Negative plate net for electrolyzing water, preparation method of negative plate net and electrolyzing device
Through atmospheric plasma spraying and laser heating technology, a nickel-aluminum mixed coating with high bonding strength is formed, which solves the problem of poor bonding between the electrode catalytic layer and the electrode matrix, and improves the stability and life of the water electrolysis hydrogen production electrode.
Patent Information
- Application Number
- CN202410845510.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-27
AI Technical Summary
In the existing electrolysis water hydrogen production technology, the combination of the electrode catalytic layer and the electrode matrix is not tight, resulting in peeling, falling off and performance degradation of the catalytic layer, affecting electrolysis efficiency and electrode life.
The atmospheric plasma spraying method is used to spray molten nickel and aluminum droplets onto the surface of the heated electrode plate to form a nickel-aluminum mixed coating, and laser heating is used to promote the diffusion of the nickel-aluminum interface to form a nickel-aluminum alloy, which improves the catalytic layer and the electrode matrix. binding strength and activity.
A porous nickel coating with high interface bonding strength and high activity is achieved, which improves the stability and life of the electrode and meets the requirements for efficient and stable service.
Smart Images

Figure CN118756201A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogen production by electrolyzing water, and in particular to a cathode plate mesh for electrolyzing water, a preparation method thereof and an electrolysis device. Background Art
[0002] Hydrogen energy has been vigorously promoted as a clean energy source. The most promising way to produce hydrogen is to use renewable energy to generate electricity and produce green hydrogen by alkaline water electrolysis. One of the important factors restricting the industrial application of water electrolysis hydrogen production technology is the cost of electricity. Therefore, developing highly active and stable water electrolysis hydrogen production catalytic electrodes to achieve higher current density is one of the important development directions of water electrolysis hydrogen production electrodes.
[0003] At present, there are many methods for preparing water electrolysis electrodes, such as using hydrothermal method to synthesize transition metal-based catalysts on substrates such as nickel foam; or using electroplating method to deposit alloy, sulfide, nitride and other coatings on the surface of conductive substrates; or using coating method to deposit precious metals and their oxide catalysts, but the above methods are complex processes, some of which require multiple drying and sintering, and the process flow is time-consuming, inefficient and costly. The most mainstream technology in the industry is still based on plasma spraying method, using a simple nickel-aluminum mixing method to prepare a layer of nickel-aluminum mixed coating on the surface of pure nickel electrode. The overall use effect of this method is relatively reliable. However, during use, under the continuous and violent flushing of a large amount of hydrogen and water flow, especially under high pressure and high temperature service conditions, conventional plasma spraying methods are difficult to ensure the close bonding between the deposited nickel particles and the nickel electrode substrate, resulting in the peeling, shedding and loss of the catalyst layer, which in turn causes the increase of membrane electrode internal resistance and performance degradation, which is extremely unfavorable to maintaining the performance, stability and life of the electrode.
[0004] Therefore, improving the bonding between the catalyst layer and the electrode body while improving the electrolysis efficiency can extend the operating life, which is also one of the bottlenecks faced by the development of water electrolysis electrodes. At present, it is urgent to develop a plasma spraying process suitable for large-scale industrial production, so that the prepared catalytic coating electrode has the advantages of high specific surface area and high bonding strength.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a cathode plate mesh for electrolyzing water, a preparation method thereof and an electrolysis device, aiming to provide a simple and easy method for manufacturing a porous nickel coating with high interface bonding strength and high activity on the surface of the electrode plate mesh.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides a method for preparing a cathode plate mesh for electrolyzing water, comprising:
[0009] Using the atmospheric plasma spraying method, molten nickel droplets and molten aluminum droplets are sprayed onto the surface of the heated electrode plate mesh to form a nickel-aluminum mixed coating;
[0010] The nickel-aluminum mixed coating is heated to form a nickel-aluminum alloy.
[0011] In an optional embodiment, the deposition rate of the melted nickel droplets and the melted aluminum droplets is less than 150 m / s;
[0012] Preferably, the deposition rate of the melted nickel droplets and aluminum droplets is 50 m / s-80 m / s.
[0013] In an optional embodiment, nickel powder and aluminum powder are used as raw materials and melted into nickel droplets and aluminum droplets, and the mass ratio of nickel powder to aluminum powder is 1: (0.2-0.3);
[0014] Preferably, the particle size range of nickel powder and aluminum powder is 45 μm-78 μm;
[0015] Preferably, the purity of the nickel powder and the aluminum powder is greater than 99.5%.
[0016] In an optional embodiment, the surface of the electrode plate mesh is heated to 200° C.-300° C. by a pre-treatment laser heating system, and then nickel droplets and aluminum droplets are sprayed;
[0017] Preferably, the surface of the electrode plate mesh is heated to 250°C-280°C by a pre-treatment laser heating system;
[0018] Preferably, the power of the pre-processing laser heating system is 1KW-2KW.
[0019] In an optional embodiment, the nickel-aluminum mixed coating is heated to 500° C.-600° C. using a post-processing laser, and the laser power of the post-processing laser is controlled to be 4 KW-6 KW.
[0020] In an optional embodiment, the surface of the electrode plate mesh is heated by a pre-processing laser heating head in a pre-processing laser heating system, and the nickel-aluminum mixed coating is heated by a post-processing laser heating head;
[0021] The pre-treatment laser heating head, the atmospheric plasma spray gun and the post-treatment laser heating head which are arranged in sequence are fixed on the movable slide rail, so that the pre-treatment laser heating head, the atmospheric plasma spray gun and the post-treatment laser heating head are linked with the same track and speed, and the post-treatment laser heating head irradiates the deposited nickel-aluminum mixed coating area, and controls the overall horizontal movement rate to be 500mm / s-1000mm / s;
[0022] Preferably, the spacing of atmospheric plasma spraying is 500mm-600mm;
[0023] Preferably, the atmospheric plasma spray gun is controlled to move in a U-shaped deposition path, and when moving in the reverse direction, the pre-processing laser heating head and the post-processing laser heating head exchange roles and powers.
[0024] In an optional embodiment, the light spots of the pre-processing laser heating head and the post-processing laser heating head are both square light spots, the nickel-aluminum mixed droplet area corresponding to the atmospheric plasma spray gun is circular, and the square light spots of the pre-processing laser heating head and the post-processing laser heating head are tangent to the nickel-aluminum mixed droplet area;
[0025] Preferably, the length of the square light spot is greater than the diameter of the nickel-aluminum mixed droplet zone, and the length of the square light spot is 40mm-60mm, the width is 40mm-60mm, and the diameter of the nickel-aluminum mixed droplet zone is 30mm-50mm.
[0026] In an optional embodiment, before depositing the coating, the electrode plate mesh is sequentially cleaned and sandblasted, and then a protective fixture is installed in the pores on the electrode plate mesh and the edge of the electrode plate mesh, and then dusting, degreasing, cleaning and drying are sequentially performed;
[0027] Preferably, the dried electrode plate mesh is fixed on a fixing table before coating deposition, so that the electrode plate mesh remains in a fixed position during the coating deposition process.
[0028] In a second aspect, the present invention provides a cathode plate mesh for water electrolysis, which is prepared by the preparation method of any one of the aforementioned embodiments.
[0029] In a third aspect, the present invention provides an electrolysis device, comprising the cathode plate mesh for electrolyzing water according to the aforementioned embodiment.
[0030] The present invention has the following beneficial effects: the atmospheric plasma spraying method is used to spray molten nickel droplets and molten aluminum droplets onto the surface of the heated electrode plate mesh, so that the heated electrode plate mesh surface and the molten nickel droplets and molten aluminum droplets are more likely to diffuse, and the contact nickel / aluminum and nickel / nickel bonding areas are increased, while a large amount of elements diffuse to form a strong bond; the nickel-aluminum mixed coating on the coating surface is heated, and while promoting the interface bonding of the deposited particles, the nickel-aluminum interface is diffused to form a nickel-aluminum alloy, thereby further improving the surface activity of the porous nickel coating after de-aluminization activation.
[0031] The catalytic nickel coating is prepared on the surface of the electrode plate mesh by the preparation method provided in the embodiment of the present invention, so that a porous nickel coating with high interface bonding strength and high activity can be manufactured, which can meet the requirements of efficient and stable service in the electrolytic cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 Schematic diagram for preparing a high-purity, high-activity porous catalytic layer on the surface of the electrolytic cell electrode plate mesh;
[0034] Figure 2 Microscopic morphology of the surface of the cathode electrode coating for alkaline water electrolysis prepared by conventional plasma spraying process; in the figure, (b) is a partial enlargement of (a);
[0035] Figure 3 Microscopic morphology of the surface of the cathode electrode coating for alkaline water electrolysis prepared by the method of the embodiment of the present invention; in the figure, (b) is a partial enlargement of (a). DETAILED DESCRIPTION
[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0037] The embodiment of the present invention provides a method for preparing a cathode plate mesh for electrolyzing water, comprising:
[0038] S1. Pre-treatment
[0039] Before depositing the coating, the electrode plate mesh is pre-treated to remove impurities and clean the surface, which is beneficial to improving the bonding effect between the coating and the electrode plate mesh.
[0040] In some embodiments, the pre-treatment steps include: cleaning and sandblasting the electrode plate mesh in sequence, then assembling protective fixtures in the pores on the electrode plate mesh and the edges of the electrode plate mesh, and then deashing, degreasing, cleaning and drying in sequence. Sandblasting can improve the surface roughness, which is beneficial to the bonding of the coating and the substrate. Deashing, degreasing and other means can achieve the purpose of surface cleaning, which is beneficial to further improve the bonding effect of the coating.
[0041] It should be noted that, in other embodiments, if the roughness and surface cleanliness of the electrode plate mesh meet the requirements, no pre-treatment is required.
[0042] In some embodiments, the dried electrode plate mesh is fixed on a fixed table before coating deposition, so that the electrode plate mesh remains in a fixed position during the coating deposition process, thereby improving the stability of the device operation.
[0043] Specifically, the electrode plate mesh is made of high-purity nickel with a purity of >99.9%.
[0044] S2, heating-spraying-reheating
[0045] The electrode plate mesh is first heated, and after the temperature reaches the required level, molten nickel droplets and molten aluminum droplets are sprayed onto the surface of the heated electrode plate mesh by using an atmospheric plasma spraying method, so that the heated electrode plate mesh surface and the molten nickel droplets and molten aluminum droplets are more easily diffused to form a nickel-aluminum mixed coating; after the coating is formed, the nickel-aluminum mixed coating formed on the coating surface is heated to diffuse the nickel-aluminum interface to form a nickel-aluminum alloy, thereby further improving the surface activity of the porous nickel coating after de-aluminization activation.
[0046] In some embodiments, a pre-treatment laser heating system is used to heat the surface of the electrode plate mesh to 200°C-300°C (preferably 250°C-280°C), and then nickel droplets and aluminum droplets are sprayed; similarly, a post-treatment laser is used to heat the nickel-aluminum mixed coating to 500°C-600°C (such as 500°C, 500°C, 530°C, 550°C, 580°C, 600°C, etc.). The laser heating method is easy to operate and control. The power of the pre-treatment laser heating system is 1KW-2KW, and the laser power of the post-treatment laser is controlled to be 4KW-6KW. It is advisable that the power of the front and rear laser heating is controlled within the above range so that the preset temperature can be reached faster.
[0047] Specifically, the temperature of the electrode plate mesh surface after heating by the pre-processing laser heating system can be 200°C, 230°C, 250°C, 280°C, 300°C, etc., and the power of the pre-processing laser heating system can be 1.0KW, 1.5KW, 2.0KW, etc.; the laser power of the post-processing laser can be 4.0KW, 4.5KW, 5.0KW, 5.5KW, 6.0KW, etc.
[0048] In some embodiments, please combine Figure 1, nickel powder and aluminum powder are used as raw materials, and are melted into nickel droplets and aluminum droplets by atmospheric plasma spraying. The mass ratio of nickel powder to aluminum powder is 1:(0.2-0.3), such as 1:0.20, 1:0.23, 1:0.25, 1:0.28, 1:0.30, etc. After the nickel powder and aluminum powder are mixed, they are heated and melted to produce nickel droplets and aluminum droplets. The amount ratio of nickel powder to aluminum powder is preferably within the above range to further improve the surface activity of the porous nickel coating. The particle size range of nickel powder and aluminum powder is 45μm-78μm, and the purity of nickel powder and aluminum powder is greater than 99.5%. The small particle size of nickel powder and aluminum powder is conducive to forming a uniform coating; the purity of nickel powder and aluminum powder is high, which is conducive to improving the purity of the coating.
[0049] Specifically, the particle sizes of nickel powder and aluminum powder may be the same or different, preferably between 45 μm and 78 μm, such as 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 78 μm, etc.
[0050] Further, the deposition rate of the melted nickel droplets and aluminum droplets is less than 150m / s; preferably, the deposition rate of the melted nickel droplets and aluminum droplets is 50m / s-80m / s. The deposition rate of the nickel droplets and aluminum droplets is preferably within the above range, which has reduced droplet splashing and improved interface bonding and deposition efficiency. Specifically, the deposition rate of the nickel droplets and aluminum droplets can be 10m / s, 30m / s, 50m / s, 60m / s, 70m / s, 80m / s, 100m / s, 120m / s, 140m / s, 145m / s, etc.
[0051] like Figure 1 As shown, the electrode plate mesh surface is heated by the pre-treatment laser heating head in the pre-treatment laser heating system, and the nickel-aluminum mixed coating is heated by the post-treatment laser heating head; the pre-treatment laser heating head, the atmospheric plasma spray gun and the post-treatment laser heating head are fixed on the movable slide rail in sequence, so that the pre-treatment laser heating head, the atmospheric plasma spray gun and the post-treatment laser heating head are linked with the same moving trajectory and speed. After the atmospheric plasma spray gun is treated, a conventional catalytic layer is formed, and the post-treatment laser heating head irradiates the deposited nickel-aluminum mixed coating area to form an optimized catalytic layer, while promoting the interface bonding of the deposited particles, a diffusion layer is formed at the interface of the nickel-aluminum single substance mixed coating, thereby further improving the surface activity of the porous nickel coating after de-aluminization activation. By assembling the pre-treatment laser heating head, the gas plasma spray gun and the post-treatment laser heating head, the spraying process can be more conveniently controlled, and the conditions of each area of the coating can be better controlled, thereby improving the uniformity of the coating.
[0052] Specifically, during the movement, the pre-treatment laser heating head is first used to heat a part of the electrode plate mesh, and then atmospheric plasma spraying is used to spray molten nickel droplets and aluminum droplets in this area for deposition to form a coating. The post-treatment laser heating head irradiates the area where the coating has been formed to achieve nickel-aluminum diffusion. The high-frequency post-treatment laser heating head linked with atmospheric plasma spraying can irradiate the area to be overlapped with the old catalyst layer before starting a new round of deposition on the surface of the formed catalyst layer, so that a diffusion layer is formed at the interface of the nickel-aluminum single-element mixed coating, thereby further improving the surface activity of the porous nickel coating after de-aluminization activation.
[0053] In some embodiments, control Figure 1 The overall horizontal moving speed of the device is 500mm / s-1000mm / s, such as 500mm / s, 600mm / s, 700mm / s, 800mm / s, 900mm / s, 1000mm / s, etc. The spacing of atmospheric plasma spraying is 500mm-600mm (such as 500mm, 530mm, 550mm, 580mm, 600mm, etc.), and the spacing of atmospheric plasma spraying refers to the spacing between the spray gun and the electrode plate mesh. By controlling parameters such as spacing, moving speed, and heating temperature, the temperature of the heated electrode plate mesh can be further controlled to improve the bonding strength of the coating on the electrode plate mesh.
[0054] The atmospheric plasma spray gun can be controlled to move in a U-shaped deposition path. When moving in the reverse direction, the pre-processing laser heating head and the post-processing laser heating head exchange roles and powers, that is, when moving in the reverse direction, the original pre-processing laser heating head becomes the post-processing laser heating head, and the original post-processing laser heating head becomes the pre-processing laser heating head.
[0055] like Figure 1 As shown, the light spots of the pre-treatment laser heating head and the post-treatment laser heating head are both square spots. For the pre-treatment light spots and the post-treatment light spots in the figure, the nickel-aluminum mixed droplet area corresponding to the atmospheric plasma spray gun is a circle with a diameter of D, and the square light spots of the pre-treatment laser heating head and the post-treatment laser heating head are tangent to the nickel-aluminum mixed droplet area. Figure 1 In the figure, the circular plasma spraying area is tangent to the square spots on both sides. When working, the pre-treatment laser heating head, atmospheric plasma spraying and post-treatment laser heating head work simultaneously. For the same area, it is heated first, then sprayed, and finally heated and diffused. The "tangent" here means roughly tangent, and there can also be a small gap. The short sides of the two square spots of the post-treatment laser heating head and the laser heating head overlap, and cover the overlapping area of the new and old catalyst layers.
[0056] Furthermore, the length of the square light spot is greater than the diameter of the nickel-aluminum mixed droplet area, that is, L>D, and the length of the square light spot is 40mm-60mm (such as 40mm, 50mm, 60mm, etc.), the width is 40mm-60mm (such as 40mm, 50mm, 60mm, etc.), and the diameter of the nickel-aluminum mixed droplet area is 30mm-50mm (such as 30mm, 40mm, 50mm, etc.). By optimizing the size of each area, the temperature can be controlled more accurately, so that the coating is evenly attached to the plate mesh.
[0057] The embodiment of the present invention provides a cathode plate mesh for electrolyzing water, which is prepared by the above-mentioned preparation method. The nickel coating on the surface of the electrode plate mesh has very high bonding strength and can meet the requirement of long-term service above 80°C.
[0058] The embodiment of the present invention further provides an electrolysis device, including the above-mentioned cathode plate mesh for electrolyzing water, and may also include an electrolytic cell, etc., to form a complete set of water electrolysis device.
[0059] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0060] Example 1
[0061] This embodiment provides a method for preparing a cathode plate mesh for electrolyzing water, comprising:
[0062] (1) Pretreatment: The surface of the electrolytic cell electrode plate mesh (made of 40#, 99.9% pure nickel mesh) is cleaned and sandblasted in turn, and then protective clamps are installed in the pores on the electrode plate mesh and the edges of the electrode plate mesh. Then, the mesh is deashed, degreased, cleaned and dried. The surface of the treated electrode plate mesh is required to be free of impurities. Finally, the electrode plate mesh is installed on the electrode plate mesh fixing table and fixed to ensure that the electrode plate mesh does not move during the preparation of the catalyst layer.
[0063] (2) Figure 1 As shown, the pre-treatment laser heating head, the atmospheric plasma spray gun, and the post-treatment laser heating head are fixed on a movable slide rail, and the three are linked, with the same moving trajectory and speed; when the catalytic layer on the surface of the electrode plate mesh is prepared, the nozzle movement path is a simple U-shaped deposition path; in conjunction with the movable slide rail, the solid-state deposition atmospheric plasma spray can move at a constant speed of 500mm / s relative to the surface of the electrode plate mesh.
[0064] (3) Mobile laser heating head, atmospheric plasma spray gun and high-frequency post-processing laser heating head. Before depositing powder, the laser heating system is used to heat the surface of the electrode plate mesh. The supersonic melted nickel droplets and aluminum droplets ejected from the nozzle, where the volume ratio of nickel and aluminum powder is 1:0.25, collide with the laser-heated electrode plate mesh surface. The melted nickel droplets and aluminum droplets and the electrode plate mesh surface materials will be more likely to diffuse, and the contact and bonding area will increase. At the same time, a large number of elements diffuse to form a strong bond. Among them, the front and rear treatment laser heating heads are square spots with a side length of 50mm, and the diameter of the nickel-aluminum mixed droplet area is 40mm; the power of the front treatment laser heating head is 2000W, and the pre-treatment laser heating system makes the temperature of the square area with a side length of 50mm on the surface of the electrode plate mesh reach about 250℃. Through plasma spraying, nickel powder and aluminum powder with purity greater than 99.5%, spherical shape and average particle size of 50μm are melted and accelerated to 80m / s. When the molten nickel droplets and aluminum droplets are successively deposited on the surface of the heated electrode plate mesh, a catalytic coating with a thickness of 50μm is formed on the wall of the electrode plate mesh.
[0065] (4) A 6000W post-processing laser heating head is used to irradiate the surface of the formed catalytic layer, and the surface of the catalytic layer is heated to about 550°C, so that a diffusion layer is formed at the interface of the nickel-aluminum mixed coating, thereby further improving the surface activity of the porous nickel coating after de-aluminization activation.
[0066] The cathode plate mesh prepared in this example was subjected to performance testing using the following testing methods: (1) physical folding; (2) precise weighing; and (3) electrochemical testing.
[0067] After testing, the catalytic coating was folded 90° and kept in this form for more than 5 seconds, and the coating did not fall off at the crease and no substrate was exposed; the catalytic coating was folded 120° and kept in this form for more than 5 seconds, and the coating did not fall off at the crease and no substrate was exposed; the catalytic coating was folded 180° and kept in this form for more than 5 seconds, and the coating did not fall off at the crease and no substrate was exposed; after the coating was activated with 30wt% potassium hydroxide solution for 24h and ultrasonicated for 30min, the coating weight loss rate was 15%; the hydrogen evolution current was 100mA / cm 2 , hydrogen evolution overpotential is 0.3V.
[0068] Comparative Example 1
[0069] The only difference between this comparative example and Example 1 is that no post-processing laser is used to heat and diffuse the deposited catalytic layer, and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.
[0070] The surface microstructure of the electrode coating prepared in this comparative example is as follows Figure 2 As shown, the surface microstructure of the electrode coating prepared in Example 1 is as follows Figure 3As shown. It can be seen that: the results show that compared with Example 1, the catalytic coating is folded at 90°, 120°, and 180°, and there is no shedding of the coating at the fold and no substrate is exposed; after the coating is activated by 30wt% potassium hydroxide solution for 24h and ultrasonicated for 30min, the coating weight loss rate is 18%; the hydrogen evolution current is 100mA / cm 2 The hydrogen evolution overpotential is 0.33V, which has increased, and the hydrogen evolution performance is poor.
[0071] Comparative Example 2
[0072] The only difference between this comparative example and Example 1 is that a laser heating device is used, the heating temperature of the electrode plate mesh surface is 600° C., and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.
[0073] The results show that compared with Example 1, in Comparative Example 2, molten particles splashed severely, the plate mesh was deformed, a uniform catalytic coating could not be obtained, and the appearance inspection failed.
[0074] Comparative Example 3
[0075] The only difference between this comparative example and Example 1 is that the collision deposition speed of the molten nickel droplet and the molten aluminum droplet is 300 m / s, and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.
[0076] The results show that compared with Example 1, in Comparative Example 3, the molten particles splashed severely, a uniform catalytic coating could not be obtained, and the appearance test failed.
[0077] Comparative Example 4
[0078] The only difference between this comparative example and Example 1 is that no pre-treatment laser heating device is used, that is, the electrode plate mesh is not heated before depositing the coating, and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.
[0079] The results showed that when the catalytic coating was folded 90° and kept in this form for more than 5 seconds, the coating fell off at the fold, and the exposed substrate accounted for 40%; after the coating was activated by 30wt% potassium hydroxide solution for 24h and ultrasonicated for 30min, the coating weight loss rate was 36%; the hydrogen evolution current was 100mA / cm 2 , hydrogen evolution overpotential is 0.36V.
[0080] Comparative Example 5
[0081] The only difference between this comparative example and Example 1 is that nickel powder and aluminum powder with an average particle size of 350 μm are used, and the other conditions (including structure, materials, parameters, etc.) are the same as those in Example 1.
[0082] The results showed that after the coating was activated with 30wt% potassium hydroxide solution for 24h and then subjected to ultrasound for 30min, the coating weight loss rate was 55%, which was a significant increase and the electrode stability was poor.
[0083] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a cathode plate mesh for electrolyzing water, characterized in that: include: Using the atmospheric plasma spraying method, molten nickel droplets and molten aluminum droplets are sprayed onto the surface of the heated electrode plate mesh to form a nickel-aluminum mixed coating; The nickel-aluminum mixed coating is heated to form a nickel-aluminum alloy.
2. The preparation method according to claim 1, characterized in that: The deposition rate of the melted nickel droplets and aluminum droplets is less than 150 m / s; Preferably, the deposition rate of the melted nickel droplets and aluminum droplets is 50 m / s-80 m / s.
3. The preparation method according to claim 2, characterized in that: Using nickel powder and aluminum powder as raw materials, melting them into the nickel molten droplets and the aluminum molten droplets, wherein the mass ratio of the nickel powder to the aluminum powder is 1:(0.2-0.3); Preferably, the particle size range of the nickel powder and the aluminum powder is 45 μm-78 μm; Preferably, the purity of the nickel powder and the aluminum powder is greater than 99.5%.
4. The preparation method according to claim 1, characterized in that: Using a pre-treatment laser heating system to heat the surface of the electrode plate mesh to 200° C.-300° C., and then spraying the nickel molten droplets and the aluminum molten droplets; Preferably, the surface of the electrode plate mesh is heated to 250° C.-280° C. by using the pre-treatment laser heating system; Preferably, the power of the pre-processing laser heating system is 1KW-2KW.
5. The preparation method according to claim 4, characterized in that: The nickel-aluminum mixed coating is heated to 500° C.-600° C. by using a post-processing laser, and the laser power of the post-processing laser is controlled to be 4KW-6KW.
6. The preparation method according to claim 5, characterized in that: The surface of the electrode plate mesh is heated by using a pre-processing laser heating head in a pre-processing laser heating system, and the nickel-aluminum mixed coating is heated by using a post-processing laser heating head; The pre-treatment laser heating head, the atmospheric plasma spray gun and the post-treatment laser heating head which are arranged in sequence are fixed on a movable slide rail, so that the pre-treatment laser heating head, the atmospheric plasma spray gun and the post-treatment laser heating head are linked with the same track and speed, and the post-treatment laser heating head irradiates the deposited nickel-aluminum mixed coating area, and controls the overall horizontal movement rate to be 500mm / s-1000mm / s; Preferably, the spacing of the atmospheric plasma spraying is 500mm-600mm; Preferably, the atmospheric plasma spray gun is controlled to move in a U-shaped deposition path, and when moving in the reverse direction, the pre-processing laser heating head and the post-processing laser heating head exchange roles and powers.
7. The preparation method according to claim 6, characterized in that: The light spots of the pre-treatment laser heating head and the post-treatment laser heating head are both square light spots, the nickel-aluminum mixed droplet area corresponding to the atmospheric plasma spray gun is circular, and the square light spots of the pre-treatment laser heating head and the post-treatment laser heating head are both tangent to the nickel-aluminum mixed droplet area; Preferably, the length of the square light spot is greater than the diameter of the nickel-aluminum mixed droplet zone, and the length of the square light spot is 40mm-60mm, the width is 40mm-60mm, and the diameter of the nickel-aluminum mixed droplet zone is 30mm-50mm.
8. The preparation method according to claim 1, characterized in that: Before depositing the coating, the electrode plate mesh is sequentially cleaned and sandblasted, and then a protective fixture is installed in the pores on the electrode plate mesh and the edge of the electrode plate mesh, and then dust removal, degreasing, cleaning and drying are sequentially performed; Preferably, the dried electrode plate mesh is fixed on a fixing table before coating deposition, so that the electrode plate mesh remains in a fixed position during the coating deposition process.
9. A cathode plate mesh for electrolyzing water, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 8.
10. An electrolysis device, characterized in that: It comprises the cathode plate mesh for electrolyzing water as described in claim 9.
Citation Information
Patent Citations
Preparation method of alkali type electrolytic water electrode
CN110846609A
Cathode for hydrogen production through alkaline water electrolysis and preparation method and application thereof
CN116288509A
Nickel coating catalyst, preparation method and application thereof
CN117822024A
Porous catalytic electrode and preparation method and application thereof
CN117966072A
Method for modifying and optimizing hydrogen evolution electrode, hydrogen evolution electrode and hydrogen production device
CN118064921A