Optical member and method for manufacturing same

By forming a dense TiO2 coating on the titanium or titanium alloy substrate of the protective film frame, the problems of temperature strain and low dust and low outgassing properties under short-wavelength exposure light sources are solved, achieving a lightweight, low-cost The effect of thermal expansion and efficient foreign body capture.

CN118742853APending Publication Date: 2024-10-01NIPPON LIGHT METAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280090396.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-04
Filing Date
2022-11-22
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing protective film frame suffers from strain problems caused by temperature rise when short-wavelength exposure light sources are used, and it is difficult to meet the requirements for low dust and low outgassing properties, especially under extreme ultraviolet irradiation.

Method used

Use titanium or titanium alloy as the base material, and form a dense and homogeneous TiO2 coating on its surface. The sol-gel method and salt catalyst are used to promote the polycondensation reaction of TiO2 to form a high crystallinity ceramic layer to reduce thermal expansion and Captures foreign matter and improves low dust and outgassing properties.

Benefits of technology

A lightweight, low thermal expansion protective film frame is achieved, which significantly reduces the outgassing of hydrogen and other gases under extreme ultraviolet light, enhances the ability to capture foreign matter, and ensures excellent low dust and low outgassing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742853A_ABST
    Figure CN118742853A_ABST
Patent Text Reader

Abstract

Provided are: an optical member which is a lightweight optical member that can be manufactured at a relatively low cost, is capable of suppressing strain caused by a temperature increase, and has excellent low dust raising properties and low gas escape properties; and a method for efficiently manufacturing the optical member. A pellicle frame (1) according to the present invention is characterized by comprising: a base material (4) comprising titanium or a titanium alloy; and a TiO2 coating layer (2) formed on the surface of the base material (4), preferably containing nitrogen in the TiO2 coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical member such as a pellicle frame for a dust cover in an exposure process required in the manufacture of semiconductors, and a method for manufacturing the same. Background Art

[0002] Semiconductor devices such as large scale integration (LSI) and ultra-LSI or liquid crystal panels form patterns by irradiating light to a semiconductor wafer or a liquid crystal master (patterning by photolithography). Here, when using an exposure master with dust attached, the dust absorbs and / or reverses the light, so the pattern cannot be transferred well (for example, the pattern is deformed or the edge is unclear). As a result, the quality and appearance of the semiconductor device or liquid crystal panel are impaired, resulting in problems such as reduced performance or manufacturing yield.

[0003] Therefore, processes related to photolithography are usually performed in a clean room, but even in such an environment, it is impossible to completely prevent dust from adhering to the exposure original plate, so generally a protective film is provided on the surface of the exposure original plate to prevent dust. The protective film includes a protective film frame and a protective film extending on the protective film frame, and is provided to surround the pattern area formed on the surface of the exposure original plate. If the focus is on the pattern of the exposure original plate during photolithography, even if dust is attached to the protective film, the dust will not affect the transfer.

[0004] In recent years, the miniaturization of LSI patterns has been rapidly advancing, and in response, the wavelength of the exposure light source has been continuously shortened. Specifically, the g-ray (wavelength: 436nm) and i-ray (wavelength: 365nm) based on mercury lamps, which have been the mainstream so far, are being replaced by KrF excimer lasers (wavelength: 248nm), ArF excimer lasers (wavelength: 193nm) and F 2 Excimer laser (wavelength: 157nm) and other transitions.

[0005] These short-wavelength exposure light sources are high-output and have high light energy. Therefore, if inorganic acids such as sulfuric acid or phosphoric acid remain in the anodized film on the surface of the aluminum material that forms the protective film, they react with alkaline substances such as ammonia remaining in the exposure environment to form reaction products (mist) such as ammonium sulfate. The reaction products make the protective film turbid, thereby affecting the pattern transfer image.

[0006] In contrast, for example, Patent Document 1 (Japanese Patent Gazette No. 2010-237282) discloses a method for manufacturing a support frame for a protective membrane, which is formed from an aluminum material including aluminum or an aluminum alloy and includes an optical film body and is used as a protective membrane. The method is characterized in that an anodic oxidation film is formed on the surface of the aluminum material by anodizing treatment using an alkaline aqueous solution including tartaric acid, and after dyeing with an organic dye, a sealing treatment is performed using water vapor.

[0007] In the method for manufacturing a support frame for a protective membrane described in Patent Document 1, sulfuric acid, which is the main cause of fog, is not used, but an alkaline aqueous solution containing tartaric acid is used to anodize the aluminum material, thereby obtaining a support frame for a protective membrane that has excellent corrosion resistance and durability and minimizes the generation of fog.

[0008] In addition, the pellicle frame also has other problems. If the strain of the pellicle frame caused by thermal expansion is large, the exposure process cannot be carried out accurately. In particular, with regard to exposure equipment, due to the demand for improved productivity (throughput), the increase in light source output or the miniaturization of circuit line widths have continued to advance, and the exposure light source has been shortened in wavelength. Strain caused by temperature rise in the pellicle frame arranged in the optical path has become a problem.

[0009] In the past, aluminum was used for the pellicle frame due to its low specific gravity and good machinability. However, aluminum has a high linear expansion coefficient, and the aluminum pellicle frame is prone to strain caused by temperature rise. In contrast, the material of the pellicle frame is not limited to aluminum, and research is also underway on the use of ceramics or steel.

[0010] For example, patent document 2 (Japanese Patent Gazette No. 2016-177120) discloses a protective film frame formed in a frame shape, wherein the protective film frame includes a sintered body having a Young's modulus of greater than 150 GPa and a Vickers hardness of greater than 800, wherein the corners in the frame shape ensure a width greater than the width of the straight line portion, and at least one width of the corners is wider than the width of the straight line portion, and the protective film frame is made of ceramic, superhard alloy or metal ceramic.

[0011] In the pellicle frame described in Patent Document 2, a sintered body with high Young's modulus and Vickers hardness is used, so that deformation of the pellicle frame due to film tension generated when the pellicle is extended on the pellicle frame can be suppressed. In addition, the width of at least one corner is wider than the width of the straight portion, so the strength of the corner can be increased, and deformation or damage of the pellicle frame can be further suppressed.

[0012] In addition, patent document 3 (Japanese Patent Gazette No. 2014-085435) discloses a protective film frame, which is made of a metal flat plate by stamping. The protective film frame is characterized in that its cross-section is L-shaped, and the outer surface bent at a right angle from the inner wall surface of the protective film frame toward the outside has a protective film bonding surface, and the end surface connected to the inner wall surface has a mask bonding surface. The protective film frame is made of carbon steel or stainless steel.

[0013] The pellicle frame described in Patent Document 3 is manufactured by press working with excellent mass productivity, so the manufacturing cost is extremely low, and is formed into an L-shaped or U-shaped cross section, so sufficient rigidity required as a pellicle frame can be ensured.

[0014] Prior art literature

[0015] Patent Literature

[0016] Patent Document 1: Japanese Patent Application Publication No. 2010-237282

[0017] Patent Document 2: Japanese Patent Application Publication No. 2016-177120

[0018] Patent Document 3: Japanese Patent Application Publication No. 2014-085435 Summary of the invention

[0019] Problems to be solved by the invention

[0020] However, the pellicle frame described in Patent Document 1 is made of aluminum, and when a shorter wavelength exposure light source is used (when irradiating with extreme ultraviolet rays), strain due to temperature rise becomes a serious problem.

[0021] In addition, the pellicle frame described in Patent Document 2 is made of a raw material that lacks toughness and is very brittle, making it difficult to handle. In addition, it lacks processability and the manufacturing cost is also high. In addition, the specific gravity of the superhard alloy or metal ceramic is high, and the weight of the pellicle frame increases.

[0022] Furthermore, although the pellicle frame described in Patent Document 3 can be manufactured at low cost, carbon steel or stainless steel has a high specific gravity, and the weight of the pellicle frame increases.

[0023] Furthermore, the pellicle housing is required to have low dust emission and low outgassing during extreme ultraviolet ray irradiation, but the pellicle housings described in Patent Documents 1 to 3 cannot be said to fully meet these requirements.

[0024] In view of the problems in the prior art as described above, the object of the present invention is to provide an optical component and an efficient manufacturing method thereof, wherein the optical component is a lightweight optical component such as a protective film frame that can be manufactured relatively inexpensively, can suppress the strain caused by temperature rise, and has excellent low dust generation and low outgassing properties.

[0025] Technical means of solving problems

[0026] In order to achieve the above-mentioned purpose, the inventors have repeatedly studied the material and surface state of optical components, and found that it is extremely effective to use titanium or titanium alloy as the raw material and form TiO on the surface by the sol-gel method. 2 coating, etc., thereby completing the present invention.

[0027] That is, the present invention provides an optical component characterized by having:

[0028] a substrate comprising titanium or a titanium alloy; and

[0029] TiO 2 A coating is formed on the surface of the substrate.

[0030] The optical member of the present invention has both light weight and low thermal expansion because the base material is made of titanium or titanium alloy. 2 The coating has excellent low dust emission and low outgassing properties. 2 The coating also imparts good hydrogen plasma resistance to the optical component of the present invention.

[0031] TiO 2 The coating layer not only has the effect of capturing foreign matter present on the surface of the substrate and suppressing its detachment, but is also a dense and stable ceramic layer, so that even when irradiated with extreme ultraviolet rays, almost no outgassing is generated.

[0032] In the optical member of the present invention, it is preferred that the TiO 2 The coating contains nitrogen. The nitrogen comes from the TiO formed by the sol-gel method. 2 Salt catalyst during coating. By using salt catalyst, the formation of TiO 2 The Ti alkoxide of the coating material undergoes polycondensation to form a dense and homogeneous TiO 2 Coating, thereby more reliably ensuring the capture effect and low outgassing of different materials.

[0033] In the optical member of the present invention, it is preferred that a through hole exists in the substrate, and the TiO 2When a through hole exists in the substrate, it is extremely difficult to completely remove foreign matter attached to the inner surface of the through hole. However, in the optical component of the present invention, a dense and homogeneous TiO2 coating is formed on the inner surface of the through hole by a sol-gel method. 2 Coating, thus ensuring excellent low dusting properties.

[0034] In the optical member of the present invention, the amount of hydrogen gas generated by extreme ultraviolet irradiation is preferably 1.2 times or less the amount of hydrogen gas generated when the substrate is irradiated with extreme ultraviolet light under the same conditions. 2 The coating is a dense, homogeneous and chemically stable ceramic layer. Even when exposed to extreme ultraviolet light, the TiO 2 The outgassing generated by the coating also becomes extremely small. As a result, the amount of hydrogen generated by extreme ultraviolet irradiation can be set to 1.2 times or less of the amount of hydrogen generated when the substrate is irradiated with extreme ultraviolet rays under the same conditions. The more preferred amount of hydrogen generated is 1.1 times or less, and the most preferred amount of hydrogen generated is 1.05 times or less.

[0035] In the optical member of the present invention, when immersed in 3 L of pure water and subjected to ultrasonic irradiation for 1 minute, the number of particles having a particle size of 1 μm to 15 μm in 50 ml of the pure water is preferably 600 particles / 68 cm 2 In the optical member of the present invention, dense and homogeneous TiO 2 Since the coating captures foreign matter, even under severe conditions such as immersing the optical member in pure water and irradiating it with ultrasonic waves, the detachment of foreign matter (particles) can be extremely effectively suppressed.

[0036] In the optical member of the present invention, when immersed in 3 L of pure water and subjected to ultrasonic irradiation for 1 minute, the number of particles having a particle size of 0.5 μm to 1 μm in 50 ml of the pure water is preferably 2000 particles / 68 cm 2 In the optical member of the present invention, dense and homogeneous TiO 2 Since the coating captures foreign matter, even under severe conditions such as immersing the optical member in pure water and irradiating it with ultrasonic waves, the detachment of foreign matter (particles) can be extremely effectively suppressed.

[0037] The optical component of the present invention is preferably set as a protective film frame, but there is no special limitation as long as the effect of the present invention is not impaired. For example, it can be set as various existing well-known optical parts (casings, various support parts inside the casing, shutter blades and apertures, etc.) that constitute optical devices such as digital cameras, digital video cameras and mobile phones with cameras.

[0038] In addition, the present invention also provides a method for manufacturing an optical component, characterized by comprising:

[0039] an optical member substrate manufacturing step of processing a substrate made of titanium or a titanium alloy into a shape of an optical member substrate; and

[0040] In a coating step, TiO is formed on the surface of the optical member substrate by a sol-gel method. 2 coating,

[0041] In the coating step, a salt catalyst containing nitrogen is used.

[0042] The method for manufacturing an optical component of the present invention is characterized in that: (1) the optical component substrate is made of titanium or a titanium alloy; (2) a sol-gel method is used; and (3) a salt catalyst containing nitrogen is used in the sol-gel method. In particular, by using a salt catalyst, a dense and homogeneous TiO2 layer can be efficiently formed on the entire surface of the substrate. 2 coating.

[0043] In the method for manufacturing an optical member of the present invention, it is preferred that a through hole is formed in the optical member substrate in the optical member substrate manufacturing step, and the TiO2 is also formed on the inner surface of the through hole in the coating step. 2 In the method for producing the optical member of the present invention, the sol-gel method is used, so TiO can be easily formed inside the through-hole. 2 In particular, by performing dip coating, TiO can be easily and efficiently formed inside the through-holes. 2 coating.

[0044] In the method for producing an optical member of the present invention, a salt catalyst containing nitrogen is used to promote the polycondensation reaction of the coating raw material, and even when TiO is formed by low-temperature calcination at about 200°C to 300°C, 2 In the case of coating, it can also promote TiO 2 As a result, the final TiO 2 The coating layer is a good ceramic layer with high crystallinity.

[0045] Effects of the Invention

[0046] According to the present invention, an optical member that is lightweight and can be manufactured at a relatively low cost, can suppress strain caused by temperature rise, and has excellent low dust emission and low outgassing properties, and an efficient manufacturing method thereof can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] [ Figure 1 ] is a three-dimensional diagram of the protective film frame of the implementation form.

[0048] [ Figure 2 ] is a CC' cross-sectional view of the protective film frame of the implementation form.

[0049] [ Figure 3 ] is a process diagram of a method for manufacturing a protective film frame according to an embodiment.

[0050] [ Figure 4 ] is a SEM photograph of the protective film frame 1.

[0051] [ Figure 5 ] is a SEM photograph of the protective film frame 2.

[0052] [ Figure 6 ] is a SEM photograph of the comparative pellicle frame 1.

[0053] [ Figure 7 ] is a SEM photograph of the comparative pellicle frame 2.

[0054] [ Figure 8 ] is a SEM photograph of the comparative pellicle frame 4.

[0055] [ Fig. 9 ] is an IR spectrum of the protective film frame 1.

[0056] [ Fig.10 ] is the IR spectrum of the protective film frame 2.

[0057] [ Fig.11 ] is the IR spectrum of the pellicle frame 1 for comparison.

[0058] [ Fig.12 ] is the IR spectrum of the comparative pellicle frame 2.

[0059] [ Fig.13 ] is the IR spectrum of the comparative pellicle frame 4.

[0060] [ Fig.14 ] is the measurement result of hydrogen.

[0061] [ Fig.15 ] is the measurement result of water and ammonia.

[0062] [ Fig.16 ] is the measurement result of hydrocarbons. DETAILED DESCRIPTION

[0063] Below, the protective film frame is set as a representative example, and the representative embodiments of the optical component and the manufacturing method thereof of the present invention are described in detail with reference to the accompanying drawings, but the present invention is not limited to these. In addition, the components in the embodiment may be appropriately combined in part or in whole. In addition, in the following description, the same or equivalent parts are marked with the same symbols, and repeated descriptions are sometimes omitted. In addition, since the accompanying drawings are used to conceptually illustrate the present invention, the dimensions of the components shown or their ratios are sometimes different from the actual ones.

[0064] 1. Protective film frame

[0065] like Figure 1 and Figure 2 As shown, the protective film frame 1 is composed of a TiO 2 The coating 2 is formed of a frame 4 made of titanium or a titanium alloy.

[0066] Since frame 4 is made of titanium or titanium alloy, it has higher strength and Young's modulus than conventional pellicle frames made of aluminum alloy. In addition, titanium and titanium alloys have a specific gravity of about 4.5 and are relatively light, which can suppress the increase in weight of pellicle frame 1.

[0067] As long as the effect of the present invention is not impaired, the titanium alloy used for the frame 4 is not particularly limited, and various titanium alloys known in the art can be used. Examples of the titanium alloy include Ti-6Al-4V alloy, Ti-6Al-6V-2Sn alloy, Ti-6Al-2Sn-4Zr-6Mo alloy, Ti-10V-2Fe-3Al alloy, Ti-7Al-4Mo alloy, Ti-5Al-2.5Sn alloy, Ti-6Al-5Zr-0.5Mo-0.2Si alloy, Ti-5.5Al-3.5Sn-3Zr-0.3Mo-1Nb-0.3 Si alloy, Ti-8Al-1Mo-1V alloy, Ti-6Al-2Sn-4Zr-2Mo alloy, Ti-5Al-2Sn-2Zr-4Mo-4Cr alloy, Ti-11.5Mo-6Zr-4.5Sn alloy, Ti-15V-3Cr-3Al-3Sn alloy, Ti-15Mo-5Zr-3Al alloy, Ti-15Mo-5Zr alloy, or Ti-13V-11Cr-3Al alloy, etc.

[0068] From the perspective of ensuring good processability or purity, it is preferred to use titanium (pure titanium). From the perspective of achieving both high strength and good processability, it is preferred to use an α+β type alloy. From the perspective of material price or ease of acquisition, it is preferred to use a Ti-6Al-4V alloy.

[0069] As long as the effect of the present invention is not impaired, the shape of the protective film frame 1 is not particularly limited and can be set to various existing known shapes according to the shape of the exposure original plate. However, in general, the planar shape of the protective film frame 1 is annular, rectangular or square, and has a size and shape that covers the circuit pattern portion set on the exposure original plate.

[0070] The height (thickness) of pellicle frame 1 is preferably 0.5 mm to 10 mm, more preferably 1 mm to 7 mm, and most preferably 1.0 mm to 3.0 mm. By setting the height (thickness) of pellicle frame 1 to these values, deformation of pellicle frame 1 can be suppressed and good operability can be ensured.

[0071] As long as the effects of the present invention are not impaired, the cross-sectional shape of the pellicle frame 1 is not particularly limited, and can be set to various shapes known in the art, but is preferably set to a quadrilateral with parallel upper and lower sides. The upper side of the pellicle frame 1 needs to have a width for expanding the pellicle film, and the lower side needs to have a width for setting a bonding adhesive layer and bonding with the exposure original. For the above reasons, the width (W) of the upper and lower sides of the pellicle frame 1 is preferably set to about 1 mm to 3 mm.

[0072] The flatness of the pellicle frame 1 is preferably set to 30 μm or less, and more preferably set to 20 μm or less. By improving the flatness of the pellicle frame 1, the deformation of the exposure original when the pellicle is attached to the exposure original can be reduced. In addition, the flatness of the pellicle frame 1 can be calculated by measuring the height at a total of 8 points, 4 points at each corner of the pellicle frame 1 and 4 points in the center of the four sides, to calculate a virtual plane, and using the difference obtained by subtracting the lowest point from the highest point in the distance from each point of the virtual plane.

[0073] TiO 2 The coating 2 is formed by a sol-gel method, preferably on a TiO 2 The coating 2 contains nitrogen. The nitrogen is derived from the TiO formed by the sol-gel method. 2 Salt catalyst in coating 2. By using a salt catalyst, the formation of TiO 2 The Ti alkoxide of the raw material of coating 2 undergoes polycondensation reaction to form a dense and homogeneous TiO 2 The coating 2 can thereby more reliably ensure the capture effect of different materials and low outgassing. Here, the method for detecting nitrogen is not particularly limited, and various conventional element analysis methods can be used.

[0074] TiO 2 The coating layer 2 is formed on the entire surface of the frame body 4. The film thickness is not particularly limited unless the effects of the present invention are impaired, but is preferably 10 nm to 50 μm.

[0075] In addition, it is preferred that a through hole (not shown) is present in the pellicle frame 1, and a TiO 2 Coating 2. When there is a through hole in the frame 4, it is extremely difficult to completely remove foreign matter attached to the inner surface of the through hole. However, by forming a dense and homogeneous TiO 2 Coating 2 ensures excellent low dusting properties.

[0076] In the pellicle frame 1, the amount of hydrogen gas generated by extreme ultraviolet ray irradiation is preferably 1.2 times or less the amount of hydrogen gas generated when the frame 4 is irradiated with extreme ultraviolet rays under the same conditions. 2 Coating 2 is a dense, homogeneous and chemically stable ceramic layer. Even when irradiated with extreme ultraviolet light, the TiO 2 The outgassing generated by the coating 2 also becomes extremely small. As a result, the amount of hydrogen generated by extreme ultraviolet irradiation can be set to 1.2 times or less of the amount of hydrogen generated when the frame 4 is irradiated with extreme ultraviolet rays under the same conditions. The more preferred amount of hydrogen generated is 1.1 times or less, and the most preferred amount of hydrogen generated is 1.05 times or less.

[0077] In addition, regarding outgassing during extreme ultraviolet irradiation, the generation of outgassing is not limited to hydrogen. For example, C 3 H 5 The method for measuring the amount of these outgases generated is not particularly limited, and various conventionally known gas analysis methods can be used.

[0078] In addition, in the pellicle frame 1, when it is immersed in 3 L of pure water and subjected to ultrasonic irradiation for 1 minute, the number of particles having a particle size of 1 μm to 15 μm in 50 ml of the pure water is preferably 600 particles / 68 cm 2 In the pellicle frame 1, a dense and homogeneous TiO 2 Since coating layer 2 captures foreign matter, even under severe conditions such as immersing pellicle frame 1 in pure water and irradiating it with ultrasonic waves, it is possible to extremely effectively suppress the detachment of foreign matter (particles).

[0079] Here, when the pellicle frame 1 is immersed in 3L of pure water and subjected to ultrasonic irradiation for 1 minute, the particles to be suppressed from detaching are not limited to particles having a particle size of 1μm to 15μm. For example, the number of particles present in 50ml of pure water is preferably 2000 particles / 68cm when the particle size is 0.5μm to 1μm. 2 the following.

[0080] 2. Method for manufacturing protective film frame

[0081] like Figure 3 As shown, the manufacturing method of the pellicle frame of this embodiment comprises: a frame (optical member substrate) manufacturing step (S01) of processing a substrate including titanium or a titanium alloy into the shape of a frame 4; and a coating step (S02) of forming TiO on the surface of the frame 4 using a sol-gel method. 2 Coating 2. Hereinafter, each step and the like will be described in detail.

[0082] (1) Frame production process (S01)

[0083] The frame manufacturing step ( S01 ) is a step for obtaining frame 4 , and is a step for obtaining frame 4 of pellicle frame 1 with high dimensional accuracy by performing bonding and cutting on titanium or titanium alloy material as necessary.

[0084] When the titanium or titanium alloy material has a sufficient size, the frame 4 can be cut out from the material. On the other hand, the frame 4 can also be obtained by joining the titanium or titanium alloy material, in which case the yield of the titanium or titanium alloy material can be improved. Here, it is preferred to use solid phase bonding in the joining of the titanium or titanium alloy material. By using solid phase bonding, the strain generated in the joint can be suppressed, and the difference in mechanical properties between the joint and the parent material can be reduced. In addition, the frame 4 obtained by cutting out or joining can also be further cut.

[0085] In addition, it is preferable to form a through hole in the frame 4, and to form a TiO film on the inner surface of the through hole in the coating step (S02). 2 Coating 2. Since the sol-gel method is used in the coating step (S02), TiO can be easily formed inside the through-hole. 2 Coating 2.

[0086] (2) Coating step (S02)

[0087] The coating step (S02) is to form TiO on the surface of the frame 4 obtained in the substrate preparation step (S01). 2 Coating 2 process.

[0088] As a pre-treatment of the coating step (S02), it is preferable to degrease the frame 4. Specifically, the frame 4 can be cleaned with acetone or the like, then cleaned with pure water and dried to remove oil. In addition, in order to smooth the surface, the frame 4 is preferably subjected to chemical polishing.

[0089] Next, Ti alkoxide was used as TiO 2 The raw material of the coating 2 can form TiO on the surface of the frame 4 through the hydrolysis and polycondensation reaction of Ti alkoxide. 2Coating 2. The method of coating the surface of the frame 4 with Ti alkoxide is not particularly limited unless the effects of the present invention are impaired, but it is preferred to immerse the frame 4 (immersion coating). By performing immersion coating, TiO can be formed simply and efficiently. 2 Coating 2.

[0090] TiO 2 The morphology of the coating 2 changes depending on the degree of hydrolysis and subsequent polymerization of the Ti alkoxide. Specifically, if hydrolysis is suppressed and polycondensation is promoted, low-dimensional growth occurs, and if hydrolysis is promoted and polycondensation is suppressed, high-dimensional growth occurs. Here, since gelation occurs in the case of low-dimensional growth, it is preferred to promote polycondensation when a Ti alkoxide with a slow polycondensation rate is used as a raw material.

[0091] In addition, in the TiO 2 A salt catalyst containing nitrogen is used in the process of forming the coating layer 2. By using a salt catalyst containing nitrogen, the polycondensation reaction can be accelerated.

[0092] In addition, by low-temperature heating the Ti alkoxide gelled on the surface of the frame 4, a dense and homogeneous TiO 2 Coating 2. The heating temperature is not particularly limited unless the effects of the present invention are impaired. 2 The state of the coating layer 2 can be adjusted appropriately, and preferably low-temperature heating at 200°C to 300°C is performed. The polycondensation reaction of Ti alkoxide is promoted by using a salt catalyst, and even when TiO is formed by low-temperature calcination at about 200°C to 300°C, 2 In the case of coating, TiO 2 As a result, the final TiO 2 The coating layer 2 is a good ceramic layer with high crystallinity.

[0093] As mentioned above, although the representative embodiments of the present invention have been described, the present invention is not limited to these, and various design changes can be made, and all of these design changes are included in the technical scope of the present invention.

[0094] Example

[0095] 《Example 1》

[0096] A 50 mm × 50 mm × 1.5 mm optical component substrate was cut out from a 2 mm thick pure titanium plate (optical component substrate production process), and the surface was smoothed by chemical polishing. Next, Ti alkoxide was used as a raw material, and TiO was formed on the entire surface of the frame by a sol-gel method. 2Coating (coating process): In the coating process, a nitrogen-containing salt catalyst is used to form a gelled Ti alkoxide layer on the entire surface of the frame by immersion coating. The frame is immersed in the raw material at a speed of 5 mm / s and the pulling speed is 1 mm / s.

[0097] Next, the frame with a gelled Ti alkoxide layer formed on the entire surface was calcined at 300°C for 2 h to form TiO 2 The pellicle frame 1 as an embodiment of the present invention was obtained. The TiO 2 The coating thickness was found to be 20 nm to 30 nm.

[0098] 《Example 2》

[0099] A pellicle frame 2 was obtained in the same manner as in Example 1 except that the calcination temperature was 200°C.

[0100] Comparative Example 1

[0101] A comparative pellicle frame 1 was obtained in the same manner as in Example 1 except that "Honnyceran PI-20" manufactured by Honny Chemicals Co., Ltd. was dip-coated on the entire surface of the frame and the calcination conditions were set at 150° C. for 1 hour.

[0102] "Honnyceran PI-20" is a sintered 1-component paint for glass raw materials with polysiloxane resin as the main component. It forms SiO on the surface of the frame by calcination. 2 coating.

[0103] Comparative Example 2

[0104] Comparative pellicle frame 2 was obtained in the same manner as in Example 1 except that "Sanserazan #200-1" manufactured by Sanwa Chemical Co., Ltd. was dip-coated on the entire surface of the frame and the calcination conditions were set at 150° C. for 1 hour.

[0105] "Sanserazan #200-1" is a mixture of 1% inorganic polysilazane and 90% to 99% dibutyl ether. It forms SiO on the surface of the frame by calcination. 2 coating.

[0106] 《Comparative Example 3》

[0107] A comparative pellicle frame 3 was obtained in the same manner as in Example 1 except that chemical polishing and coating treatment were not performed.

[0108] 《Comparative Example 4》

[0109] A comparative pellicle frame 4 was obtained in the same manner as in Example 1 except that the coating process was not performed.

[0110] [evaluate]

[0111] (1) Surface morphology changes caused by extreme ultraviolet radiation

[0112] The surface of each pellicle frame was irradiated with 4W / cm 2 The surface conditions before and after irradiation were observed using a scanning electron microscope (manufactured by Carl Zeiss, ULTRA PLUS). Scanning electron microscope (SEM) photographs of the pellicle frame 1, pellicle frame 2, comparative pellicle frame 1, comparative pellicle frame 2, and comparative pellicle frame 4 are shown in FIG. Figure 4 , Figure 5 , Figure 6 , Figure 7 and Figure 8 .

[0113] In the pellicle frame 1 and the pellicle frame 2, no cracks were generated due to the irradiation of extreme ultraviolet rays, and a good surface condition was maintained. On the other hand, in the comparative pellicle frame, it was found that the coating was uneven since before the irradiation, and the film forming property was poor. In addition, in the comparative pellicle frame 2, peeling of the coating due to the irradiation was also confirmed.

[0114] The infrared (IR) spectrum of the surface before and after extreme ultraviolet irradiation was measured. The Fourier-Transform Infrared Spectroscopy (FT-IR) 660-IR / 620-IR manufactured by Agilent Technology was used for the measurement. The IR spectra of the implemented pellicle frame 1, implemented pellicle frame 2, comparative pellicle frame 1, comparative pellicle frame 2, and comparative pellicle frame 4 are shown in FIG. Fig. 9 , Fig.10 , Fig.11 , Fig.12 and Fig.13 .

[0115] In pellicle frame 1 and pellicle frame 2, no significant change was observed in the IR spectrum by irradiation with extreme ultraviolet rays, indicating that a good surface condition was maintained.

[0116] (2) Measurement of outgassing associated with extreme ultraviolet irradiation

[0117] Each pellicle frame was placed in a vacuum chamber and evacuated. Next, the ultraviolet light was measured in the range of 1amu to 200amu before irradiation. Next, 4W / cm 2 After irradiating the extreme ultraviolet rays, the mass peak was measured in the range of 1amu to 200amu for 12 minutes. Next, after irradiating the extreme ultraviolet rays to different areas, the change over time (0 minutes to 30 minutes) was measured using a specific amu.

[0118] The results of hydrogen gas measurement are shown in Fig.14 , the results of water and ammonia determination are shown in Fig.15 The results of hydrocarbon determination are shown in Fig.16 . Regarding hydrogen and hydrocarbons, it is known that TiO 2 The amount of gas discharged from the coated pellicle frame 1 and the pellicle frame 2 was significantly reduced. In addition, the amount of water and ammonia was also poor when the coating was not applied, but it was different from the amount of gas discharged from the coated pellicle frame 1 and the pellicle frame 2 when the coating was applied. 2 Compared with the coating case, the discharge volume is significantly reduced.

[0119] (3) Evaluation of dust emission

[0120] The dust emission was evaluated by the particle-in-liquid evaluation. Specifically, a glass beaker was ultrasonically cleaned with pure water, 3 L of pure water was stored in the beaker, and a liquid particle counter (NP500T manufactured by Nippon Denshoku Industries Co., Ltd.) was used to measure the blank value.

[0121] Next, the pellicle frame was immersed in pure water and irradiated with ultrasonic waves for 1 minute. After that, the pellicle frame was extracted and the number of particles in 50 ml of pure water was measured using a liquid particle counter. The results obtained are shown in Table 1. In addition, the values ​​in Table 1 are converted values ​​(pieces / 68 cm 2 ).

[0122] [Table 1]

[0123]

[0124] In the formation of SiO 2 In the case of the coating (Comparative pellicle frame 1 and Comparative pellicle frame 2), the amount of dust generated due to the formation of the coating was not reduced, and a tendency of an increase in the amount of dust was confirmed compared to the state of chemical polishing alone (Comparative pellicle frame 4). 2 The amount of dust generated by the coated pellicle frame 1 and the coated pellicle frame 2 is significantly reduced.

[0125] (4) Evaluation of ion elution amount

[0126] The pellicle frame was immersed in 100 ml of pure water in a polyethylene bag, placed in a 90°C water bath and left to stand for 3 hours. Afterwards, it was moved to a room temperature water bath for cooling and then analyzed by ion chromatography (anion) and absorptiometry (NH 4 ) was used to measure the amount of ions in pure water (protective film frame immersion liquid). ThermoIntegrion RFIC was used as an ion chromatograph, and Spectrophotometer V-630 manufactured by JASCO was used for the absorptiometry. The obtained results are shown in Table 2.

[0127] [Table 2]

[0128] (Unit: ppb / 68cm 2 )

[0129]

[0130] In the formation of TiO 2 No significant increase in the amount of ion elution was observed in the coated pellicle frame 1 and the coated pellicle frame 2, indicating that the pellicle frame of the present invention also has good characteristics from the viewpoint of the amount of ion elution.

[0131] Explanation of symbols

[0132] 1: Protective film frame

[0133] 2: TiO 2 coating

[0134] 4: Frame

Claims

1. An optical component, characterized in that have: a substrate comprising titanium or a titanium alloy; and A TiO2 coating is formed on the surface of the substrate.

2. The optical component according to claim 1, wherein Nitrogen is contained in the TiO2 coating.

3. The optical component according to claim 1 or 2, characterized in that: There are through holes in the substrate, The TiO2 coating layer is also formed on the inner surface of the through hole.

4. The optical component according to claim 1 or 2, characterized in that: The amount of hydrogen gas generated by extreme ultraviolet ray irradiation is 1.2 times or less the amount of hydrogen gas generated when the substrate is irradiated with extreme ultraviolet rays under the same conditions.

5. The optical component according to claim 1 or 2, characterized in that: When the sample was immersed in 3 L of pure water and subjected to ultrasonic irradiation for 1 minute, the number of particles having a particle size of 1 μm to 15 μm in 50 ml of the pure water was 600 particles / 68 cm 2 the following.

6. The optical component according to claim 1 or 2, characterized in that: When the sample was immersed in 3 L of pure water and subjected to ultrasonic irradiation for 1 minute, the number of particles having a particle size of 0.5 μm to 1 μm in 50 ml of the pure water was 2000 particles / 68 cm 2 the following.

7. A method for manufacturing an optical component, characterized in that have: an optical member substrate manufacturing step of processing a substrate including titanium or a titanium alloy into a shape of an optical member substrate; as well as A coating step of forming a TiO2 coating layer on the surface of the optical member substrate using a sol-gel method, In the coating step, a salt catalyst containing nitrogen is used.

8. The method for manufacturing an optical component according to claim 7, wherein: In the optical member substrate manufacturing step, a through hole is formed in the optical member substrate. In the coating step, the TiO 2 coating layer is also formed on the inner surface of the through hole.