the polyurethane material b used in the following examples and comparative examples of the present invention were purchased from Heilongjiang Luobei Yunshan Carbon Industry Co., Ltd.
[0047] All raw materials used in the following examples and comparative examples of the present invention are commercially available products.
[0048] Example 1
[0049] Preparation of carbon foam:
[0050] (1) Weigh 2.0g of polyurethane material a and 1.0g of metal silicon powder, pour them into a beaker, and then stir and mix them with a glass rod. After they are evenly mixed, weigh 2.2g of polyurethane material b and add them into the beaker. Add a magnet to stir them rapidly on a magnetic stirrer at a speed of 1300r / min for 5 minutes. After foaming begins, turn off the magnetic stirrer. After waiting for 10 minutes, the foaming is completed. Put the foamed beaker into a 70°C oven for aging and take it out after 2 hours. Silicon-containing polyurethane foam is obtained.
[0051] (2) Take the silicon-containing polyurethane foam out of the beaker and put it into a graphite crucible. Take another larger alumina crucible, spread a layer of carbon powder in the alumina crucible, put the graphite crucible in, and then continue to add carbon powder until the graphite crucible is completely covered. Then, spread a layer of alumina powder a, a layer of silica powder, and a layer of alumina powder b on the top of the carbon powder in turn, and press them tightly. The thickness of the alumina powder a layer is 2 cm; the thickness of the silica powder layer is 2 cm; the thickness of the alumina powder b layer is 2 cm.
[0052] (3) placing the alumina crucible in a high-temperature lifting furnace, heating it to 1500° C. at a heating rate of 5° C. / min, keeping the temperature for 1 hour, and then cooling it with the furnace to obtain a carbon foam containing chain-like silicon carbide nanostructures.
[0053] Using the vector network analyzer coaxial method (test standard GJB5239-2004), when the amount of absorbing material added is 30% of the total mass of the test absorbing ring, it is measured that it has the best microwave absorption in the Ku band, the specific reflection loss RL value is -59.321dB (11.28GHz), the effective absorbing bandwidth is 2.64GHz, and the thickness is 2mm; using the laser flash point method to measure its thermal conductivity is 0.035W / (m·K), and using the Archimedean drainage method to measure its volume density is 26.3kg / m 3 .
[0054] Example 2
[0055] The only difference from Example 1 is that the amount of metallic silicon powder added is changed to 0.5 g.
[0056] Using the vector network analyzer coaxial method (test standard GJB5239-2004), when the amount of absorbing material added is 10% of the total mass of the test absorbing ring, it is measured that it has the best microwave absorption in the Ku band, the specific reflection loss RL value is -45.695dB (9.68GHz), the effective absorbing bandwidth is 4.88GHz, and the thickness is 3.1mm; using the laser flash point method to measure its thermal conductivity is 0.048W / (m·K), and using the Archimedean drainage method to measure its volume density is 26.1kg / m 3 .
[0057] Example 3
[0058] The only difference from Example 1 is that the amount of metallic silicon powder added is changed to 2.0 g.
[0059] Using the vector network analyzer coaxial method (test standard GJB5239-2004), when the amount of absorbing material added is 30% of the total mass of the test absorbing ring, it is measured that it has the best microwave absorption in the Ku band, the specific reflection loss RL value is -51.524dB (6.48GHz), the effective absorbing bandwidth is 1.84GHz, and the thickness is 4.1mm; using the laser flash point method to measure its thermal conductivity is 0.042W / (m·K), and using the Archimedean drainage method to measure its volume density is 26.5kg / m 3 .
[0060] Example 4
[0061] The only difference from Example 1 is that the amount of metallic silicon powder added is changed to 3.0 g.
[0062] Using the vector network analyzer coaxial method (test standard GJB5239-2004), when the amount of absorbing material added is 25% of the total mass of the test absorbing ring, it is measured that it has the best microwave absorption in the Ku band, the specific reflection loss RL value is -57.211dB (6.8GHz), the effective absorbing bandwidth is 4GHz, and the thickness is 4.9mm; using the laser flash point method to measure its thermal conductivity is 0.052W / (m·K), and using the Archimedean drainage method to measure its volume density is 26.8kg / m 3 .
[0063] Example 5
[0064] Preparation of carbon foam:
[0065] (1) Weigh 2.0g of polyurethane material a and 1.0g of metal silicon powder, pour them into a beaker, and then stir and mix them with a glass rod. After they are evenly mixed, weigh 2.2g of polyurethane material b and add them into the beaker. Add a magnet to stir them rapidly on a magnetic stirrer at a speed of 1500r / min for 7 minutes. After foaming begins, turn off the magnetic stirrer. After waiting for 5 minutes, the foaming is completed. Put the foamed beaker into a 70°C oven for aging and take it out after 2 hours. Silicon-containing polyurethane foam is obtained.
[0066] (2) Take the silicon-containing polyurethane foam out of the beaker and put it into a graphite crucible. Take another larger alumina crucible, spread a layer of carbon powder in the alumina crucible, put the graphite crucible in, and then continue to add carbon powder until the graphite crucible is completely covered. Then, spread a layer of alumina powder a, a layer of silica powder, and a layer of alumina powder b on the top of the carbon powder in turn, and press them tightly. The thickness of the alumina powder a layer is 2 cm; the thickness of the silica powder layer is 2 cm; the thickness of the alumina powder b layer is 2 cm.
[0067] (3) placing the alumina crucible in a high-temperature lifting furnace, heating it to 1600° C. at a heating rate of 5° C. / min, keeping it at that temperature for 1 hour, and then cooling it with the furnace to obtain a carbon foam containing bamboo-like silicon carbide nanostructures.
[0068] Using the vector network analyzer coaxial method (test standard GJB5239-2004), when the amount of absorbing material added is 20% of the total mass of the test absorbing ring, it is measured that it has the best microwave absorption in the Ku band, the specific reflection loss RL value is -42.786dB (15.2GHz), the effective absorbing bandwidth is 3.12GHz, and the thickness is 5.1mm; using the laser flash point method to measure its thermal conductivity is 0.032W / (m·K), and using the Archimedean drainage method to measure its volume density is 26.4kg / m 3 .
[0069] Example 6
[0070] Preparation of carbon foam:
[0071] (1) Weigh 2.0g of polyurethane material a and 1.0g of metal silicon powder, pour them into a beaker, and then stir and mix them with a glass rod. After they are evenly mixed, weigh 2.2g of polyurethane material b and add them into the beaker. Add a magnet to stir them rapidly on a magnetic stirrer at a speed of 1300r / min for 6 minutes. After foaming begins, turn off the magnetic stirrer. After waiting for 8 minutes, the foaming is completed. Put the foamed beaker into a 70°C oven for aging and take it out after 2 hours. Silicon-containing polyurethane foam is obtained.
[0072] (2) Take the silicon-containing polyurethane foam out of the beaker and put it into a graphite crucible. Take another larger alumina crucible, spread a layer of carbon powder in the alumina crucible, put the graphite crucible in, and then continue to add carbon powder until the graphite crucible is completely covered. Then, spread a layer of alumina powder a, a layer of silica powder, and a layer of alumina powder b on the top of the carbon powder in turn, and press them tightly. The thickness of the alumina powder a layer is 2 cm; the thickness of the silica powder layer is 2 cm; the thickness of the alumina powder b layer is 2 cm.
[0073] (3) placing the alumina crucible in a high-temperature lifting furnace, heating it to 1400° C. at a heating rate of 5° C. / min, keeping it at that temperature for 1 hour, and then cooling it with the furnace to obtain a carbon foam containing small spherical silicon carbide nano-morphology.
[0074] Using the vector network analyzer coaxial method (test standard GJB5239-2004), when the amount of absorbing material added is 40% of the total mass of the test absorbing ring, it is measured that it has the best microwave absorption in the Ku band, the specific reflection loss RL value is -37.502dB (4.08GHz), the effective absorbing bandwidth is 2.32GHz, the thickness is 4.5mm, and it shows a certain full-band electromagnetic wave absorption performance; using the laser flash point method to measure its thermal conductivity is 0.043W / (m·K), and using the Archimedean drainage method to measure its volume density is 26.1kg / m 3 .
[0075] Comparative Example 1
[0076] The only difference from Example 1 is that the stirring with a magnetic stirrer in step (1) is changed to mechanical stirring with a glass rod.
[0077] The test results showed that the polyurethane B material was not mixed evenly and the foaming was not thorough, which led to the aggregation of silicon powder distribution and the uneven silicon carbide nanostructure generated. The carbon foam base in some areas was consumed in large quantities and the structure was destroyed.
[0078] Comparative Example 2
[0079] The only difference from Example 1 is that the holding time in step (3) is changed to 0.5 h.
[0080] The test results show that the in-situ reaction in the material was not fully carried out, there was a lot of silicon powder residue, and the generated chain bead nanostructure was less. Using the vector network analyzer coaxial method (test standard GJB5239-2004), when the amount of absorbing material added was 30% of the total mass of the test absorbing ring, it was measured that it had the best microwave absorption in the Ku band, with a specific reflection loss RL value of -25.328dB (8.34GHz), an effective absorbing bandwidth of 3.35GHz, and a thickness of 3.6mm; using the laser flash point method to measure its thermal conductivity is 0.047W / (m·K), and using the Archimedean drainage method to measure its volume density is 26.8kg / m 3 .
[0081] Effect Example 1
[0082] By modifying the amount of metal silicon powder added in Example 1 (0.5, 1.0, 2.0, 3.0 g) and the insulation temperature in step (3) (1400, 1500, 1600° C.), the corresponding products were obtained and then subjected to X-ray diffraction tests. The test results are as follows: Figure 1 shown.
[0083] Figure 1The X-ray diffraction patterns of different products in Effect Example 1. Among them, (a) is the X-ray diffraction pattern of the product obtained at different insulation temperatures when the addition amount of metal silicon powder is 0.5g; (b) is the X-ray diffraction pattern of the product obtained at different insulation temperatures when the addition amount of metal silicon powder is 1.0g; (c) is the X-ray diffraction pattern of the product obtained at different insulation temperatures when the addition amount of metal silicon powder is 2.0g; (d) is the X-ray diffraction pattern of the product obtained at different insulation temperatures when the addition amount of metal silicon powder is 3.0g.
[0084] Depend on Figure 1 It can be seen that the high-temperature heat treatment of silicon-containing polyurethane foam at three temperatures with different silicon powder addition amounts all reacted smoothly to generate silicon carbide, achieving the expected goal. And with the increase in the amount of silicon powder added, the diffraction peak intensity of carbon decreased and the diffraction peak intensity of silicon carbide increased, indicating that the output of silicon carbide is constantly increasing.
[0085] Effect Example 2
[0086] By respectively modifying the holding temperature (1400, 1600°C) in step (3) of Example 1, the corresponding products were obtained, and then the microscopic morphology of the corresponding products was observed. The test results are as follows: Figure 2-3 shown.
[0087] Figure 2 The following are scanning electron microscope images of different products in Example 2. Among them, (a) and (d) are scanning electron microscope images of products obtained at 1400°C; (b) and (e) are scanning electron microscope images of products obtained at 1500°C; (c) and (f) are scanning electron microscope images of products obtained at 1600°C.
[0088] from Figure 2 It can be seen from (a) and (d) that the microscopic morphology of the material after heat treatment at 1400°C is that a large number of silicon carbide nanospheres are distributed on the carbon foam; it can be seen from (b) and (e) that the microscopic morphology of the material after heat treatment at 1500°C is that a large number of silicon carbide nanochain beads are distributed on the carbon foam; it can be seen from (c) and (f) that the microscopic morphology of the material after heat treatment at 1600°C is that a large number of silicon carbide nanostructures are distributed on the carbon foam.
[0089] Figure 3 The microscopic data of the product at a holding temperature of 1400°C in Example 2 are shown in Figure 2. (a) is a diffraction spot diagram; (b) is a transmission electron microscope diagram; (c)-(e) are EDS element spectrum analysis diagrams.
[0090] from Figure 3It can be seen from (c) and (d) that the main elements of the SiC nanospheres include Si and O, and exist in the form of SiO2. However, the diffraction spots in (a) are only those of SiC, indicating that SiC is crystalline and SiO2 is amorphous.
[0091] Figure 4 The microscopic data of the product at a holding temperature of 1500°C in Example 2. (a) and (c) are transmission electron microscope images of different parts; (b) is a local enlarged image of the marked part in (a) and a lattice diffraction fringe image; (d)-(f) are EDS element spectrum analysis images.
[0092] Figure 5 The microscopic data of the product at a holding temperature of 1600°C in Example 2. (a)-(b) are transmission electron microscope images at different magnifications; (c) is a local magnification of the marked part in (b) and a lattice diffraction fringe image; (d)-(f) are EDS element spectrum analysis images.
[0093] from Figure 3-5 It can be seen that the nanostructures of different morphologies of this material are all grown from a mixed growth source of amorphous SiO2 and crystalline SiC.
[0094] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing in-situ generated silicon carbide nanostructure reinforced carbon foam, characterized in that: The following steps are involved: A carbon source, silicon powder and a foaming agent are mixed and foamed to obtain a silicon-containing foam precursor; The silicon-containing foam precursor is subjected to high-temperature heat treatment using a carbon embedding method to obtain the in-situ generated silicon carbide nanostructure reinforced carbon foam.
2. The preparation method according to claim 1, characterized in that: The following steps are involved: The polyurethane material A, metal silicon powder and polyurethane material B are mixed and reacted to obtain silicon-containing polyurethane foam; The silicon-containing polyurethane foam is placed in crucible A, and then crucible A is placed in crucible B with carbon powder on the bottom, and then carbon powder is continued to be added to crucible B until crucible A is completely covered, and then a layer of alumina powder a, a layer of silica powder, and a layer of alumina powder b are laid on the top of the carbon powder in sequence, and then the crucible B is heat-treated to obtain the in-situ generated silicon carbide nanostructure reinforced carbon foam.
3. The preparation method according to claim 2, characterized in that: The mass ratio of the polyurethane material a, the metal silicon powder and the polyurethane material b is 1:0.5-3:1-1.
2.
4. The preparation method according to claim 2, characterized in that: The reaction is carried out by stirring at a rotation speed of 1000-1500 r / min for 5-10 min and then standing for 2-10 min.
5. The preparation method according to claim 2, characterized in that: After the reaction is completed, a aging step is further included; the aging temperature is 70-90° C. and the time is 1-2 hours.
6. The preparation method according to claim 2, characterized in that: The heat treatment is to heat the temperature to 1400-1600° C. at a heating rate of 5° C. / min and then keep the temperature for 1 hour.
7. The preparation method according to claim 6, characterized in that: The morphology of silicon carbide in the in-situ generated silicon carbide nanostructure-enhanced carbon foam is controlled by adjusting the heat treatment temperature, specifically: When the heat treatment temperature is 1350-1400° C., the generated silicon carbide nanostructure is spherical in shape; When the heat treatment temperature is 1450-1500° C., the generated silicon carbide nanostructure has a bead-like shape; When the heat treatment temperature is 1550-1600° C., the generated silicon carbide nanostructure has a bamboo-like shape.
8. An in-situ generated silicon carbide nanostructure reinforced carbon foam obtained according to the preparation method according to any one of claims 1 to 7.
9. Use of the in-situ generated silicon carbide nanostructure reinforced carbon foam according to claim 8 in the field of electromagnetic absorption materials.
Citation Information
Cited By
Method for preparing core-shell silicon nanowire material by using retired photovoltaic cell silicon wafer and application of core-shell silicon nanowire material