Porous catalytic electrode for electrolyzing water, preparation method of porous catalytic electrode and electrolyzing device

The solid-state deposition method forms a multi-scale catalytic functional layer on the surface of the nickel mesh, which solves the problems of pollution and low bonding strength caused by alkali activation treatment, achieves efficient and environmentally friendly electrode preparation, and improves the stability and catalytic performance of the electrode.

CN118756192AActive Publication Date: 2024-10-11HANDAN KELING NEW MATERIALS CO LTD

Patent Information

Application Number
CN202410845522.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-11
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

In the existing electrolysis water hydrogen production technology, the alkali activation treatment method pollutes the environment and has limited pore-forming capabilities, resulting in low bonding strength of porous electrodes and affecting long-term service performance.

Method used

The solid-state deposition method is used to accelerate the deposition of nickel carbonyl powder on the surface of the preheated nickel mesh to form a catalytic functional layer with a multi-scale structure, eliminating the alkali activation step and improving the bonding strength between the catalytic functional layer and the nickel mesh.

Benefits of technology

It significantly reduces environmental pollution, improves the bonding strength between the catalytic functional layer and the nickel mesh, increases the specific surface area and catalytic performance of the electrode, and extends the service life of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756192A_ABST
    Figure CN118756192A_ABST
Patent Text Reader

Abstract

The invention discloses a porous catalytic electrode for electrolyzing water, a preparation method of the porous catalytic electrode and an electrolysis device, and relates to the technical field of hydrogen production by electrolyzing water. A solid deposition method is adopted, carbonyl nickel powder is accelerated and then deposited on the surface of a preheated nickel net, when the carbonyl nickel powder collides with the surface of the nickel net, kinetic energy of the carbonyl nickel powder is converted into internal energy so that the surface of the nickel net can be melted, and then the carbonyl nickel powder is welded to the surface of the nickel net. When a large amount of carbonyl nickel powder is welded to the surface of the nickel net, a catalytic function layer with a multi-scale structure is formed on the surface of the nickel net. According to the method provided by the invention, the step of alkali liquor activation treatment can be omitted, the environmental pollution can be remarkably reduced, and meanwhile, the bonding strength of the catalytic functional layer and the nickel net is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen production by electrolysis of water, and in particular to a porous catalytic electrode for electrolysis of water, a preparation method thereof and an electrolysis device. Background Art

[0002] Hydrogen energy is an ideal clean energy and energy carrier with high energy density and no pollution. The use of renewable energy to generate electricity and produce hydrogen by electrolysis of water is considered to be one of the solutions for large-scale energy storage in the future. Among the mature or gradually commercialized water electrolysis hydrogen production technologies, alkaline water electrolysis (AWE) technology has the advantages of high efficiency and safety, and is very suitable for large-scale promotion in conjunction with renewable energy. It has broad application prospects in the fields of renewable energy and hydrogen energy.

[0003] In recent years, the plasma spraying method has been widely used in industry. A mixed powder containing metal powder and aluminum pore-forming agent is melted and sprayed onto a conductive substrate. Alkaline solution activation treatment is used to prepare a porous electrode to achieve the preparation of a porous catalytic coating on the electrode surface. The alkali solution activation treatment method not only pollutes the environment, but also has limited pore-forming capacity. In order to obtain more holes and a larger specific surface area, it is generally necessary to increase the aluminum powder content or increase the aluminum powder size. However, as the pore-forming aluminum powder content is too high or the size is too large, the interface bonding area of ​​the activated porous coating will be greatly reduced, resulting in low coating bonding strength, making the activated coating very easy to fall off, and the performance will be greatly reduced during long-term service.

[0004] Therefore, there is an urgent need to develop a method for preparing highly stable pure nickel electrodes, which can significantly improve the refinement of the electrode mesh surface structure without reducing the bonding strength of the activation layer, while reducing environmental pollution.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide a porous catalytic electrode for electrolyzing water, a preparation method thereof and an electrolysis device, aiming at preparing a porous catalytic electrode with strong coating bonding force without performing alkaline solution activation treatment.

[0007] The present invention is achieved in that:

[0008] In a first aspect, the present invention provides a method for preparing a porous catalytic electrode for electrolyzing water, comprising: preheating a nickel mesh, accelerating and depositing carbonyl nickel powder on the surface of the nickel mesh by a solid-state deposition method to form a catalytic functional layer.

[0009] In an optional embodiment, the carbonyl nickel powder is in the shape of a spherical ball, and the average particle size of the carbonyl nickel powder is 15 μm-30 μm.

[0010] In an optional embodiment, the deposition speed of the carbonyl nickel powder is 100 m / s-200 m / s, and the deposition thickness is 10 μm-20 μm;

[0011] Preferably, the carbonyl nickel powder is accelerated using a spray gun.

[0012] In an optional embodiment, the temperature of the nickel mesh after preheating is greater than 1400°C, preferably 1400°C-1450°C.

[0013] In an optional embodiment, a high-energy laser is used to preheat the area of ​​the nickel mesh where the coating is to be deposited, and the power of the laser is controlled to be 5kw-6kw;

[0014] Preferably, the preheating depth of the nickel mesh surface is less than 1 μm.

[0015] In an optional embodiment, before preheating the nickel mesh, the nickel mesh is pretreated to make the surface roughness Ra greater than 5 μm.

[0016] In an optional embodiment, the pretreatment process includes: sandblasting the nickel mesh to make the surface roughness meet the requirements, and then cleaning and drying.

[0017] In an optional embodiment, before depositing the carbonyl nickel powder, the nickel mesh is fixed on the platform and protected by a tooling.

[0018] In a second aspect, the present invention provides a porous catalytic electrode for electrolysis of water, which is prepared by the preparation method of any one of the aforementioned embodiments;

[0019] Preferably, the bonding strength between the catalytic functional layer and the nickel mesh is greater than 15 MPa.

[0020] In a third aspect, the present invention provides an electrolysis device, comprising the porous catalytic electrode for electrolyzing water according to the aforementioned embodiment.

[0021] The present invention has the following beneficial effects: the present invention adopts a solid-state deposition method to accelerate the base nickel powder and deposit it on the preheated nickel mesh surface. When the carbonyl nickel powder hits the nickel mesh surface, the kinetic energy of the carbonyl nickel powder is converted into internal energy to melt the nickel mesh surface, and then welded to the nickel mesh surface. When a large amount of carbonyl nickel powder is welded to the nickel mesh surface, a catalytic functional layer with a multi-scale structure will be formed on the nickel mesh surface. The method provided by the present invention can save the step of alkali solution activation treatment, can significantly reduce environmental pollution, and at the same time improve the bonding strength between the catalytic functional layer and the nickel mesh. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 A schematic diagram of the formation principle of the catalytic functional layer provided in an embodiment of the present invention;

[0024] Figure 2 This is a SEM image of the spherical carbonyl nickel powder used in the embodiment of the present invention;

[0025] Figure 3 The surface morphology of the catalytic functional layer prepared in the embodiment of the present invention;

[0026] Figure 4 This is a partial enlarged view of the surface of the catalytic functional layer prepared in an embodiment of the present invention;

[0027] Figure 5 This is a SEM image of the conventional nickel powder used in the comparative example;

[0028] Figure 6 This is a surface morphology image of a catalytic functional layer prepared in a comparative example;

[0029] Figure 7 This is a partial enlarged view of the surface prepared in comparative example. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0031] The present invention provides a method for preparing a porous catalytic electrode for water electrolysis, comprising the following steps:

[0032] S1. Provide carbonyl nickel powder and nickel mesh

[0033] The embodiment of the present invention uses micron-level carbonyl nickel powder with high surface activity, which has higher purity than the nickel powder used for conventional plasma spraying, and is beneficial to improving the catalytic performance of the electrode.

[0034] In some embodiments, Figure 1As shown, the carbonyl nickel powder is in the shape of a spherical ball, and the average particle size of the carbonyl nickel powder is 15 μm-30 μm. The use of the carbonyl nickel powder with a micro-nano structure can form a catalytic functional layer with a multi-scale structure on the surface of the nickel mesh.

[0035] Specifically, the carbonyl nickel powder used in the embodiment of the present invention can be a commercially available material, such as carbonyl nickel powder model D5015 that can be purchased from Changsha Tianjiu Metal Materials Co., Ltd.

[0036] The nickel mesh can be a commercially available nickel plate mesh. Any nickel plate mesh suitable for use as an electrolytic water electrode is suitable for the preparation method provided in the embodiment of the present invention, such as a 60# nickel mesh model purchased from Jiangyin Baike Nickel Mesh Co., Ltd.

[0037] S2. Nickel mesh pretreatment

[0038] Before step S3, the nickel mesh is pretreated to make the surface roughness Ra greater than 5 μm, forming a roughened electrode to facilitate laser absorption during heating and further improve the bonding strength between the catalytic functional layer and the nickel mesh.

[0039] In some embodiments, the pretreatment process includes: sandblasting the nickel mesh to make the surface roughness meet the requirements, and then cleaning and drying. Specifically, different sandblasting conditions can be used to sandblast the surface of the plate mesh to make the surface roughness meet the requirements. The reagents used for cleaning are not limited, and organic reagents (such as acetone) can be used for cleaning; the drying method is not limited, and compressed gas can be used to blow dry the surface of the plate mesh, so that the surface of the nickel mesh is flat and defect-free after pretreatment.

[0040] In some embodiments, before depositing the carbonyl nickel powder, the nickel mesh is fixed on the platform and protected by a tooling to save the powder raw materials. The nickel mesh is fixed and clamped to prevent loosening during the deposition process.

[0041] In another embodiment, if the surface roughness of the nickel mesh meets the requirements, no pretreatment is required.

[0042] S3. Deposition of catalytic functional layer

[0043] After preheating the nickel mesh, the carbonyl nickel powder is accelerated and deposited on the surface of the nickel mesh by solid deposition to form a catalytic functional layer (i.e., catalytic working layer). After the accelerated carbonyl nickel powder hits the surface of the nickel mesh, the kinetic energy of the carbonyl nickel powder is converted into internal energy to melt the surface of the nickel mesh, and then welded to the surface of the nickel mesh. When a large amount of carbonyl nickel powder is welded to the surface of the nickel mesh, a catalytic functional layer with a multi-scale structure will be formed on the surface of the nickel mesh.

[0044] In some embodiments, the preheated temperature of the nickel mesh is greater than 1400°C, preferably 1400°C-1450°C, and the preheated temperature of the nickel mesh is regulated so that the carbonyl nickel powder can form a uniform catalytic functional layer after impacting the surface of the nickel mesh. Specifically, the preheated temperature of the nickel mesh can be 1410°C, 1420°C, 1430°C, 1440°C, 1450°C, etc.

[0045] In some embodiments, a high-energy laser can be used to preheat the area of ​​the nickel mesh to be deposited with a coating. The laser power is controlled to be 5kw-6kw. The high-energy laser can be used for preheating, so that the area to be deposited with the coating can quickly reach the preheating temperature. The preheating depth of the nickel mesh surface can be less than 1μm. If the preheating depth is too large, the energy consumption will increase significantly and the nickel mesh will be deformed.

[0046] Furthermore, the carbonyl nickel powder can be accelerated by a spray gun. In actual operation, the electrolytic nickel powder can be accelerated by a high-pressure inert gas (such as argon) through a spray gun, and the accelerated carbonyl nickel powder is embedded in the nickel mesh, and the formed catalytic functional layer has a high bonding strength with the nickel mesh. Specifically, the gas pressure of the high-pressure inert gas is 3MPa-10MPa.

[0047] In some embodiments, the deposition rate of the carbonyl nickel powder is 100m / s-200m / s, and the deposition thickness is 10μm-20μm. By adjusting the deposition rate of the carbonyl nickel powder so that the carbonyl nickel powder hits the surface of the nickel mesh, the collision surface of the carbonyl nickel powder can be melted, thereby enabling the carbonyl nickel powder to be directly welded to the surface of the nickel mesh. The deposition rate and deposition thickness of the carbonyl nickel powder within the above range can further improve the bonding strength between the catalytic functional layer and the nickel mesh, thereby improving the catalytic effect of the electrode.

[0048] Specifically, the deposition speed of the carbonyl nickel powder can be 100 m / s, 130 m / s, 150 m / s, 180 m / s, 200 m / s, etc., and the deposition thickness can be 10 μm, 13 μm, 15 μm, 18 μm, 20 μm, etc.

[0049] It should be noted that, compared with the traditional spraying and activation process, the preparation method provided by the embodiment of the present invention is not limited in preparation size, and a catalytic functional layer with a multi-scale structure and fineness can be obtained. The manufactured electrode has a large specific surface area and excellent catalytic performance. In addition, the catalytic functional layer prepared by the embodiment of the present invention has a high interface bonding strength with the nickel mesh, which can greatly improve the stability of the nickel mesh, and the catalytic functional layer is not easy to fall off; the efficiency of catalytic electrode preparation can be greatly improved, the preparation cycle is significantly shortened, and the equipment, maintenance, and manufacturing costs are significantly reduced.

[0050] The embodiment of the present invention also provides a porous catalytic electrode for electrolyzing water, which is prepared by the above preparation method, and a catalytic functional layer with very high bonding strength is formed on the nickel mesh, and the bonding strength between the catalytic functional layer and the nickel mesh is greater than 15MPa.

[0051] An embodiment of the present invention further provides an electrolysis device, including the above-mentioned porous catalytic electrode for electrolyzing water, and may also include an electrolytic cell to form a complete set of water electrolysis devices.

[0052] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0053] Example 1

[0054] This embodiment provides a method for preparing a porous catalytic electrode for electrolysis of water, comprising the following steps:

[0055] (1) Provide carbonyl nickel powder and nickel mesh

[0056] The carbonyl nickel powder used in this embodiment is in the shape of a spherical ball, and the average particle size of the carbonyl nickel powder is 20 μm. Figure 2 As shown, it can be seen that the carbonyl nickel powder is in a relatively uniform spherical shape.

[0057] The nickel mesh wire diameter is 150 μm and the mesh number is 40 meshes.

[0058] (2) Nickel mesh pretreatment

[0059] Sandblast the nickel mesh to make the surface roughness Ra reach 6μm, then clean it with acetone, and then blow dry the surface of the plate mesh with compressed gas. The surface of the plate mesh after treatment is required to be free of impurities. Fix the nickel mesh on the platform and protect it with tooling.

[0060] (3) Deposition of catalytic functional layer

[0061] First, the area of ​​the nickel mesh where the coating is to be deposited is preheated using a fiber high-energy laser (5.5 kW). When the preheating temperature of the nickel mesh surface reaches the set temperature of 1400°C, a spray gun is used to accelerate the spherical carbonyl nickel powder, and the deposition speed is controlled to be 150 m / s and the deposition thickness to be 15 μm.

[0062] The morphology of the catalytic functional layer prepared in this example is shown in Figure 3 and Figure 4 As shown, it can be seen that the coating surface is uniform, with high roughness and many pores and protrusions.

[0063] The test shows that the hydrogen production current density of the catalytic functional layer prepared in this embodiment can reach 0.8A / cm 2 .

[0064] Example 2

[0065] The only difference from Example 1 is that the parameters of step (3) are different, as follows:

[0066] First, the area of ​​the nickel mesh where the coating is to be deposited is preheated using a fiber high-energy laser (5.0 kW). When the preheating temperature of the nickel mesh surface reaches the set temperature of 1450°C, a spray gun is used to accelerate the spherical carbonyl nickel powder, and the deposition speed is controlled to be 100 m / s and the deposition thickness is 10 μm.

[0067] Example 3

[0068] The only difference from Example 1 is that the parameters of step (3) are different, as follows:

[0069] First, the area of ​​the nickel mesh where the coating is to be deposited is preheated using a fiber high-energy laser (6.0 kW). When the preheating temperature of the nickel mesh surface reaches the set temperature of 1420°C, a spray gun is used to accelerate the spherical carbonyl nickel powder, and the deposition speed is controlled to be 200 m / s and the deposition thickness is 20 μm.

[0070] Comparative Example 1

[0071] The only difference between this comparative example and Example 1 is that the nickel mesh is not laser heated, the temperature of the nickel mesh is room temperature, and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.

[0072] The results showed that the surface temperature of the nickel mesh was too low, the hardness was too high, the surface of the deposited particles was not melted, and the carbonyl nickel powder could not be deposited.

[0073] Comparative Example 2

[0074] The only difference between this comparative example and Example 1 is that the surface of the nickel mesh is not roughened by sandblasting, and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.

[0075] The results showed that the laser absorption rate was insufficient, the surface temperature of the nickel mesh was too low, the deposition efficiency of the carbonyl nickel powder was low, the interface bonding was weak, and the bonding strength was less than 5MPa.

[0076] Comparative Example 3

[0077] The only difference between this comparative example and Example 1 is that a nozzle is used to accelerate the carbonyl nickel powder with an average particle size of 20 μm to 800 m / s, and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.

[0078] The results show that the carbonyl nickel powder speed is too high, and the kinetic energy of the carbonyl nickel powder is largely converted into the internal energy of the material, resulting in the overall softening and collapse of the carbonyl nickel powder particles, the destruction of the micro-nano structure, the reduction of the electrolytic catalytic area, and the hydrogen production current density can reach 0.6A / cm 2 .

[0079] Comparative Example 4

[0080] The only difference between this comparative example and Example 1 is that conventional aerosolized spherical nickel powder is used, and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.

[0081] The results show that the deposition of spherical powder cannot form a micro-nanoscale structure on the surface of the nickel mesh, the electrocatalytic contact area is greatly reduced, and the hydrogen production current density can reach 0.5A / cm 2 .

[0082] Comparative Example 5

[0083] The difference between this comparative example and Example 1 is that conventional atomized spherical nickel powder (same as comparative example 4) is used, and the catalytic functional layer is prepared by conventional plasma spraying method. The morphology of the atomized spherical nickel powder used in this comparative example is shown in FIG. Figure 5 , it can be seen that the inner powder is spherical or quasi-spherical.

[0084] The morphology of the catalytic functional layer prepared in Comparative Example 5 is as follows Figure 6 and Figure 7 As shown, it can be seen that the powder is fully melted, the coating is relatively dense, and no large-scale micron or nano-scale holes are formed. After testing, the hydrogen production current density of the catalytic functional layer prepared in Comparative Example 5 is only 0.3A / cm 2 .

[0085] Comparative Example 6

[0086] The only difference between this comparative example and Example 1 is that the preheating temperature in step (3) is 1500°C.

[0087] The results showed that the nickel mesh was partially melted and deformed as a whole and could not be used.

[0088] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a porous catalytic electrode for water electrolysis, characterized in that: include: After the nickel mesh is preheated, the carbonyl nickel powder is accelerated and deposited on the surface of the nickel mesh by a solid-state deposition method to form a catalytic functional layer.

2. The preparation method according to claim 1, characterized in that: The carbonyl nickel powder is in the shape of a spherical ball, and the average particle size of the carbonyl nickel powder is 15 μm-30 μm.

3. The preparation method according to claim 1, characterized in that: The deposition speed of the carbonyl nickel powder is 100m / s-200m / s, and the deposition thickness is 10μm-20μm; Preferably, the carbonyl nickel powder is accelerated using a spray gun.

4. The preparation method according to claim 1, characterized in that: The temperature of the nickel mesh after preheating is greater than 1400°C, preferably 1400°C-1450°C.

5. The preparation method according to claim 4, characterized in that: A high-energy laser is used to preheat the area of ​​the nickel mesh to be coated, and the power of the laser is controlled to be 5kw-6kw; Preferably, the preheating depth of the nickel mesh surface is less than 1 μm.

6. The preparation method according to claim 1, characterized in that: Before preheating the nickel mesh, the nickel mesh is pretreated to make the surface roughness Ra greater than 5 μm.

7. The preparation method according to claim 6, characterized in that: The pretreatment process includes: sandblasting the nickel mesh to make the surface roughness meet the requirements, and then cleaning and drying.

8. The preparation method according to claim 1, characterized in that: Before depositing the carbonyl nickel powder, the nickel mesh is fixed on a platform and protected by a tooling.

9. A porous catalytic electrode for water electrolysis, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8; Preferably, the bonding strength between the catalytic functional layer and the nickel mesh is greater than 15 MPa.

10. An electrolysis device, characterized in that: It comprises the porous catalytic electrode for water electrolysis as claimed in claim 9.

Citation Information

Patent Citations

  • Porous nickel net water electrolysis catalysis material and preparation method thereof

    CN113174600A

  • Coating preparation method based on cold spraying, cold spraying device and cold spraying coating

    CN114277367A

  • Porous metal material and manufacturing method and application thereof

    CN115229188A

  • Ni-Fe coating based on solid deposition technology and preparation method and application of Ni-Fe coating

    CN116145126A

  • Nickel coating catalyst, preparation method and application thereof

    CN117822024A

Cited By

  • Alkaline electrolytic bath, nickel net catalyst coating of alkaline electrolytic bath and spraying process and application of nickel net catalyst coating

    CN119020770A