Multifunctional catalytic and dust removal composite metal filter cartridge and preparation method thereof

By designing a multi-functional catalytic and dust removal composite metal filter cartridge, fiber products and modifiers are used to improve the load and stability of the catalyst, the existing equipment with high temperature dust removal and denitrification technology has solved the problem of large area, high cost and maintenance difficulties, and achieved multiple results Efficient treatment and environmental protection effects of pollutants.

CN118751233BActive Publication Date: 2024-12-06HANGZHOU XIFU ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410855079.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-12-06
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

The existing high-temperature dust removal and denitrification technology has the problems of large equipment area, high cost, difficult maintenance and low treatment efficiency of multiple pollutants. Especially in the chemical and environmental protection fields, a more convenient and efficient flue gas multi-pollutants are needed. Processing method.

Method used

Using a multifunctional catalytic and dust removal composite metal filter cartridge, it is made of fiber products, has a large specific surface area and a stable channel structure, and improves the load capacity and stability of the catalyst through modifiers to realize the integrated design of multi-layer catalytic layers. , reduce the number of equipment and land occupation, and improve the catalytic effect.

Benefits of technology

It realizes efficient catalytic reactions of a variety of pollutants, reduces operating costs and environmental pollution, extends the service life of the equipment, improves heat recovery rate, avoids dust clogging and catalyst poisoning, and simplifies maintenance and waste catalyst recycling and treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751233B_ABST
    Figure CN118751233B_ABST
Patent Text Reader

Abstract

The present invention discloses a multifunctional catalytic and dust removal composite metal filter cartridge and a preparation method thereof. The preparation method steps are as follows: S1: dispersing and mixing inorganic fibers, organic fibers, inorganic binders, organic binders, modifiers and water to prepare slurry; S2: molding the slurry in a mold, and calcining to form a plurality of mutually nested catalytic layer substrates; S3: impregnating a plurality of catalytic layer substrates with catalyst slurry, and obtaining catalytic layers after drying and calcining; S4: inserting a plurality of catalytic layers into the bracket in sequence, and then arranging a porous metal film on the outer side of the outermost catalytic layer to form a filter cartridge body, connecting and assembling a plurality of filter cartridge bodies, and installing flanges and sealing bottom covers at both ends, respectively, to obtain a multifunctional catalytic and dust removal composite metal filter cartridge. The multifunctional catalytic and dust removal composite metal filter cartridge prepared by the present invention has excellent catalytic dust removal performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flue gas treatment, and in particular to a multifunctional catalytic and dust-removing composite metal filter cartridge and a preparation method thereof. Background Art

[0002] At present, high-temperature dust removal and denitrification are attracting more and more attention. Dust removal at a higher temperature stage can not only improve the recovery efficiency of waste heat in the second half of the flue gas, but also reduce the blockage of pipelines caused by high dust. At the same time, after dust removal at high temperature, the dust content of flue gas is low, which reduces the mechanical scouring, dust blockage, catalyst poisoning and other problems caused by dust on the catalyst, greatly improving the service life of the catalyst. In addition, it also avoids the temperature resistance defects of traditional dust removal bags. The flue gas needs to be cooled and dusted before denitrification. At this time, the flue gas temperature is low, and the low-temperature performance requirements of the catalyst are high. ABS is easily formed at low temperatures, which affects the denitrification reaction.

[0003] With the promotion of high-temperature dust removal and denitrification technology, the current mainstream product technologies are mainly catalytic ceramic fiber filter cartridges and metal dust removal filter bags + SCR catalysts. Catalytic ceramic fiber filter cartridges are mainly to implant catalysts inside catalytic ceramic fiber tubes. When the flue gas passes through the ceramic fiber tube, the dust is first filtered, and then the flue gas passes through the catalytic layer of the ceramic fiber tube to react and remove NO in the flue gas. X . Ceramic fiber tubes are mainly composed of aluminum silicate ceramic fibers and binders, so considering the actual use intensity, the general length of ceramic fiber tubes is 2-3m. Despite this, there are still many broken tubes in actual use, and due to the limited length of ceramic fiber tubes, in order to ensure the filtration wind speed between 0.8-1.2m / min, more chambers will be set up, resulting in a large footprint and one-time investment. In order to ensure the filtration accuracy and strength, more fibers are used in the tube body during manufacturing, the pores are relatively small, and the density is high. Therefore, the pressure difference during operation is relatively large, and the system consumes more energy. Another metal dust filter bag + SCR catalyst process mainly uses a porous metal membrane to filter the flue gas to remove most of the dust, and then a single-layer or multi-layer SCR denitrification catalyst layer is set behind the metal filter bag. Various forms of traditional SCR catalysts are mainly used, such as honeycomb catalysts, corrugated plate catalysts, and plate catalysts. The length of the metal filter bag can reach 2-9 meters, but in order to achieve denitrification, an additional mechanism is required to install the catalyst, which increases the installation cost to a certain extent and reduces the space utilization rate. At the same time, when the service life increases and single or multiple metal membranes are perforated, the dust directly passes through the defects and reaches the catalytic layer, which will block the post-catalyst and is difficult to clean and maintain.

[0004] In the fields of chemical industry and environmental protection, the types and concentrations of flue gas pollutants are becoming more and more stringent. For example, in addition to denitrification and dust removal, it also involves the removal of VOCs and CO, and the removal of various pollutants such as ammonia. To achieve other functions on the basis of the current high-temperature dust removal and denitrification, it is necessary to set up new equipment or add new catalyst layers, which requires a larger one-time investment. The more environmental protection devices are introduced, the greater the operating resistance and operating cost of the entire system will be.

[0005] In order to solve the shortcomings of the two current high-temperature dust removal and denitrification processes, and on this basis provide a more convenient and less investment method for treating multiple types of pollutants in flue gas, the development of a multifunctional multifunctional catalytic and dust removal composite metal filter cartridge is the key to solving the above problems. Summary of the invention

[0006] Based on the technical problems existing in the background technology, the present invention proposes a multifunctional catalytic and dust removal composite metal filter cartridge and a preparation method thereof. The prepared first catalytic layer substrate and the second catalytic layer substrate have a larger specific surface area and a more stable pore structure, can load more catalysts, and the catalysts in the first catalytic layer substrate and the second catalytic layer substrate are highly stable, thereby improving the catalytic effect of the first catalytic layer and the second catalytic layer.

[0007] The preparation method of the multifunctional catalytic and dust removal composite metal filter cartridge proposed by the present invention comprises the following steps:

[0008] S1: dispersing and mixing inorganic fibers, organic fibers, inorganic binders, organic binders, modifiers and water to prepare slurry;

[0009] S2: forming the slurry in a mold, and calcining it to form a plurality of catalyst layer substrates that can be nested with each other;

[0010] S3: impregnating a plurality of catalyst layer substrates with catalyst slurry, and obtaining a catalyst layer after drying and calcination;

[0011] S4: inserting the support (14) into a plurality of catalytic layers in sequence, and then arranging a porous metal membrane (11) on the outer side of the outermost catalytic layer to form a filter cartridge body (1), connecting and assembling a plurality of filter cartridge bodies (1), and installing flanges (2) and sealing bottom covers (3) at both ends, respectively, to obtain a multifunctional catalytic and dust removal composite metal filter cartridge;

[0012] The modifier is composed of potato starch, seaweed polysaccharide and chitosan in a mass ratio of 2:1-4:1-4.

[0013] Preferably, the slurry in S1 comprises the following raw materials in parts by weight: 10-20 parts of inorganic fibers, 2-8 parts of organic fibers, 4-8 parts of inorganic binders, 1-5 parts of organic binders, 0.5-1.5 parts of modifiers and 100 parts of water.

[0014] Preferably, the inorganic fiber is one or more of aluminum silicate fiber, alumina fiber, glass fiber, and zirconium oxide fiber; the organic fiber is one or more of plant fiber, polyvinyl alcohol fiber, nylon fiber, polypropylene fiber, and polyester fiber; the inorganic binder is one or more of sodium silicate, silica sol, and aluminum sol; the organic binder is one or more of epoxy resin, silicone, and sodium carboxymethyl cellulose.

[0015] Preferably, the catalytic layer comprises a first catalytic layer (12) and a second catalytic layer (13), the first catalytic layer (12) is impregnated with a denitration catalytic slurry, and the second catalytic layer (13) is impregnated with a decarbon monoxide catalytic slurry;

[0016] The denitration catalytic slurry comprises the following raw materials in parts by weight: 80-90 parts of denitration catalytic powder, 5-10 parts of nano-silicon dioxide, 1-5 parts of an auxiliary agent, and the balance is water;

[0017] The carbon monoxide removal catalytic slurry comprises the following raw materials in parts by weight: 70-90 parts of carbon monoxide removal catalytic powder, 5-10 parts of nano silicon dioxide, 1-5 parts of an auxiliary agent, and the balance is water;

[0018] The solid content of the denitration catalytic slurry and the decarbon monoxide catalytic slurry is 5-25%.

[0019] Preferably, the denitration catalytic powder is composed of titanium dioxide and vanadium pentoxide in a mass ratio of 10:2-6; the decarbon monoxide catalytic powder is composed of aluminum oxide, platinum oxide and palladium oxide in a mass ratio of 100:0.1-3:0.1-3.

[0020] Preferably, the auxiliary agent is one or more of ethylene glycol, polyvinyl pyrrolidone, polyoxyethylene alkyl ether, aluminum sol and sodium hexametaphosphate.

[0021] Preferably, the catalyst slurry is processed by a ball mill with a rotation speed of 200-400 rpm, the ball milling medium is 0.6-0.8 mm zirconium oxide beads, the material-ball ratio is 1:10-20, and the grinding time is 10-20 hours.

[0022] Preferably, the calcination temperature in S2 is 300-450° C., the heating rate is 2-5° C. / min, and the calcination time is 4-8 h.

[0023] Preferably, the calcination temperature in S3 is 400-500° C., the heating rate is 5-10° C. / min, and the calcination time is 4-8 h.

[0024] The invention provides a multifunctional catalytic and dust-removing composite metal filter cartridge prepared by the method mentioned above.

[0025] Beneficial technical effects of the present invention:

[0026] (1) The present invention uses fiber products as the catalyst layer matrix. The pores formed on the surface of the inorganic fibers and between the fibers can provide more catalytic powder loading sites, which is convenient for catalytic powder loading. The catalytic powder loading amount can be easily controlled by adjusting the solid content of the active liquid, and it is not easy to fall off. In addition, the present invention can further increase the specific surface area of ​​the catalyst layer matrix and the stability of the pore structure by adding a modifier, thereby improving the catalytic effect of the catalyst layer.

[0027] (2) The present invention can easily complete the catalytic reaction of various types of pollutants through the assembly of single-layer or multi-layer catalytic layers, avoiding the cumbersome setting of the exhaust gas purification device, reducing the one-time investment to a certain extent, and setting up catalytic layers separately for different catalytic reactions to avoid mutual interference or reaction between catalytic powders, which is beneficial to the catalytic reaction. The highly integrated filter cartridge also avoids the loss of flue gas heat and improves the heat recovery rate.

[0028] (3) In the dust removal process of the present invention, the resistance has a great impact on the operating cost. Although two layers of catalyst layers are added, the catalyst layer has a very low resistance due to its large pores and high porosity, which has little effect on the increase of system resistance and saves operating costs; when the filter cartridge is damaged, it is only necessary to cut the bin to replace the damaged filter cartridge in the bin. Compared with the traditional dust removal + SCR catalyst combination process, there will be no problem of dust blocking the entire honeycomb, corrugated plate and other catalyst layers after the filter cartridge is perforated, causing long-term shutdown and difficulty in dust cleaning; after reaching the service life, the metal film and catalyst layer can be disassembled and processed separately, and different catalytic powder raw materials are different. The layered coating assembly also facilitates the recovery and processing of waste catalysts in the later stage and avoids cross contamination. The metal film of the exhaust gas filter cartridge can be recycled and reused, and the failed or inefficient catalyst layer adopts a fiber matrix, which has more load positions and can be re-coated with active liquid and reused, which can reduce environmental pollution to a certain extent and reduce replacement costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the structure of the multifunctional catalytic and dust removal composite metal filter cartridge proposed by the present invention;

[0030] Figure 2 This is a partial AA enlarged view of the multifunctional catalytic and dust-removing composite metal filter cartridge proposed by the present invention.

[0031] In the figure: 1-filter cartridge body, 11-porous metal membrane, 12-first catalytic layer, 13-second catalytic layer, 14-bracket, 2-flange, 3-sealed bottom cover. DETAILED DESCRIPTION

[0032] The present invention will be further explained below in conjunction with specific embodiments.

[0033] Example 1

[0034] The preparation method of the multifunctional catalytic and dust removal composite metal filter cartridge proposed by the present invention comprises the following steps:

[0035] S1: dispersing and mixing inorganic fibers, organic fibers, inorganic binders, organic binders, modifiers and water to prepare slurry;

[0036] S2: continuously injecting the prepared slurry into a cylindrical mold with holes on the inner surface, and subjecting the inside of the cylindrical mold to vacuum treatment until the water is drained, taking out the sample in the mold, drying and calcining it, and preparing a first catalytic layer substrate and a second catalytic layer substrate that can be nested with each other;

[0037] S3: impregnating the first catalyst slurry into the first catalyst layer substrate, and impregnating the second catalyst slurry into the second catalyst layer substrate, and obtaining the first catalyst layer and the second catalyst layer after drying and calcination;

[0038] S4: Insert the bracket into the second catalytic layer and the first catalytic layer in turn, and then arrange a porous metal membrane on the outside of the first catalytic layer to form a filter cartridge body. Connect and assemble several filter cartridge bodies, and install flanges and sealing bottom covers at both ends to obtain a multifunctional catalytic and dust removal composite metal filter cartridge. The porous metal membrane can be made of metal fiber sintered felt or metal powder sintered felt, and the filtration accuracy can be adjusted according to actual needs.

[0039] The modifier is composed of potato starch, seaweed polysaccharide and chitosan in a mass ratio of 1:1:1.

[0040] The slurry in S1 contains the following raw materials in parts by weight: 15 parts of inorganic fibers, 5 parts of organic fibers, 6 parts of inorganic binders, 3 parts of organic binders, 1 part of modifiers and 100 parts of water.

[0041] The inorganic fiber is aluminum silicate fiber; the organic fiber is polyvinyl alcohol fiber; the inorganic binder is sodium silicate; and the organic binder is sodium carboxymethyl cellulose.

[0042] The first catalyst slurry comprises the following raw materials in parts by weight: 85 parts of vanadium-titanium denitrification catalytic powder, 8 parts of nano-silicon dioxide, 3 parts of additives, and the balance is water; the second catalyst slurry comprises the following raw materials in parts by weight: 80 parts of precious metal decarbon monoxide catalytic powder, 8 parts of nano-silicon dioxide, 3 parts of additives, and the balance is water; the solid content of the first catalyst slurry and the second catalyst slurry is 15%.

[0043] The vanadium-titanium denitrification catalytic powder is composed of titanium dioxide and vanadium pentoxide in a mass ratio of 5:2; the precious metal decarbon monoxide catalytic powder is composed of aluminum oxide, platinum oxide and palladium oxide in a mass ratio of 100:1:1.

[0044] The auxiliary agent is polyvinyl pyrrolidone.

[0045] The first catalyst slurry and the second catalyst slurry were processed by a planetary ball mill to a particle size of about 600 nm, the rotation speed was 300 rpm, the ball milling medium was 0.7 mm zirconia beads, the material-to-ball ratio was 1:15, and the grinding time was 15 h.

[0046] The calcination temperature in S2 is 380°C, the heating rate is 3°C / min, and the calcination time is 6h; the calcination temperature in S3 is 450°C, the heating rate is 8°C / min, and the calcination time is 6h.

[0047] Example 2

[0048] The preparation method of the multifunctional catalytic and dust removal composite metal filter cartridge proposed by the present invention comprises the following steps:

[0049] S1: dispersing and mixing inorganic fibers, organic fibers, inorganic binders, organic binders, modifiers and water to prepare slurry;

[0050] S2: continuously injecting the prepared slurry into a cylindrical mold with holes on the inner surface, and subjecting the inside of the cylindrical mold to vacuum treatment until the water is drained, taking out the sample in the mold, drying and calcining it, and preparing a first catalytic layer substrate and a second catalytic layer substrate that can be nested with each other;

[0051] S3: impregnating the first catalyst slurry into the first catalyst layer substrate, and impregnating the second catalyst slurry into the second catalyst layer substrate, and obtaining the first catalyst layer and the second catalyst layer after drying and calcination;

[0052] S4: insert the bracket into the second catalytic layer and the first catalytic layer in sequence, and then arrange a porous metal membrane on the outside of the first catalytic layer to form a filter cartridge body, connect and assemble several filter cartridge bodies, and install flanges and sealing bottom covers at both ends respectively, so as to obtain a multifunctional catalytic and dust removal composite metal filter cartridge;

[0053] The modifier is composed of potato starch, seaweed polysaccharide and chitosan in a mass ratio of 2:1:1.

[0054] The slurry in S1 contains the following raw materials in parts by weight: 10 parts of inorganic fiber, 2 parts of organic fiber, 4 parts of inorganic binder, 1 part of organic binder, 0.5 parts of modifier and 100 parts of water.

[0055] The inorganic fibers are alumina fibers and glass fibers; the organic fibers are plant fibers, nylon fibers and polypropylene fibers; the inorganic binder is silica sol; and the organic binder is epoxy resin.

[0056] The first catalyst slurry comprises the following raw materials in parts by weight: 80 parts of vanadium-titanium denitrification catalytic powder, 5 parts of nano-silicon dioxide, 1 part of auxiliary agent, and the balance is water; the second catalyst slurry comprises the following raw materials in parts by weight: 70 parts of precious metal decarbon monoxide catalytic powder, 5 parts of nano-silicon dioxide, 1 part of auxiliary agent, and the balance is water; the solid content of the first catalyst slurry and the second catalyst slurry is 5%.

[0057] The vanadium-titanium denitrification catalytic powder is composed of titanium dioxide and vanadium pentoxide in a mass ratio of 5:1; the precious metal decarbon monoxide catalytic powder is composed of aluminum oxide, platinum oxide and palladium oxide in a mass ratio of 100:0.1:0.1.

[0058] The auxiliary agent is ethylene glycol.

[0059] The first catalyst slurry and the second catalyst slurry were processed by a planetary ball mill to a particle size of about 600 nm, the rotation speed was 200 rpm, the ball milling medium was 0.6 mm zirconia beads, the material-to-ball ratio was 1:10, and the grinding time was 10 h.

[0060] The calcination temperature in S2 is 300°C, the heating rate is 2°C / min, and the calcination time is 4h; the calcination temperature in S3 is 400°C, the heating rate is 5°C / min, and the calcination time is 4h.

[0061] Example 3

[0062] The preparation method of the multifunctional catalytic and dust removal composite metal filter cartridge proposed by the present invention comprises the following steps:

[0063] S1: dispersing and mixing inorganic fibers, organic fibers, inorganic binders, organic binders, modifiers and water to prepare slurry;

[0064] S2: continuously injecting the prepared slurry into a cylindrical mold with holes on the inner surface, and subjecting the inside of the cylindrical mold to vacuum treatment until the water is drained, taking out the sample in the mold, drying and calcining it, and preparing a first catalytic layer substrate and a second catalytic layer substrate that can be nested with each other;

[0065] S3: impregnating the first catalyst slurry into the first catalyst layer substrate, and impregnating the second catalyst slurry into the second catalyst layer substrate, and obtaining the first catalyst layer and the second catalyst layer after drying and calcination;

[0066] S4: insert the bracket into the second catalytic layer and the first catalytic layer in sequence, and then arrange a porous metal membrane on the outside of the first catalytic layer to form a filter cartridge body, connect and assemble several filter cartridge bodies, and install flanges and sealing bottom covers at both ends respectively, so as to obtain a multifunctional catalytic and dust removal composite metal filter cartridge;

[0067] The modifier is composed of potato starch, seaweed polysaccharide and chitosan in a mass ratio of 1:2:2.

[0068] The slurry in S1 contains the following raw materials in parts by weight: 20 parts of inorganic fiber, 8 parts of organic fiber, 8 parts of inorganic binder, 5 parts of organic binder, 1.5 parts of modifier and 100 parts of water.

[0069] The inorganic fibers are glass fibers and zirconia fibers; the organic fibers are polyester fibers; the inorganic binder is aluminum sol; and the organic binder is silicone.

[0070] The first catalyst slurry comprises the following raw materials in parts by weight: 90 parts of vanadium-titanium denitrification catalytic powder, 10 parts of nano-silicon dioxide, 5 parts of additives, and the balance is water; the second catalyst slurry comprises the following raw materials in parts by weight: 90 parts of precious metal decarbon monoxide catalytic powder, 10 parts of nano-silicon dioxide, 5 parts of additives, and the balance is water; the solid content of the first catalyst slurry and the second catalyst slurry is 25%.

[0071] The vanadium-titanium denitrification catalytic powder is composed of titanium dioxide and vanadium pentoxide in a mass ratio of 5:3; the precious metal decarbon monoxide catalytic powder is composed of aluminum oxide, platinum oxide and palladium oxide in a mass ratio of 100:3:3.

[0072] The auxiliary agent is sodium hexametaphosphate.

[0073] The first catalyst slurry and the second catalyst slurry were processed by a planetary ball mill to a particle size of about 600 nm, the rotation speed was 400 rpm, the ball milling medium was 0.8 mm zirconia beads, the material-to-ball ratio was 1:20, and the grinding time was 20 h.

[0074] The calcination temperature in S2 is 450°C, the heating rate is 5°C / min, and the calcination time is 8h; the calcination temperature in S3 is 500°C, the heating rate is 10°C / min, and the calcination time is 8h.

[0075] Comparative Example 1

[0076] The modifier of this scheme is composed of potato starch and seaweed polysaccharide in a mass ratio of 1:1, and the other conditions are the same as those in Example 1.

[0077] Comparative Example 2

[0078] The modifier of this scheme is composed of potato starch and chitosan in a mass ratio of 1:1, and the other conditions are the same as those in Example 1.

[0079] Comparative Example 3

[0080] The modifier of this scheme is composed of seaweed polysaccharide and chitosan in a mass ratio of 1:1, and the other conditions are the same as those in Example 1.

[0081] in:

[0082] The test method for denitration and deCO efficiency is as follows: punch holes in the denitration and deCO catalyst layers to take samples with a diameter of 30 mm for testing, insert the deCO catalyst layer and the denitration catalyst layer in turn, and control the gas concentration (vol%) by mass flow meter: NO: 500ppm, NH 3 : 500ppm, CO: 5000ppm, O 2 : 5%, H 2 O: 10%, N 2 The air is balanced, the filtration speed is 1m / min, and the test temperature is 200℃. The calculation formula for denitrification rate is η 1 =(C 1 -C 2 ) / C 1 × 100%, where C 1 Yes NO X The inlet concentration, C 2 Yes NO X The concentration at the outlet is measured by a flue gas analyzer. The formula for calculating the CO removal rate is η 2 =(D 1 -D 2 ) / D 1 × 100%, where D 1 is the inlet concentration of CO, D 2 It is the concentration of CO at the outlet, which is obtained by testing with a flue gas analyzer.

[0083] Resistance test method: Connect a differential pressure transmitter to the air inlet and outlet of the reactor of the efficiency evaluation device, detect the differential pressure of the catalytic layer while testing the efficiency, and compare the resistance of each sample.

[0084] Catalyst shedding rate test method: Take a sample of catalyst substrate for coating and calcination, and record the catalyst loading m 3 , dry the catalyst layer sample at 120±10℃ and record the mass m 1 , put the sample into the mold and blow it with compressed air, the blowing pressure is 0.3Mpa, the blowing times are 10000 times, and the mass m is recorded after the treated sample is completely dried 2 The formula for calculating the shedding rate is X = (m 1 -m 2 ) / m 3 ×100%.

[0085] The test results are shown in Table 1 and Table 2:

[0086] Table 1 Test results of denitrification and deCO efficiency

[0087] Group Denitrification rate (%) CO conversion rate (%) Example 1 99.8 100.0 Example 2 95.2 98.1 Example 3 97.3 99.8 Comparative Example 1 89.5 93.2 Comparative Example 2 84.3 94.5 Comparative Example 3 88.2 92.3

[0088] Table 2 Test results of resistance and shedding rate

[0089] Group Pressure difference (kPa) Dropout rate (%) Example 1 198 0.81 Example 2 201 0.95 Example 3 210 0.85 Comparative Example 1 244 1.82 Comparative Example 2 266 2.15 Comparative Example 3 230 1.63

[0090] It can be seen from the test results of Examples 1-3 in Table 1 that the present invention uses fiber products as the substrate of the catalyst layer, and the pores formed on the surface of the inorganic fiber and between the fibers can provide more catalytic powder loading sites, which is convenient for catalytic powder loading. By adjusting the solid content of the active liquid, the catalytic powder loading amount can be easily controlled, and it is not easy to fall off; and the present invention can further improve the specific surface area of ​​the catalyst layer substrate and the stability of the pore structure by adding a modifier, thereby improving the catalytic effect of the catalyst layer. In addition, it can be seen from the test results of Example 1 and Comparative Examples 1-3 that the modifiers of the present invention are potato starch, seaweed polysaccharide and chitosan, which can make the slurry have a larger specific surface area when calcined to form a catalyst layer substrate, thereby absorbing more catalysts and improving the catalytic effect of the filter cartridge, and potato starch, seaweed polysaccharide and chitosan have a synergistic effect in improving the catalytic effect of the filter cartridge, improving the specific surface area, oxygen vacancy concentration and chemical bond properties of the substrate, forming a stable three-dimensional pore structure, thereby ensuring the high stability and high catalytic performance of the catalyst layer. At the same time, it can be seen from the test results in Table 2 that the catalyst shedding rate on the catalyst substrate of the embodiment of the present invention is significantly lower than the catalyst shedding rate on the catalyst substrate of the comparative example, which further proves that the three-dimensional pore structure formed by the modifier of the present invention can significantly improve the stability of the catalytic layer, thereby reflecting excellent catalytic performance during use.

[0091] In addition, the catalyst layer of the present invention can be provided with multiple layers, and different catalytic slurries can be used for impregnation to achieve the removal of different components in the gas; the denitration catalytic slurry and the decarbonation catalytic slurry are also not limited to the description in the embodiments of the present invention.

Claims

1. A method for preparing a multifunctional catalytic and dust removal composite metal filter cartridge, characterized in that: The steps are as follows: S1: dispersing and mixing inorganic fibers, organic fibers, inorganic binders, organic binders, modifiers and water to prepare slurry; S2: forming the slurry in a mold, and calcining it to form a plurality of catalyst layer substrates that can be nested with each other; S3: impregnating a plurality of catalyst layer substrates with catalyst slurry, and obtaining a catalyst layer after drying and calcination; S4: inserting the support (14) into a plurality of catalytic layers in sequence, and then arranging a porous metal membrane (11) on the outer side of the outermost catalytic layer to form a filter cartridge body (1), connecting and assembling a plurality of filter cartridge bodies (1), and installing flanges (2) and sealing bottom covers (3) at both ends, respectively, to obtain a multifunctional catalytic and dust removal composite metal filter cartridge; The catalytic layer comprises a first catalytic layer (12) and a second catalytic layer (13), the first catalytic layer (12) being impregnated with a denitration catalytic slurry, and the second catalytic layer (13) being impregnated with a decarbon monoxide catalytic slurry; The denitration catalytic slurry comprises the following raw materials in parts by weight: 80-90 parts of denitration catalytic powder, 5-10 parts of nano-silicon dioxide, 1-5 parts of an auxiliary agent, and the balance is water; The carbon monoxide removal catalytic slurry comprises the following raw materials in parts by weight: 70-90 parts of carbon monoxide removal catalytic powder, 5-10 parts of nano silicon dioxide, 1-5 parts of an auxiliary agent, and the balance is water; The solid content of the denitration catalytic slurry and the decarbonation catalytic slurry is 5-25%; The denitration catalytic powder is composed of titanium dioxide and vanadium pentoxide in a mass ratio of 10:2-6; the decarbon monoxide catalytic powder is composed of aluminum oxide, platinum oxide and palladium oxide in a mass ratio of 100:0.1-3:0.1-3; The modifier is composed of potato starch, seaweed polysaccharide and chitosan in a mass ratio of 2:1-4:1-4.

2. The method for preparing the multifunctional catalytic and dust removal composite metal filter cartridge according to claim 1, characterized in that: The slurry in S1 contains the following raw materials in parts by weight: 10-20 parts of inorganic fibers, 2-8 parts of organic fibers, 4-8 parts of inorganic binders, 1-5 parts of organic binders, 0.5-1.5 parts of modifiers and 100 parts of water.

3. The method for preparing the multifunctional catalytic and dust removal composite metal filter cartridge according to claim 1, characterized in that: The inorganic fiber is one or more of aluminum silicate fiber, aluminum oxide fiber, glass fiber, and zirconium oxide fiber; the organic fiber is one or more of plant fiber, polyvinyl alcohol fiber, nylon fiber, polypropylene fiber, and polyester fiber; the inorganic binder is one or more of sodium silicate, silica sol, and aluminum sol; the organic binder is one or more of epoxy resin, silicone, and sodium carboxymethyl cellulose.

4. The method for preparing the multifunctional catalytic and dust removal composite metal filter cartridge according to claim 1, characterized in that: The auxiliary agent is one or more of ethylene glycol, polyvinyl pyrrolidone, polyoxyethylene alkyl ether, aluminum sol and sodium hexametaphosphate.

5. The method for preparing the multifunctional catalytic and dust removal composite metal filter cartridge according to claim 1, characterized in that: The catalyst slurry is processed by a ball mill with a rotation speed of 200-400 rpm, a ball milling medium of 0.6-0.8 mm zirconium oxide beads, a material-ball ratio of 1:10-20, and a grinding time of 10-20 hours.

6. The method for preparing the multifunctional catalytic and dust removal composite metal filter cartridge according to claim 1, characterized in that: The calcination temperature in S2 is 300-450°C, the heating rate is 2-5°C / min, and the calcination time is 4-8h.

7. The method for preparing the multifunctional catalytic and dust removal composite metal filter cartridge according to claim 1, characterized in that: The calcination temperature in S3 is 400-500°C, the heating rate is 5-10°C / min, and the calcination time is 4-8h.

8. A multifunctional catalytic and dust-removing composite metal filter cartridge prepared by the method according to any one of claims 1 to 7.