A method for preparing light-converting agricultural film
By preparing acyl chloride-treated hydrotalcite and mixing it with light-converting masterbatch for granulation, a five-layer light-converting agricultural film was prepared. This solved the problems of low fluorescence intensity, poor mechanical properties, and poor durability of the light-converting film, enabling its efficient use in humid, high-temperature, and high-light environments, and improving the film's heat preservation performance and transparency.
Patent Information
- Application Number
- CN202411250207.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-06
AI Technical Summary
Existing light-converting films suffer from low fluorescence intensity, decreased mechanical properties, poor durability, and short lifespan in humid environments. In particular, the poor compatibility between inorganic light-converting agents and plastics leads to low fluorescence intensity and short lifespan of the films.
A heat-insulating and light-converting masterbatch was prepared by mixing and granulating acyl chloride-treated hydrotalcite with light-converting masterbatch. A five-layer light-converting agricultural film was then used, consisting of an outer layer, a second outer layer, a middle layer, a second inner layer, and an inner layer. Organic and inorganic light-converting agents were compounded, and polyamide wax was added to improve the film's heat-insulating and mechanical properties.
It improves the fluorescence intensity and lifespan of the light conversion film, especially in humid and high-temperature and high-light environments, maintaining high fluorescence intensity and excellent heat preservation performance, while also improving the film's transparency and UV blocking rate.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a light-converting agricultural film, and belongs to the field of polymer compound compositions. Background Art
[0002] With the increase of world population, food supply has become tense. With the extensive use of pesticides and fertilizers, the potential for increasing food production is becoming increasingly limited, and the environment has also been greatly polluted. Therefore, it is very necessary to seek other ways to increase production with less pollution and better results. Using agricultural light-conversion film to improve plant photosynthesis is an environmentally friendly and effective way. Light-conversion film can increase the light conversion function by adding light-conversion agents to polyethylene, polyvinyl chloride and other greenhouse films that have the functions of heat preservation, cold protection, wind and rain protection, so as to improve the light quality of the greenhouse film, absorb the purple and green light in the sunlight that is not needed for plant photosynthesis, emit blue or red light, strengthen plant photosynthesis, promote crop growth and development, promote greenhouse crops photosynthesis, and have a positive impact on plant growth and development, nutrient absorption, chlorophyll content, agricultural product quality and other aspects, so as to improve crop quality and achieve the effect of increasing production.
[0003] The light stability of different light conversion agents against sunlight exposure is directly related to its actual application value and affects the promotion and application of light conversion films. At present, the main light conversion agents are divided into organic light conversion agents and inorganic light conversion agents. Among them, organic fluorescent dyes are used as light conversion agents for agricultural films. They have good compatibility with resins and are easier to make films, but they are prone to oxidation and decomposition, have a short service life, have low absorption and conversion efficiency of sunlight, and will also affect the light transmission characteristics of agricultural films. The price and cost are higher than inorganic light conversion agents.
[0004] Currently, the widely used type of inorganic light conversion agent is rare earth inorganic light conversion agent. The system of rare earth inorganic light conversion agent is relatively simple, mainly based on metal sulfide system. Although this system has low cost, the compatibility of rare earth inorganic light conversion agent with plastic is usually poor, resulting in low fluorescence intensity of the light conversion film and a significant decrease in the mechanical properties of the film. This is a common problem in the compatibility between inorganic systems and polymers.
[0005] In order to improve the performance of the light-converting film, inorganic and organic light-converting agents can be selected at the same time and mixed for use. This can not only improve the light-converting film's filtering and absorption effect on light at different wavelengths, making the transmission wavelength more reasonable, but also reduce the effect of a single inorganic light-converting agent on the film's strength. In addition, in order to make the light-converting film have a certain thermal insulation performance, a certain amount of hydrotalcite needs to be added to block infrared rays and achieve the effect of thermal insulation. Hydrotalcite can also improve the durability of the light-converting film to a certain extent, and the light-converting performance decays more slowly. However, due to the hygroscopicity of hydrotalcite, when it is used in combination with the easily deliquescent metal sulfide system inorganic light-converting agent, the life of the light-converting film in a humid environment will be greatly reduced. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the defects of the prior art. The invention prepares acyl chloride treated hydrotalcite, mixes and granulates the prepared acyl chloride treated hydrotalcite with light conversion masterbatch by a special method, obtains thermal insulation light conversion masterbatch, and finally prepares light conversion agricultural film, so that the agricultural film has better thermal insulation performance and mechanical properties, and at the same time solves the problem that the light conversion performance life of the light conversion film in a humid environment is reduced due to the addition of hydrotalcite.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] A method for preparing a light-converting agricultural film comprises preparing acyl chloride-treated hydrotalcite, blending to prepare heat-insulating light-converting masterbatch, and blow molding to prepare a light-converting film.
[0009] The following are further improvements to the above technical solution:
[0010] The method for preparing acyl chloride treated hydrotalcite comprises: crushing the hydrotalcite until all of it passes through a 400-600 mesh sieve, then mixing it with isopropyl acetate, stirring to make it uniformly dispersed, then adding 4-toluenesulfonyl chloride, controlling the temperature to 83-87° C., controlling the stirring speed to 75-120 r / min, stirring for 4-8 min, adding diethylenetriamine and imidazole, and after the addition is completed, raising the temperature to 92-95° C., keeping the stirring speed unchanged, continuing to stir for 42-52 min, filtering after the stirring is completed, and drying the filtered hydrotalcite in an oven at 120° C. for 8 h, and after the drying is completed, dispersing the hydrotalcite until all of it passes through a 400-600 mesh sieve to obtain acyl chloride treated hydrotalcite;
[0011] The hydrotalcite is magnesium aluminum hydrotalcite with a density of 2.0 g / cm 3 ;
[0012] The mass ratio of the hydrotalcite, isopropyl acetate, 4-toluenesulfonyl chloride, diethylenetriamine and imidazole is 500-600:2300-2800:130-170:8-12:0.9-1.1.
[0013] The method for preparing the thermal insulation light conversion masterbatch by blending is as follows: adding an organic light conversion agent, an inorganic light conversion agent, acyl chloride treated hydrotalcite and polyamide wax into a high-speed mixer for mixing; after the mixing is completed, the temperature is controlled to be 135-147° C., the speed is controlled to be 600-900 r / min, stirring is performed, and the stirring time is 14-25 min; then, linear low-density polyethylene, an antioxidant and a light stabilizer are added, the temperature is controlled to be 153-161° C., mixing is performed, and the mixing time is 45-60 min; after the mixing is completed, extrusion granulation is performed to obtain the thermal insulation light conversion masterbatch;
[0014] The mass ratio of the organic light conversion agent, the inorganic light conversion agent, the acyl chloride treated hydrotalcite, the polyamide wax, the linear low density polyethylene, the antioxidant and the light stabilizer is 4.5-5.5:6.5-7.5:8-12:1.8-2.2:70-90:4.5-5.5:5.5-6.5;
[0015] The model of the organic light conversion agent is Ruiers R12;
[0016] The model of the inorganic light conversion agent is Xiweier GTR650-II;
[0017] The density of the linear low-density polyethylene is 0.919 g / cm 3 ;
[0018] The model of the antioxidant is antioxidant 1076;
[0019] The light stabilizer is a hindered amine stabilizer, and its model is XT100.
[0020] The method for preparing the light-converting film by blow molding is as follows: respectively mixing the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material evenly, respectively adding them into five extruders corresponding to the outer layer, the sub-outer layer, the middle layer, the sub-inner layer and the inner layer, setting the extrusion working temperature of the screws of the outer layer and the inner layer to 178-182° C., the extrusion working temperature of the screws of the sub-outer layer and the sub-inner layer to 171-180° C., and the extrusion working temperature of the screws of the middle layer to 168-175° C., sequentially performing melting, mixing and plasticizing, and then squeezing the plasticized materials in the five extruders into the die head of the same five-layer co-extrusion film blowing machine for fusion, and extruding them in a tubular shape through the die, and then blowing, cooling and winding to obtain the light-converting agricultural film;
[0021] The structure of the light-converting agricultural film is an outer layer, a sub-outer layer, a middle layer, a sub-inner layer, and an inner layer from top to bottom. The thickness of the outer layer is 0.002mm, the thickness of the sub-outer layer is 0.001mm, the thickness of the middle layer is 0.002mm, the thickness of the sub-inner layer is 0.001mm, the thickness of the inner layer is 0.002mm, and the total thickness of the light-converting agricultural film is 0.008mm.
[0022] The outer layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 45-55 parts of linear low-density polyethylene, 13-17 parts of metallocene polyethylene, 0.6-1.0 parts of antioxidant, 0.6-1.0 parts of light stabilizer, and 0.4-0.6 parts of antioxidant;
[0023] The secondary outer layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 43-47 parts of linear low-density polyethylene, 12-14 parts of metallocene polyethylene, 4.5-5.5 parts of thermal insulation and light-conversion masterbatch, and 0.4-0.6 parts of antioxidant;
[0024] The middle layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 50-60 parts of linear low-density polyethylene, 16-20 parts of metallocene polyethylene, 6.5-7.5 parts of thermal insulation and light-conversion masterbatch, and 0.4-0.6 parts of antioxidant;
[0025] The secondary inner layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 43-47 parts of linear low-density polyethylene, 12-14 parts of metallocene polyethylene, 4.5-5.5 parts of thermal insulation and light-conversion masterbatch, and 0.4-0.6 parts of antioxidant;
[0026] The inner layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 45-55 parts of linear low-density polyethylene, 13-17 parts of metallocene polyethylene, 0.6-1.0 parts of antioxidant, 0.6-1.0 parts of light stabilizer, and 0.4-0.6 parts of antioxidant;
[0027] The density of the low-density polyethylene in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material is 0.917 g / cm 3 The density of linear low-density polyethylene is 0.919 g / cm 3 The density of metallocene polyethylene is 0.925 g / cm 3 ;
[0028] The antioxidants in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material are all antioxidant 124; the light stabilizer hindered amine stabilizer in the outer layer material and the inner layer material is model XT100; the antioxidant in the outer layer material and the inner layer material is antioxidant 1076.
[0029] Compared with the prior art, the present invention achieves the following beneficial effects:
[0030] The light-converting film prepared by the present invention has excellent tensile properties. According to the method in GB / T1040.1-2006, the transverse tensile strength, longitudinal tensile strength, transverse elongation at break, and longitudinal elongation at break of the film are tested. The transverse tensile strength is 43.47-43.66MPa, the longitudinal tensile strength is 41.17-42.04MPa, the transverse elongation at break is 817.9-836.0%, and the longitudinal elongation at break is 747.8-762.5%;
[0031] The light-converting film prepared by the present invention has excellent light-converting performance and high red fluorescence emission intensity. The intensity of red fluorescence converted after absorbing purple light is measured by a fluorescence spectrometer, and the intensity is 8267-8341a.u.;
[0032] The light-converting film prepared by the present invention has a relatively high service life when placed in a long-term humid environment, and the fluorescence intensity can be maintained at a relatively high level. The relative humidity of the environment on the outer layer side is set to 70%, the relative humidity of the environment on the inner layer side is 70%, and the placement time is 90 days. The red fluorescence emission intensity of the light-converting film is 8143-8178 a.u.; the relative humidity of the environment on the outer layer side is set to 70%, the relative humidity of the environment on the inner layer side is 80%, and the placement time is 90 days. The red fluorescence emission intensity of the light-converting film is 8071-8102 a.u.; the relative humidity of the environment on the outer layer side is set to 80%, the relative humidity of the environment on the inner layer side is 80%, and the placement time is 90 days. The red fluorescence emission intensity of the light-converting film is 7965-8015 a.u.;
[0033] The light-converting film prepared by the present invention has a relatively high service life in a long-term high-temperature and strong-light environment, and the fluorescence intensity can be maintained at a relatively high level. When the outer layer of the agricultural film is irradiated with simulated sunlight of an intensity of 80,000 LUX, the temperature of the environment during irradiation is controlled to be 40° C., and the irradiation time is controlled to be 90 days, the red fluorescence emission intensity of the light-converting film is 8006-8088 a.u.; when the outer layer of the agricultural film is irradiated with simulated sunlight of an intensity of 100,000 LUX, the temperature of the environment during irradiation is controlled to be 45° C., and the irradiation time is controlled to be 90 days, the red fluorescence emission intensity of the light-converting film is 7903-7968 a.u.; when the outer layer of the agricultural film is irradiated with simulated sunlight of an intensity of 150,000 LUX, the temperature of the environment during irradiation is controlled to be 50° C., and the irradiation time is controlled to be 90 days, the red fluorescence emission intensity of the light-converting film is 7847-7892 a.u.;
[0034] The light-converting film prepared by the present invention has excellent heat preservation performance. The inner layer side and the outer layer side of the light-converting film are completely isolated, and the outer layer side of the agricultural film is irradiated with simulated sunlight with an intensity of 100000LUX. The temperature of the environment during irradiation is controlled to be 45°C, and the irradiation time is controlled to be 8h. At 0h after the irradiation, the temperature of the inner layer side is 71.5-72.1°C; at 2h after the irradiation, the temperature of the inner layer side is 67.6-68.3°C; at 6h after the irradiation, the temperature of the inner layer side is 53.6-54.3°C; at 12h after the irradiation, the temperature of the inner layer side is 47.3-48.2°C.
[0035] The light-converting film prepared by the present invention has high transparency and low haze, and the ultraviolet blocking rate of the film is high. According to the method in GB / T2410-2008, the transmittance and haze of the light-converting film are tested, and the transmittance is 91.94-92.40%, the haze is 9.41-10.14%, and the ultraviolet blocking rate is 63.39-64.21%. DETAILED DESCRIPTION Example 1
[0036] (1) Preparation of acyl chloride treated hydrotalcite
[0037] The hydrotalcite was crushed until all of it passed through a 500-mesh sieve, and then mixed with isopropyl acetate and stirred to be evenly dispersed, and then 4-toluenesulfonyl chloride was added, the temperature was controlled to 85° C., the stirring speed was controlled to 90 r / min, and stirring was performed for 5 min. After the stirring was completed, diethylenetriamine and imidazole were added. After the addition was completed, the temperature was raised to 93° C., the stirring speed was kept unchanged, and stirring was continued for 45 min. After the stirring was completed, it was filtered, and the filtered hydrotalcite was dried in an oven at 120° C. for 8 h. After the drying was completed, the hydrotalcite was dispersed until all of it passed through a 500-mesh sieve to obtain acyl chloride-treated hydrotalcite;
[0038] The hydrotalcite is magnesium aluminum hydrotalcite with a density of 2.0 g / cm 3 ;
[0039] The mass ratio of the hydrotalcite, isopropyl acetate, 4-toluenesulfonyl chloride, diethylenetriamine and imidazole is 550:2500:150:10:1.
[0040] (2) Blending to prepare thermal insulation and light-conversion masterbatch
[0041] Add organic light conversion agent, inorganic light conversion agent, acyl chloride treated hydrotalcite and polyamide wax into a high-speed mixer and mix them. After mixing, control the temperature to 142°C and the speed to 750r / min, stir for 17 minutes, then add linear low-density polyethylene, antioxidant and light stabilizer, control the temperature to 157°C, mix for 50 minutes, and extrude and granulate after mixing to obtain heat preservation light conversion masterbatch.
[0042] The mass ratio of the organic light conversion agent, the inorganic light conversion agent, the acyl chloride treated hydrotalcite, the polyamide wax, the linear low density polyethylene, the antioxidant and the light stabilizer is 5:7:10:2:80:5:6;
[0043] The model of the organic light conversion agent is Ruiers R12;
[0044] The model of the inorganic light conversion agent is Xiweier GTR650-II;
[0045] The density of the linear low-density polyethylene is 0.919 g / cm 3 ;
[0046] The model of the antioxidant is antioxidant 1076;
[0047] The light stabilizer is a hindered amine stabilizer, and its model is XT100.
[0048] (3) Blow molding to prepare light-converting film
[0049] The outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material are mixed evenly respectively, and added into five extruders corresponding to the outer layer, the sub-outer layer, the middle layer, the sub-inner layer and the inner layer respectively, and the extrusion working temperature of the screws of the outer layer and the inner layer is set to 180°C, the extrusion working temperature of the screws of the sub-outer layer and the sub-inner layer is set to 175°C, and the extrusion working temperature of the screws of the middle layer is set to 170°C, and the melting, mixing and plasticizing are carried out in sequence, and then the plasticized materials in the five extruders are squeezed into the die head of the same five-layer co-extrusion film blowing machine for fusion, and extruded in a tubular shape through the die, and then blown, cooled and rolled to obtain a light-converting agricultural film;
[0050] The structure of the light-converting agricultural film is an outer layer, a sub-outer layer, a middle layer, a sub-inner layer, and an inner layer from top to bottom. The thickness of the outer layer is 0.002mm, the thickness of the sub-outer layer is 0.001mm, the thickness of the middle layer is 0.002mm, the thickness of the sub-inner layer is 0.001mm, the thickness of the inner layer is 0.002mm, and the total thickness of the light-converting agricultural film is 0.008mm.
[0051] The outer layer material comprises the following components by weight: 25 parts of low-density polyethylene, 50 parts of linear low-density polyethylene, 15 parts of metallocene polyethylene, 0.8 parts of antioxidant, 0.8 parts of light stabilizer, and 0.5 parts of antioxidant;
[0052] The secondary outer layer material comprises the following components by weight: 25 parts of low-density polyethylene, 45 parts of linear low-density polyethylene, 13 parts of metallocene polyethylene, 5 parts of thermal insulation and light-conversion masterbatch, and 0.5 parts of antioxidant;
[0053] The middle layer material comprises the following components by weight: 25 parts of low-density polyethylene, 55 parts of linear low-density polyethylene, 18 parts of metallocene polyethylene, 7 parts of thermal insulation and light-conversion masterbatch, and 0.5 parts of antioxidant;
[0054] The secondary inner layer material comprises the following components by weight: 25 parts of low-density polyethylene, 45 parts of linear low-density polyethylene, 13 parts of metallocene polyethylene, 5 parts of thermal insulation and light-conversion masterbatch, and 0.5 parts of antioxidant;
[0055] The inner layer material comprises the following components by weight: 25 parts of low-density polyethylene, 50 parts of linear low-density polyethylene, 15 parts of metallocene polyethylene, 0.8 parts of antioxidant, 0.8 parts of light stabilizer, and 0.5 parts of antioxidant;
[0056] The density of the low-density polyethylene in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material is 0.917 g / cm 3 The density of linear low-density polyethylene is 0.919 g / cm 3 The density of metallocene polyethylene is 0.925 g / cm 3 ;
[0057] The antioxidants in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material are all antioxidant 124; the light stabilizer hindered amine stabilizer in the outer layer material and the inner layer material is model XT100; the antioxidant in the outer layer material and the inner layer material is antioxidant 1076. Example 2
[0058] (1) Preparation of acyl chloride treated hydrotalcite
[0059] The hydrotalcite was crushed until all of it passed through a 400-mesh sieve, and then mixed with isopropyl acetate and stirred to be evenly dispersed, and then 4-toluenesulfonyl chloride was added, the temperature was controlled to 83° C., the stirring speed was controlled to 120 r / min, and stirring was performed for 4 minutes. After the stirring was completed, diethylenetriamine and imidazole were added. After the addition was completed, the temperature was raised to 92° C., the stirring speed was kept unchanged, and stirring was continued for 52 minutes. After the stirring was completed, it was filtered, and the filtered hydrotalcite was dried in an oven at 120° C. for 8 hours. After the drying was completed, the hydrotalcite was dispersed until all of it passed through a 400-mesh sieve to obtain acyl chloride-treated hydrotalcite;
[0060] The hydrotalcite is magnesium aluminum hydrotalcite with a density of 2.0 g / cm 3 ;
[0061] The mass ratio of the hydrotalcite, isopropyl acetate, 4-toluenesulfonyl chloride, diethylenetriamine and imidazole is 500:2300:130:8:0.9.
[0062] (2) Blending to prepare thermal insulation and light-conversion masterbatch
[0063] Add an organic light conversion agent, an inorganic light conversion agent, acyl chloride treated hydrotalcite and polyamide wax into a high-speed mixer and mix them. After mixing, control the temperature to 135°C and the speed to 600r / min, stir for 25 minutes, then add linear low-density polyethylene, an antioxidant and a light stabilizer, control the temperature to 153°C, mix for 60 minutes, and extrude and granulate after mixing to obtain heat-insulating light conversion masterbatch.
[0064] The mass ratio of the organic light conversion agent, the inorganic light conversion agent, the acyl chloride treated hydrotalcite, the polyamide wax, the linear low density polyethylene, the antioxidant and the light stabilizer is 4.5:6.5:8:1.8:70:4.5:5.5;
[0065] The model of the organic light conversion agent is Ruiers R12;
[0066] The model of the inorganic light conversion agent is Xiweier GTR650-II;
[0067] The density of the linear low-density polyethylene is 0.919 g / cm 3 ;
[0068] The model of the antioxidant is antioxidant 1076;
[0069] The light stabilizer is a hindered amine stabilizer, and its model is XT100.
[0070] (3) Blow molding to prepare light-converting film
[0071] The outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material are mixed evenly respectively, and added into five extruders corresponding to the outer layer, the sub-outer layer, the middle layer, the sub-inner layer and the inner layer respectively, and the extrusion working temperature of the screws of the outer layer and the inner layer is set to 182°C, the extrusion working temperature of the screws of the sub-outer layer and the sub-inner layer is set to 171°C, and the extrusion working temperature of the screws of the middle layer is set to 168°C, and the materials are melted, mixed and plasticized in sequence, and then the plasticized materials in the five extruders are squeezed into the die head of the same five-layer co-extrusion film blowing machine for fusion, and extruded in a tubular shape through the die, and then blown, cooled and rolled to obtain a light-converting agricultural film;
[0072] The structure of the light-converting agricultural film is an outer layer, a sub-outer layer, a middle layer, a sub-inner layer, and an inner layer from top to bottom. The thickness of the outer layer is 0.002mm, the thickness of the sub-outer layer is 0.001mm, the thickness of the middle layer is 0.002mm, the thickness of the sub-inner layer is 0.001mm, the thickness of the inner layer is 0.002mm, and the total thickness of the light-converting agricultural film is 0.008mm.
[0073] The outer layer material comprises the following components by weight: 22.5 parts of low-density polyethylene, 45 parts of linear low-density polyethylene, 13 parts of metallocene polyethylene, 0.6 parts of antioxidant, 0.6 parts of light stabilizer, and 0.4 parts of antioxidant;
[0074] The secondary outer layer material comprises the following components by weight: 22.5 parts of low-density polyethylene, 43 parts of linear low-density polyethylene, 12 parts of metallocene polyethylene, 4.5 parts of thermal insulation and light-conversion masterbatch, and 0.4 parts of antioxidant;
[0075] The middle layer material comprises the following components by weight: 22.5 parts of low-density polyethylene, 50 parts of linear low-density polyethylene, 16 parts of metallocene polyethylene, 6.5 parts of thermal insulation and light-conversion masterbatch, and 0.4 parts of antioxidant;
[0076] The secondary inner layer material comprises the following components by weight: 22.5 parts of low-density polyethylene, 43 parts of linear low-density polyethylene, 12 parts of metallocene polyethylene, 4.5 parts of thermal insulation and light-conversion masterbatch, and 0.4 parts of antioxidant;
[0077] The inner layer material comprises the following components by weight: 22.5 parts of low-density polyethylene, 45 parts of linear low-density polyethylene, 13 parts of metallocene polyethylene, 0.6 parts of antioxidant, 0.6 parts of light stabilizer, and 0.4 parts of antioxidant;
[0078] The density of the low-density polyethylene in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material is 0.917 g / cm 3 The density of linear low-density polyethylene is 0.919 g / cm 3 The density of metallocene polyethylene is 0.925 g / cm 3 ;
[0079] The antioxidants in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material are all antioxidant 124; the light stabilizer hindered amine stabilizer in the outer layer material and the inner layer material is model XT100; the antioxidant in the outer layer material and the inner layer material is antioxidant 1076. Example 3
[0080] (1) Preparation of acyl chloride treated hydrotalcite
[0081] The hydrotalcite was crushed until all of it passed through a 600-mesh sieve, and then mixed with isopropyl acetate and stirred to be evenly dispersed, and then 4-toluenesulfonyl chloride was added, the temperature was controlled to 87° C., the stirring speed was controlled to 75 r / min, and stirring was performed for 8 minutes. After the stirring was completed, diethylenetriamine and imidazole were added. After the addition was completed, the temperature was raised to 95° C., the stirring speed was kept unchanged, and stirring was continued for 42 minutes. After the stirring was completed, it was filtered, and the filtered hydrotalcite was dried in an oven at 120° C. for 8 hours. After the drying was completed, the hydrotalcite was dispersed until all of it passed through a 600-mesh sieve to obtain acyl chloride-treated hydrotalcite;
[0082] The hydrotalcite is magnesium aluminum hydrotalcite with a density of 2.0 g / cm 3 ;
[0083] The mass ratio of the hydrotalcite, isopropyl acetate, 4-toluenesulfonyl chloride, diethylenetriamine and imidazole is 600:2800:170:12:1.1.
[0084] (2) Blending to prepare thermal insulation and light-conversion masterbatch
[0085] Add an organic light conversion agent, an inorganic light conversion agent, acyl chloride treated hydrotalcite and polyamide wax into a high-speed mixer and mix them. After mixing, control the temperature to 147°C and the speed to 900r / min, stir for 14 minutes, then add linear low-density polyethylene, an antioxidant and a light stabilizer, control the temperature to 161°C, mix for 45 minutes, and extrude and granulate after mixing to obtain heat-insulating light conversion masterbatch.
[0086] The mass ratio of the organic light conversion agent, the inorganic light conversion agent, the acyl chloride treated hydrotalcite, the polyamide wax, the linear low density polyethylene, the antioxidant and the light stabilizer is 5.5:7.5:12:2.2:90:5.5:6.5;
[0087] The model of the organic light conversion agent is Ruiers R12;
[0088] The model of the inorganic light conversion agent is Xiweier GTR650-II;
[0089] The density of the linear low-density polyethylene is 0.919 g / cm 3 ;
[0090] The model of the antioxidant is antioxidant 1076;
[0091] The light stabilizer is a hindered amine stabilizer, and its model is XT100.
[0092] (3) Blow molding to prepare light-converting film
[0093] The outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material are mixed evenly respectively, and added into five extruders corresponding to the outer layer, the sub-outer layer, the middle layer, the sub-inner layer and the inner layer respectively, and the extrusion working temperature of the screws of the outer layer and the inner layer is set to 182°C, the extrusion working temperature of the screws of the sub-outer layer and the sub-inner layer is set to 180°C, and the extrusion working temperature of the screws of the middle layer is set to 175°C, and the materials are melted, mixed and plasticized in sequence, and then the plasticized materials in the five extruders are squeezed into the die head of the same five-layer co-extrusion film blowing machine for fusion, and extruded in a tubular shape through the die, and then blown, cooled and rolled to obtain a light-converting agricultural film;
[0094] The structure of the light-converting agricultural film is an outer layer, a sub-outer layer, a middle layer, a sub-inner layer, and an inner layer from top to bottom. The thickness of the outer layer is 0.002mm, the thickness of the sub-outer layer is 0.001mm, the thickness of the middle layer is 0.002mm, the thickness of the sub-inner layer is 0.001mm, the thickness of the inner layer is 0.002mm, and the total thickness of the light-converting agricultural film is 0.008mm.
[0095] The outer layer material comprises the following components by weight: 27.5 parts of low-density polyethylene, 55 parts of linear low-density polyethylene, 17 parts of metallocene polyethylene, 1.0 parts of antioxidant, 1.0 parts of light stabilizer, and 0.6 parts of antioxidant;
[0096] The secondary outer layer material comprises the following components by weight: 27.5 parts of low-density polyethylene, 47 parts of linear low-density polyethylene, 14 parts of metallocene polyethylene, 5.5 parts of thermal insulation and light-conversion masterbatch, and 0.6 parts of antioxidant;
[0097] The middle layer material comprises the following components by weight: 27.5 parts of low-density polyethylene, 60 parts of linear low-density polyethylene, 20 parts of metallocene polyethylene, 7.5 parts of thermal insulation and light-conversion masterbatch, and 0.6 parts of antioxidant;
[0098] The secondary inner layer material comprises the following components by weight: 27.5 parts of low-density polyethylene, 47 parts of linear low-density polyethylene, 14 parts of metallocene polyethylene, 5.5 parts of thermal insulation and light-conversion masterbatch, and 0.6 parts of antioxidant;
[0099] The inner layer material comprises the following components by weight: 27.5 parts of low-density polyethylene, 55 parts of linear low-density polyethylene, 17 parts of metallocene polyethylene, 1.0 parts of antioxidant, 1.0 parts of light stabilizer, and 0.6 parts of antioxidant;
[0100] The density of the low-density polyethylene in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material is 0.917 g / cm 3 The density of linear low-density polyethylene is 0.919 g / cm 3 The density of metallocene polyethylene is 0.925 g / cm 3 ;
[0101] The antioxidants in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material are all antioxidant 124; the light stabilizer hindered amine stabilizer in the outer layer material and the inner layer material is model XT100; the antioxidant in the outer layer material and the inner layer material is antioxidant 1076.
[0102] Comparative Example 1
[0103] Different from Example 1, the step of preparing acyl chloride treated hydrotalcite is omitted, and in the step of preparing thermal insulation light conversion masterbatch by blending, untreated 500 mesh magnesium aluminum hydrotalcite is used to prepare thermal insulation light conversion masterbatch, and the remaining steps are the same to prepare light conversion agricultural film.
[0104] Comparative Example 2
[0105] Different from Example 1, the step of preparing heat preservation and light conversion masterbatch by blending is changed to the following operation:
[0106] The organic light conversion agent, the inorganic light conversion agent, the acyl chloride treated hydrotalcite, the linear low density polyethylene, the antioxidant and the light stabilizer are mixed at a temperature of 157°C for 50 minutes. After the mixing is completed, the mixture is extruded and granulated to obtain the heat preservation light conversion masterbatch.
[0107] The mass ratio of the organic light conversion agent, the inorganic light conversion agent, the acyl chloride treated hydrotalcite, the linear low density polyethylene, the antioxidant and the light stabilizer is 5:7:10:80:5:6;
[0108] The model of the organic light conversion agent is Ruiers R12;
[0109] The model of the inorganic light conversion agent is Xiweier GTR650-II;
[0110] The density of the linear low-density polyethylene is 0.919 g / cm 3 ;
[0111] The model of the antioxidant is antioxidant 1076;
[0112] The light stabilizer is a hindered amine stabilizer, model XT100;
[0113] The remaining steps are the same to prepare the light-converting agricultural film.
[0114] Example 4 Film tensile properties test
[0115] The light-converting agricultural films prepared in Examples 1-3 and Comparative Examples 1-2 were tested for transverse tensile strength, longitudinal tensile strength, transverse elongation at break, and longitudinal elongation at break according to the method in GB / T1040.1-2006. The results are shown in Table 1.
[0116] Table 1
[0117]
[0118] In Example 1-3, acyl chloride-treated hydrotalcite is prepared, and then the prepared acyl chloride-treated hydrotalcite and light-converting masterbatch are mixed and granulated by a special method to obtain a heat-insulating light-converting masterbatch, and finally a light-converting agricultural film is prepared, which can improve the tensile properties of the film, whether it is tensile strength or elongation at break, both are higher;
[0119] Comparative Example 1 omitted the step of preparing the hydrotalcite treated with acyl chloride, and used untreated 500-mesh magnesium-aluminum hydrotalcite to prepare the thermal insulation light-conversion masterbatch in the step of preparing the thermal insulation light-conversion masterbatch by blending, resulting in a decrease in the tensile properties of the agricultural film, both the tensile strength and the elongation at break decreased to a certain extent;
[0120] Comparative Example 2 omits the steps of mixing the organic light conversion agent, the inorganic light conversion agent, and the acyl chloride-treated hydrotalcite with the polyamide wax, resulting in a decrease in the tensile properties of the agricultural film, both the tensile strength and the elongation at break being greatly decreased.
[0121] Example 5: Test of light conversion performance of films under different environments
[0122] The light conversion performance of the light-converting agricultural films of Examples 1-3 and Comparative Examples 1-2 was measured using a fluorescence spectrometer. The test parameters were as follows: slit 2.5 nm / 2.5 m, photomultiplier tube voltage 700 V, scanning rate 60 nm / min, violet light with a wavelength of 279 nm was used as the excitation light, and red light with a wavelength of 635 nm was used as the monitoring excitation light. The intensity of the red fluorescence converted after absorbing violet light was tested. The results are shown in Table 2.
[0123] Table 2
[0124]
[0125] The light-converting agricultural films prepared in Examples 1-3 and Comparative Examples 1-2 were placed in a humid environment for placement. After placement, the red fluorescence intensity was detected using a fluorescence spectrometer according to the same test parameters;
[0126] There are three placement conditions, and the test is carried out under the three conditions, as follows:
[0127] Set the relative humidity of the environment on the outer layer side to 70%, the relative humidity of the environment on the inner layer side to 70%, and place it for 90 days;
[0128] Set the relative humidity of the environment on the outer side to 70% and the relative humidity of the environment on the inner side to 80%, and place it for 90 days;
[0129] Set the relative humidity of the environment on the outer layer side to 80%, the relative humidity of the environment on the inner layer side to 80%, and place it for 90 days;
[0130] The results are shown in Table 3.
[0131] Table 3
[0132]
[0133] The light-converting agricultural films prepared in Examples 1-3 and Comparative Examples 1-2 were placed in a high-temperature irradiation environment, and after the placement, the red fluorescence intensity was detected using a fluorescence spectrometer according to the same test parameters;
[0134] There are three placement conditions, and the test is carried out under the three conditions, as follows:
[0135] Use simulated sunlight with an intensity of 80,000 LUX to irradiate one side of the outer layer of the agricultural film, control the ambient temperature during irradiation to be 40°C, and control the irradiation time to be 90 days;
[0136] Use simulated sunlight with an intensity of 100,000 LUX to irradiate one side of the outer layer of the agricultural film, control the ambient temperature during irradiation to be 45°C, and control the irradiation time to be 90 days;
[0137] Use simulated sunlight with an intensity of 150,000 LUX to irradiate one side of the outer layer of the agricultural film, control the ambient temperature during irradiation to be 50°C, and control the irradiation time to be 90 days;
[0138] The results are shown in Table 4.
[0139] Table 4
[0140]
[0141] In Example 1-3, acyl chloride-treated hydrotalcite is prepared, and then the prepared acyl chloride-treated hydrotalcite and light conversion masterbatch are mixed and granulated by a special method to obtain a heat-insulating light conversion masterbatch, and finally a light conversion agricultural film is prepared, which can improve the light conversion performance of the film. The agricultural film has a high initial red fluorescence emission intensity. When used in a humid environment for a long time, the red fluorescence emission intensity can be maintained at a high level. When used in a high temperature and high-intensity light environment for a long time, the red fluorescence emission intensity can be maintained at a high level, and the light conversion film has a long service life;
[0142] Comparative Example 1 omitted the step of preparing the hydrotalcite treated with acyl chloride, and used untreated 500-mesh magnesium-aluminum hydrotalcite in the step of preparing the thermal insulation light conversion masterbatch by blending, so as to prepare the thermal insulation light conversion masterbatch, resulting in a slightly low initial red fluorescence emission intensity of the agricultural film. When used in a humid environment for a long time, the red fluorescence emission intensity dropped seriously. When used in a high temperature and high-intensity light environment for a long time, the red fluorescence emission intensity dropped seriously, and the service life of the light conversion film was short.
[0143] Comparative Example 2 omits the steps of mixing the organic light conversion agent, the inorganic light conversion agent, and the acyl chloride-treated hydrotalcite with the polyamide wax, resulting in a slightly lower initial red fluorescence emission intensity of the agricultural film. When used in a humid environment for a long time, the red fluorescence emission intensity decreases to a certain extent. When used in a high temperature and high-intensity light environment for a long time, the red fluorescence emission intensity decreases to a certain extent, and the service life of the light conversion film is short.
[0144] Example 6 Film thermal insulation performance test
[0145] The light-converting films prepared in Examples 1-3 and Comparative Examples 1-2 were tested for thermal insulation performance, and the test method was as follows:
[0146] The inner side of the light-converting film was completely isolated from the outer side, and the outer side of the agricultural film was irradiated with simulated sunlight of an intensity of 100,000 LUX. The ambient temperature during irradiation was controlled to be 45°C, and the irradiation time was controlled to be 8 hours. After the irradiation was completed, the temperature of the inner side was tested at 0h, 2h, 6h, and 12h after the irradiation was completed. The results are shown in Table 5.
[0147] Table 5
[0148]
[0149] Example 1-3: Acid chloride treated hydrotalcite is prepared, and then the prepared acid chloride treated hydrotalcite and light conversion masterbatch are mixed and granulated by a special method to obtain heat preservation light conversion masterbatch, and finally light conversion agricultural film is prepared, which can improve the heat preservation performance of the film. After the simulated sunlight irradiation is stopped, the inner layer of the film can maintain a higher temperature;
[0150] Comparative Example 1 omitted the step of preparing the hydrotalcite treated with acyl chloride, and used untreated 500-mesh magnesium-aluminum hydrotalcite to prepare the thermal insulation light-conversion masterbatch in the step of preparing the thermal insulation light-conversion masterbatch by blending, resulting in a decrease in the thermal insulation performance of the agricultural film. After the simulated sunlight irradiation was stopped, the temperature of the inner layer of the film dropped rapidly, and the thermal insulation performance was poor.
[0151] Comparative Example 2 omitted the steps of mixing the organic light conversion agent, the inorganic light conversion agent, and the acyl chloride-treated hydrotalcite with the polyamide wax, resulting in a decrease in the thermal insulation performance of the agricultural film. After the simulated sunlight exposure was stopped, the temperature of the inner layer of the film dropped rapidly, and the thermal insulation performance was poor.
[0152] Example 7 Film transmittance and UV blocking rate test
[0153] The light-conversion films prepared in Examples 1-3 and Comparative Examples 1-2 were tested for light transmittance and haze according to the method in GB / T2410-2008;
[0154] At the same time, a transmission photometer is used to detect the UV blocking rate of the light conversion film at a wavelength of 300nm;
[0155] The results are shown in Table 6.
[0156] Table 6
[0157]
[0158] In Example 1-3, acyl chloride-treated hydrotalcite is prepared, and then the prepared acyl chloride-treated hydrotalcite and light-converting masterbatch are mixed and granulated by a special method to obtain a heat-insulating light-converting masterbatch, and finally a light-converting agricultural film is prepared. The film has high transparency, low haze, and high ultraviolet blocking rate;
[0159] Comparative Example 1 omitted the step of preparing the hydrotalcite treated with acyl chloride, and used untreated 500-mesh magnesium-aluminum hydrotalcite in the step of preparing the thermal insulation light-conversion masterbatch by blending, to prepare the thermal insulation light-conversion masterbatch, resulting in a certain degree of decrease in the light transmittance of the agricultural film, a certain degree of increase in the haze, and a serious decrease in the ultraviolet blocking rate;
[0160] Comparative Example 2 omits the steps of mixing the organic light conversion agent, the inorganic light conversion agent, and the acyl chloride-treated hydrotalcite with the polyamide wax, resulting in a significant decrease in the light transmittance of the agricultural film, a significant increase in the haze, and a certain decrease in the UV blocking rate.
Claims
1. A method for preparing a light-converting agricultural film, characterized in that: The preparation method comprises preparing acyl chloride treated hydrotalcite, blending to prepare heat-insulating light-converting masterbatch, and blow molding to prepare light-converting film; The method for preparing acyl chloride treated hydrotalcite comprises: crushing the hydrotalcite until all of it passes through a 400-600 mesh sieve, then mixing it with isopropyl acetate, stirring to make it uniformly dispersed, then adding 4-toluenesulfonyl chloride, controlling the temperature to 83-87° C., controlling the stirring speed to 75-120 r / min, stirring for 4-8 min, adding diethylenetriamine and imidazole, and after the addition is completed, raising the temperature to 92-95° C., keeping the stirring speed unchanged, continuing to stir for 42-52 min, filtering after the stirring is completed, drying the filtered hydrotalcite, and after the drying is completed, dispersing the hydrotalcite until all of it passes through a 400-600 mesh sieve to obtain acyl chloride treated hydrotalcite; The mass ratio of the hydrotalcite, isopropyl acetate, 4-toluenesulfonyl chloride, diethylenetriamine and imidazole is 500-600:2300-2800:130-170:8-12:0.9-1.1; The method for preparing the thermal insulation light conversion masterbatch by blending is as follows: an organic light conversion agent, an inorganic light conversion agent, acyl chloride treated hydrotalcite and polyamide wax are mixed at a high speed, after the mixing is completed, the temperature is controlled to be 135-147° C., the speed is controlled to be 600-900 r / min, stirring is performed, and the stirring time is 14-25 min, and then linear low-density polyethylene, an antioxidant and a light stabilizer are added, and mixing is performed. After the mixing is completed, extrusion granulation is performed to obtain the thermal insulation light conversion masterbatch; The mass ratio of the organic light conversion agent, the inorganic light conversion agent, the acyl chloride treated hydrotalcite, the polyamide wax, the linear low density polyethylene, the antioxidant and the light stabilizer is 4.5-5.5:6.5-7.5:8-12:1.8-2.2:70-90:4.5-5.5:5.5-6.5; The method for preparing the light-converting film by blow molding is as follows: respectively mixing the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material and the inner layer material, respectively adding them into five extruders corresponding to the outer layer, the sub-outer layer, the middle layer, the sub-inner layer and the inner layer, sequentially performing melting, mixing and plasticizing, and then squeezing the plasticized materials in the five extruders into the die head of the same five-layer co-extrusion film blowing machine for fusion, and extruding them in a tubular shape through the die mouth, and then blowing molding, cooling and winding to obtain the light-converting agricultural film; The outer layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 45-55 parts of linear low-density polyethylene, 13-17 parts of metallocene polyethylene, 0.6-1.0 parts of antioxidant, 0.6-1.0 parts of light stabilizer, and 0.4-0.6 parts of antioxidant; The secondary outer layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 43-47 parts of linear low-density polyethylene, 12-14 parts of metallocene polyethylene, 4.5-5.5 parts of thermal insulation and light-conversion masterbatch, and 0.4-0.6 parts of antioxidant; The middle layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 50-60 parts of linear low-density polyethylene, 16-20 parts of metallocene polyethylene, 6.5-7.5 parts of thermal insulation and light-conversion masterbatch, and 0.4-0.6 parts of antioxidant; The secondary inner layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 43-47 parts of linear low-density polyethylene, 12-14 parts of metallocene polyethylene, 4.5-5.5 parts of thermal insulation and light-conversion masterbatch, and 0.4-0.6 parts of antioxidant; The inner layer material comprises the following components by weight: 22.5-27.5 parts of low-density polyethylene, 45-55 parts of linear low-density polyethylene, 13-17 parts of metallocene polyethylene, 0.6-1.0 parts of antioxidant, 0.6-1.0 parts of light stabilizer, and 0.4-0.6 parts of antioxidant.
2. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the acyl chloride treated hydrotalcite, the drying method is to dry the filtered hydrotalcite in an oven at 120° C. for 8 hours.
3. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the acyl chloride treated hydrotalcite, the hydrotalcite is magnesium aluminum hydrotalcite with a density of 2.0 g / cm 3 .
4. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the heat-insulating light-converting masterbatch by blending, the mixing method is to control the temperature to be 153-161° C., and to perform mixing for 45-60 minutes.
5. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the thermal insulation light conversion masterbatch by blending, the model of the organic light conversion agent is Ruiers R12; the model of the inorganic light conversion agent is Xiweier GTR650-II.
6. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the heat preservation and light conversion masterbatch by blending, the density of the linear low-density polyethylene is 0.919 g / cm 3 ; The model of the antioxidant is antioxidant 1076; the light stabilizer is a hindered amine stabilizer, model XT100.
7. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the light-converting film by blow molding, the extrusion working temperature of the outer and inner layer screws is set to 178-182°C, the extrusion working temperature of the sub-outer and sub-inner layer screws is set to 171-180°C, and the extrusion working temperature of the middle layer screw is set to 168-175°C.
8. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the light-converting film by blow molding, the density of the low-density polyethylene in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material, and the inner layer material is 0.917 g / cm 3 The density of linear low-density polyethylene is 0.919 g / cm 3 The density of metallocene polyethylene is 0.925 g / cm 3 .
9. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the light-converting film by blow molding, the antioxidants in the outer layer material, the sub-outer layer material, the middle layer material, the sub-inner layer material, and the inner layer material are all antioxidant 124; the light stabilizer in the outer layer material and the inner layer material is a hindered amine stabilizer, model XT100; and the antioxidant in the outer layer material and the inner layer material is antioxidant 1076.
10. The method for preparing a light-converting agricultural film according to claim 1, characterized in that: In the step of preparing the light-converting film by blow molding, the structure of the light-converting agricultural film is a five-layer structure from top to bottom, namely, an outer layer, a sub-outer layer, a middle layer, a sub-inner layer, and an inner layer. The thickness of the outer layer is 0.002 mm, the thickness of the sub-outer layer is 0.001 mm, the thickness of the middle layer is 0.002 mm, the thickness of the sub-inner layer is 0.001 mm, the thickness of the inner layer is 0.002 mm, and the total thickness of the light-converting agricultural film is 0.008 mm.