Method for improving molecular weight of chinlon 6 carpet fiber

The cross-linking chain extension of nylon 6 fiber is carried out through the reductive amination method, which solves the problems of low fiber strength and uneven dyeing of the physical regeneration method, improves the molecular weight and wear resistance of the fiber, and realizes the production of high-quality regenerated fiber, which is suitable for for high-end textile products.

CN118756492AActive Publication Date: 2024-10-11WEIHAI HAIMA NOVEL FIBRE CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411034571.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-11
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

In the existing technology, nylon fibers prepared by physical regeneration methods have low strength and uneven dyeing, resulting in poor product quality and cannot be used for high-end fabric production, which in turn triggers the need for research on chemical regeneration methods.

Method used

The reductive amination method is adopted, through the reductive amination reaction between the amine groups at the end of the nylon 6 fiber molecular chain and glutaraldehyde, using benzyl alcohol as the reaction medium, combined with formic acid to adjust the pH value and the molar ratio of glutaraldehyde, to carry out cross-linking expansion. chains, increasing the molecular weight of the fiber.

Benefits of technology

It effectively increases the molecular weight of nylon 6 fiber, enhances its mechanical properties and wear resistance, improves dyeing uniformity, and provides higher quality regenerated fiber, which is suitable for high-end textile products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756492A_ABST
    Figure CN118756492A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving molecular weight of chinlon 6 carpet fibers, which comprises the following steps: S1, cleaning waste chinlon 6 carpet fibers, removing surface impurities, then airing the cleaned fibers, and finally crushing the dried fibers into fiber fragments with proper sizes; s2, an organic acid or inorganic acid solution with the concentration being 0.1%-1% is prepared, and the waste chinlon 6 carpet fibers are soaked in the acid solution. In a pre-swelling state of the fiber, when benzyl alcohol is used as a reaction medium, the ratio of the fiber to the benzyl alcohol is 1: 20, the pH value is adjusted to be about 5-6 by formic acid, and the molar ratio of the fiber to glutaraldehyde is 1: 5, a cross-linking reaction is performed for 1 hour at the temperature of 100 DEG C, so that a better chain extension effect is obtained. Crosslinking and chain extension of PA6 are realized through aldehyde-amine reaction so as to design and optimize a greener and more convenient molecular weight multiplication approach, a new idea is provided for recycling of polyamide fibers, and the idea of green development is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nylon, and in particular to a method for increasing the molecular weight of nylon 6 carpet fibers. Background Art

[0002] Polyamide (PA), commonly known as nylon, is a synthetic polymer material. Nylon is a synthetic fiber made from polyamide material by melt spinning, which has good mechanical properties and wear resistance. The recycling of waste nylon fiber has always been a widely concerned issue.

[0003] At present, there are two methods for preparing regenerated nylon fibers from waste polyamide materials: physical regeneration and chemical regeneration. The physical regeneration technology is basically mature. However, due to the disadvantages of low strength and uneven dyeing, the physical regenerated nylon fibers have poor product quality and can only be used to produce medium and low-end fabrics. Therefore, domestic and foreign manufacturers and experts and scholars have begun to turn to the research of chemical regenerated nylon fibers.

[0004] In response to the above problems, we have introduced a method to increase the molecular weight of nylon 6 carpet fiber. Summary of the invention

[0005] The invention discloses a method for increasing the molecular weight of nylon 6 carpet fibers, aiming to solve the technical problems in the background technology.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for increasing the molecular weight of nylon 6 carpet fiber comprises the following steps:

[0008] S1, cleaning the waste nylon 6 carpet fibers, removing surface impurities, and then drying the cleaned fibers. Finally, crushing the dried fibers into fiber fragments of appropriate sizes;

[0009] The step S1 can be refined as follows:

[0010] S11. Prepare an appropriate amount of clean water and detergent, soak the waste nylon 6 carpet fibers in the detergent solution, and stir evenly;

[0011] S12. Clean the fibers with a brush or mechanical equipment to ensure that all dirt and impurities are removed;

[0012] S13, placing the cleaned fibers in a dry area and drying them naturally or using a drying device;

[0013] S14. Use a pulverizer to pulverize the dried fibers to ensure that the fiber fragments are of moderate size for subsequent processing.

[0014] S2. Prepare an organic acid or inorganic acid solution with a concentration of 0.1%-1%, soak the waste nylon 6 carpet fiber in the acid solution, control the treatment temperature at 70-100°C, and soak for 30-60 minutes to ensure that the fiber is fully cationic;

[0015] The step S2 can be refined as follows:

[0016] S21. In the laboratory, accurately weigh organic or inorganic acids and prepare 0.1%-1% acid solutions;

[0017] S22, evenly distribute the waste nylon 6 carpet fibers in the acid solution to ensure that all fibers are in contact with the acid solution;

[0018] S23, heating the acid solution to 70-100° C. and maintaining the temperature for 30-60 minutes;

[0019] S24. Stir the solution regularly to ensure that the fibers are evenly cationized.

[0020] S3, preparing a benzyl alcohol and formic acid system solution, wherein the ratio of benzyl alcohol to formic acid is 1:10-20, and immersing the cationized fiber in the swelling solution, wherein the swelling treatment temperature is 50-100° C., and the treatment time is 1-1.5 hours;

[0021] The step S3 can be refined as follows:

[0022] S31. Accurately weigh benzyl alcohol and formic acid to prepare a solution in a ratio of 1:10-20;

[0023] S32, taking out the cationized fiber from the acid solution, and gently rinsing it with water to remove excess acid;

[0024] S33, placing the rinsed fiber into the prepared benzyl alcohol and formic acid solution, ensuring that the fiber is completely immersed;

[0025] S34, heating the swelling solution to 50-100°C and maintaining it at this temperature for 1-1.5 hours, stirring the solution regularly during this period.

[0026] S4, preparing a reaction medium solution, mainly benzyl alcohol, adding an appropriate amount of formic acid as a reducing agent to the reaction medium, and preparing a glutaraldehyde solution as a cross-linking chain extender;

[0027] The step S4 can be refined as follows:

[0028] S41, prepare benzyl alcohol and formic acid solution in proportion, and ensure that the solution is evenly mixed;

[0029] S42, accurately weighing glutaraldehyde and preparing a glutaraldehyde solution of a certain concentration;

[0030] S43, gradually adding the glutaraldehyde solution to the benzyl alcohol and formic acid solution, stirring evenly to ensure sufficient mixing;

[0031] S44. Ensure that the reaction medium solution remains uniform and stable before use.

[0032] S5, placing the swollen nylon 6 fiber in a reaction medium, and mixing it with the glutaraldehyde solution at a molar ratio of 1:1-1:8, controlling the reaction temperature at 100-120° C., and the reaction time at 1-3 hours;

[0033] The step S5 can be refined as follows:

[0034] S51, taking out the nylon 6 fiber after swelling treatment from the swelling solution, and gently removing excess solution;

[0035] S52, placing the fibers into the prepared reaction medium, ensuring that the fibers are evenly distributed;

[0036] S53, adding glutaraldehyde solution to the reaction medium in a molar ratio of 1:1-1:8, and stirring evenly;

[0037] S54, heating the reaction medium to 100-120°C, maintaining the reaction time for 1-3 hours, and periodically stirring the solution during the reaction to ensure that the reaction proceeds fully.

[0038] S6. After the reaction is completed, the fiber is taken out from the reaction solution, and the fiber is washed with pure water to remove the residual reactants and by-products, and then the washed fiber is dried;

[0039] The step S6 can be refined as follows:

[0040] S61, taking out the fiber after the reaction is completed from the reaction medium, and gently removing the excess solution;

[0041] S62, washing the fiber multiple times with a large amount of pure water to remove residual reactants and by-products;

[0042] S63, placing the washed fibers in a drying area to dry them naturally or using a drying device for drying;

[0043] S64. Check the dried fibers to ensure that there is no residual moisture and impurities.

[0044] S7. Test the molecular weight change of nylon 6 fiber before and after treatment, detect the mechanical properties of the fiber, including tensile strength and elongation at break, and check the abrasion resistance and dyeing uniformity of the fiber;

[0045] The step S7 can be refined as follows:

[0046] S71. Using gel permeation chromatography (GPC) or other appropriate methods to test the molecular weight change of the fiber before and after treatment;

[0047] S72, using a tensile testing machine to detect the tensile strength and elongation at break of the fiber;

[0048] S73, perform abrasion resistance test to evaluate the performance of the fiber under abrasion conditions;

[0049] S74. Carry out dyeing tests to check the dyeing uniformity and color fastness of the fibers.

[0050] S8. Use the treated nylon 6 fiber in textile production to verify its industrial feasibility, evaluate the performance of recycled nylon 6 fiber in different application fields, record and analyze the cost-effectiveness of the treatment process, and provide data support for large-scale production.

[0051] The step S8 can be refined as follows:

[0052] S81, sending the treated nylon 6 fiber to a textile factory for actual production test to observe the performance of the fiber in the textile process;

[0053] S82. Collect and analyze the application data of recycled nylon 6 fiber in different textile products;

[0054] S83. Evaluate the cost-effectiveness of the treatment process, including material cost, energy consumption and production efficiency;

[0055] S84. Based on the test data, make improvement suggestions and provide data support and process optimization solutions for large-scale production.

[0056] The method for increasing the molecular weight of nylon 6 carpet fiber provided by the present invention has the following advantages:

[0057] The present invention uses the reductive amination method as the reaction mechanism, and utilizes the reductive amination reaction of the amino group at the end of the molecular chain of nylon 6 fiber and glutaraldehyde to multiply and extend the molecular chain of the amorphous region of nylon 6 fiber, thereby increasing the molecular weight of the amorphous region of nylon 6 fiber. In the pre-swelling state of the fiber, benzyl alcohol is used as the reaction medium, the ratio of fiber to benzyl alcohol is 1:20, the pH value is adjusted to about 5-6 by formic acid, and the molar ratio of fiber to glutaraldehyde is 1:5. The cross-linking reaction is carried out at a temperature of 100°C for 1h to obtain a better chain extension effect. The cross-linking and chain extension of PA6 using aldehyde-amine reaction is intended to design and optimize a greener and more convenient molecular weight multiplication method, provide new ideas for the recycling and reuse of polyamide fibers, and conform to the concept of green development. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 The present invention provides a schematic diagram of the overall process of a method for increasing the molecular weight of nylon 6 carpet fibers.

[0059] Figure 2 This is a schematic flow chart of step S1 of a method for increasing the molecular weight of nylon 6 carpet fiber proposed in the present invention.

[0060] Figure 3 This is a schematic diagram of the process of step S2 of a method for increasing the molecular weight of nylon 6 carpet fiber proposed by the present invention.

[0061] Figure 4 This is a schematic diagram of the process of step S3 of a method for increasing the molecular weight of nylon 6 carpet fiber proposed by the present invention.

[0062] Figure 5 This is a schematic diagram of the process of step S4 of a method for increasing the molecular weight of nylon 6 carpet fiber proposed by the present invention.

[0063] Figure 6 This is a schematic diagram of the process of step S5 of a method for increasing the molecular weight of nylon 6 carpet fiber proposed by the present invention.

[0064] Figure 7 This is a schematic diagram of the process of step S6 of a method for increasing the molecular weight of nylon 6 carpet fiber proposed by the present invention.

[0065] Figure 8 This is a schematic diagram of the process of step S7 of a method for increasing the molecular weight of nylon 6 carpet fiber proposed by the present invention.

[0066] Fig. 9 This is a schematic diagram of the process of step S8 of a method for increasing the molecular weight of nylon 6 carpet fiber proposed by the present invention. DETAILED DESCRIPTION

[0067] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application usually described and marked in the drawings here can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present application provided in the drawings is not intended to limit the scope of the application claimed for protection, but merely represents the selected embodiments of the present application. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application.

[0068] The invention discloses a method for increasing the molecular weight of nylon 6 carpet fibers.

[0069] Reference Figure 1 , Figure 2 , Figure 3 , Figure 4 , Figure 5, Figure 6 , Figure 7 , Figure 8 and Fig. 9 As shown, a method for increasing the molecular weight of nylon 6 carpet fiber comprises the following steps:

[0070] S1, cleaning the waste nylon 6 carpet fibers, removing surface impurities, and then drying the cleaned fibers. Finally, crushing the dried fibers into fiber fragments of appropriate sizes;

[0071] The step S1 can be refined as follows:

[0072] S11. Prepare an appropriate amount of clean water and detergent, soak the waste nylon 6 carpet fibers in the detergent solution, and stir evenly;

[0073] S12. Clean the fibers with a brush or mechanical equipment to ensure that all dirt and impurities are removed;

[0074] S13, placing the cleaned fibers in a dry area and drying them naturally or using a drying device;

[0075] S14. Use a pulverizer to pulverize the dried fibers to ensure that the fiber fragments are of moderate size for subsequent processing.

[0076] The waste nylon 6 carpet fibers are cleaned and surface impurities are removed. The cleaned fibers are then dried and crushed into fiber fragments of appropriate size. The advantage of this process is that the detergent solution is first soaked and stirred to fully penetrate every corner of the fiber to ensure thorough cleaning. Mechanically assisted cleaning increases the cleaning intensity and further ensures the cleanliness of the fiber surface. Drying treatment quickly removes moisture from the fiber by natural drying or using drying equipment to prevent the fiber from deteriorating in a wet environment. The final crushing step processes the fiber into fragments of appropriate size, which is beneficial to subsequent processing steps and improves the efficiency of the overall process.

[0077] Soaking and stirring use the chemical action of detergents and the permeability of water to dissolve dirt; mechanical cleaning removes stubborn stains through physical friction; drying uses air flow or heat energy to evaporate water; crushing increases the specific surface area of ​​the fiber, thereby improving the penetration and reaction efficiency of subsequent treatment liquids.

[0078] S2. Prepare an organic acid or inorganic acid solution with a concentration of 0.1%-1%, soak the waste nylon 6 carpet fiber in the acid solution, control the treatment temperature at 70-100°C, and soak for 30-60 minutes to ensure that the fiber is fully cationic;

[0079] The step S2 can be refined as follows:

[0080] S21. In the laboratory, accurately weigh organic or inorganic acids and prepare 0.1%-1% acid solutions;

[0081] S22, evenly distribute the waste nylon 6 carpet fibers in the acid solution to ensure that all fibers are in contact with the acid solution;

[0082] S23, heating the acid solution to 70-100° C. and maintaining the temperature for 30-60 minutes;

[0083] S24. Stir the solution regularly to ensure that the fibers are evenly cationized.

[0084] Prepare an organic or inorganic acid solution with a concentration of 0.1%-1%, soak the waste nylon 6 carpet fiber in the acid solution, control the treatment temperature at 70-100℃, and soak for 30-60 minutes to ensure that the fiber is fully cationized. The advantage of this process is that by accurately weighing the acid solution, the accuracy of the solution concentration is guaranteed, thereby ensuring the consistency of the treatment effect. The fibers are evenly distributed in the acid solution so that each fiber can fully contact the acid solution to ensure the uniformity of the cationization treatment. Heating the acid solution to 70-100℃ and keeping it at this temperature for 30-60 minutes helps to accelerate the reaction and improve the treatment efficiency. Stir the solution regularly to ensure that the fibers are evenly heated and reacted during the treatment process, so as to achieve the best cationization effect.

[0085] The acid solution of accurate concentration is prepared to cationize the fiber through chemical reaction; the even distribution of fiber and heating of acid solution ensures sufficient contact and reaction rate between fiber and acid solution; regular stirring promotes uniform mixing of fiber and solution through mechanical force, thus improving the treatment effect.

[0086] S3, preparing a benzyl alcohol and formic acid system solution, wherein the ratio of benzyl alcohol to formic acid is 1:10-20, and immersing the cationized fiber in the swelling solution, wherein the swelling treatment temperature is 50-100° C., and the treatment time is 1-1.5 hours;

[0087] The step S3 can be refined as follows:

[0088] S31. Accurately weigh benzyl alcohol and formic acid to prepare a solution in a ratio of 1:10-20;

[0089] S32, taking out the cationized fiber from the acid solution, and gently rinsing it with water to remove excess acid;

[0090] S33, placing the rinsed fiber into the prepared benzyl alcohol and formic acid solution, ensuring that the fiber is completely immersed;

[0091] S34, heating the swelling solution to 50-100°C and maintaining it at this temperature for 1-1.5 hours, stirring the solution regularly during this period.

[0092] Prepare a benzyl alcohol and formic acid system solution, with a ratio of benzyl alcohol to formic acid of 1:10-20, and immerse the cationized fiber in the swelling solution. The swelling treatment temperature is 50-100°C and the treatment time is 1-1.5 hours. The advantage of this process is that by accurately weighing benzyl alcohol and formic acid, the accuracy of the solution ratio is ensured, thereby ensuring the consistency of the swelling effect. Take the cationized fiber out of the acid solution and gently rinse it with water to remove excess acid and ensure a pure environment for subsequent swelling treatment. Put the rinsed fiber into the prepared benzyl alcohol and formic acid solution to ensure that the fiber is completely immersed, which helps to fully contact the swelling agent with the fiber. Heat the swelling solution to 50-100°C and keep it at this temperature for 1-1.5 hours. Stir the solution regularly during this period to accelerate the swelling process and improve the treatment efficiency and effect.

[0093] Prepare a solution of benzyl alcohol and formic acid in an accurate ratio to effectively swell the fiber through its dissolution effect and chemical reaction; rinse the fiber to remove excess acid and prevent residual acid from interfering with the swelling process; heat the swelling solution and stir it regularly to ensure efficient and uniform swelling process by increasing the temperature and promoting uniform contact between the solution and the fiber.

[0094] S4, preparing a reaction medium solution, mainly benzyl alcohol, adding an appropriate amount of formic acid as a reducing agent to the reaction medium, and preparing a glutaraldehyde solution as a cross-linking chain extender;

[0095] The step S4 can be refined as follows:

[0096] S41, prepare benzyl alcohol and formic acid solution in proportion, and ensure that the solution is evenly mixed;

[0097] S42, accurately weighing glutaraldehyde and preparing a glutaraldehyde solution of a certain concentration;

[0098] S43, gradually adding the glutaraldehyde solution to the benzyl alcohol and formic acid solution, stirring evenly to ensure sufficient mixing;

[0099] S44. Ensure that the reaction medium solution remains uniform and stable before use.

[0100] Prepare reaction medium solution, mainly benzyl alcohol, add appropriate amount of formic acid as reducing agent in reaction medium, and prepare glutaraldehyde solution as cross-linking chain extender. The advantage of this process is that, by preparing benzyl alcohol and formic acid solution in proportion, it is ensured that solution mixes evenly, thereby ensuring the stability and consistency of reaction medium. Accurately weigh glutaraldehyde, and be mixed with glutaraldehyde solution of certain concentration, ensure the accuracy of reaction dosage, avoid inaccurate dosage and cause poor reaction effect. Glutaraldehyde solution is gradually added to benzyl alcohol and formic acid solution, and fully stirred, ensure that solution mixes evenly, improves the uniformity and reaction efficiency of reaction medium. Ensure that reaction medium solution keeps uniform and stable state before use, avoids precipitation or stratification, ensures the smooth progress of reaction.

[0101] The benzyl alcohol and formic acid solutions are prepared in proportion to provide a stable reaction environment through chemical reaction and dissolution; the glutaraldehyde solution is accurately weighed and prepared to ensure the accurate dosage of the cross-linking chain extender; the glutaraldehyde solution is gradually added and fully stirred to ensure that the reaction medium is evenly mixed and provide uniform reaction conditions; the solution is kept in a uniform and stable state to ensure the smooth progress of the reaction and the consistency of the reaction effect.

[0102] S5, placing the swollen nylon 6 fiber in a reaction medium, and mixing it with the glutaraldehyde solution at a molar ratio of 1:1-1:8, controlling the reaction temperature at 100-120° C., and the reaction time at 1-3 hours;

[0103] The step S5 can be refined as follows:

[0104] S51, taking out the nylon 6 fiber after swelling treatment from the swelling solution, and gently removing excess solution;

[0105] S52, placing the fibers into the prepared reaction medium, ensuring that the fibers are evenly distributed;

[0106] S53, adding glutaraldehyde solution to the reaction medium in a molar ratio of 1:1-1:8, and stirring evenly;

[0107] S54, heating the reaction medium to 100-120°C, maintaining the reaction time for 1-3 hours, and periodically stirring the solution during the reaction to ensure that the reaction proceeds fully.

[0108] The nylon 6 fiber after swelling treatment is placed in the reaction medium and mixed with glutaraldehyde solution at a molar ratio of 1:1-1:8, the reaction temperature is controlled at 100-120°C, and the reaction time is 1-3 hours. The advantage of this process is that the nylon 6 fiber after swelling treatment is taken out from the swelling solution, and the excess solution is gently removed to ensure that there is no excess solvent on the fiber surface to interfere with the subsequent reaction. The fiber is placed in the prepared reaction medium to ensure that the fiber is evenly distributed, which helps to fully contact the reaction medium with the fiber. Glutaraldehyde solution is added to the reaction medium at a molar ratio of 1:1-1:8 and stirred evenly to ensure uniform mixing and full reaction of glutaraldehyde and fiber. Heat the reaction medium to 100-120°C and maintain the reaction time for 1-3 hours. During this period, the solution is stirred regularly to ensure that the reaction is fully carried out, thereby improving the reaction efficiency and effect.

[0109] The nylon 6 fiber after swelling treatment is taken out from the swelling solution and the excess solution is removed, and the solvent interference is reduced by mechanical methods; the fiber is evenly distributed in the reaction medium to increase the contact area between the fiber and the reactant; the glutaraldehyde solution is added in molar ratio and stirred evenly, and the reaction dosage is controlled by chemical measurement; the reaction medium is heated and stirred regularly, and the reaction is promoted by heat energy and mechanical stirring to ensure the full progress and uniformity of the reaction.

[0110] S6. After the reaction is completed, the fiber is taken out from the reaction solution, and the fiber is washed with pure water to remove the residual reactants and by-products, and then the washed fiber is dried;

[0111] The step S6 can be refined as follows:

[0112] S61, taking out the fiber after the reaction is completed from the reaction medium, and gently removing the excess solution;

[0113] S62, washing the fiber multiple times with a large amount of pure water to remove residual reactants and by-products;

[0114] S63, placing the washed fibers in a drying area to dry them naturally or using a drying device for drying;

[0115] S64. Check the dried fibers to ensure that there is no residual moisture and impurities.

[0116] After the reaction is completed, the fiber is removed from the reaction solution, washed with pure water to remove residual reactants and by-products, and then the washed fiber is dried. The advantage of this process is that the fiber after the reaction is removed from the reaction medium and the excess solution is gently removed, which can reduce the interference of the excess solution on subsequent treatment. The fiber is washed multiple times with a large amount of pure water to ensure that the residual reactants and by-products are fully removed to ensure the purity of the fiber. The washed fiber is placed in a dry area and dried naturally or using a drying equipment to quickly remove moisture from the fiber and prevent the fiber from deteriorating in a humid environment. Check the dried fiber to ensure that there is no residual moisture and impurities to ensure the final quality of the fiber.

[0117] Remove the fiber from the reaction medium and remove excess solution, and reduce the residual solution by mechanical means; use a large amount of pure water to wash multiple times, and remove the residual reactants and by-products through dissolution and flushing; dry the fiber and evaporate the water through air flow or heat energy; check the dried fiber to ensure that there is no residual moisture and impurities to ensure the purity and quality of the fiber

[0118] S7. Test the molecular weight change of nylon 6 fiber before and after treatment, detect the mechanical properties of the fiber, including tensile strength and elongation at break, and check the abrasion resistance and dyeing uniformity of the fiber;

[0119] The step S7 can be refined as follows:

[0120] S71. Using gel permeation chromatography (GPC) or other appropriate methods to test the molecular weight change of the fiber before and after treatment;

[0121] S72, using a tensile testing machine to detect the tensile strength and elongation at break of the fiber;

[0122] S73, perform abrasion resistance test to evaluate the performance of the fiber under abrasion conditions;

[0123] S74. Carry out dyeing tests to check the dyeing uniformity and color fastness of the fibers.

[0124] The molecular weight change of nylon 6 fiber before and after treatment is tested, the mechanical properties of the fiber, including tensile strength and elongation at break, are tested, and the abrasion resistance and dyeing uniformity of the fiber are checked. The advantage of this process is that the molecular weight change of the fiber before and after treatment can be accurately evaluated by using gel permeation chromatography (GPC) or other appropriate methods to test the molecular weight change of the fiber and verify the treatment effect. The tensile strength and elongation at break of the fiber are tested using a tensile testing machine to quantify the mechanical properties of the fiber to ensure that it meets the requirements of use. Abrasion resistance tests are conducted to evaluate the performance of the fiber under wear conditions, which helps to understand the durability and application potential of the fiber. Dyeing tests are conducted to check the dyeing uniformity and color fastness of the fiber, which can evaluate the performance of the fiber in the dyeing process and ensure its quality in the final product.

[0125] Use GPC and other methods to test molecular weight changes, and reflect the treatment effect through changes in molecular weight distribution; use a tensile testing machine to test the mechanical properties of the fiber by applying tension; conduct abrasion resistance tests to evaluate the wear resistance of the fiber by simulating a wear environment; conduct dyeing tests to evaluate the dyeing performance and stability of the fiber through dyeing effect and color fastness tests

[0126] S8. Use the treated nylon 6 fiber in textile production to verify its industrial feasibility, evaluate the performance of recycled nylon 6 fiber in different application fields, record and analyze the cost-effectiveness of the treatment process, and provide data support for large-scale production.

[0127] The step S8 can be refined as follows:

[0128] S81, sending the treated nylon 6 fiber to a textile factory for actual production test to observe the performance of the fiber in the textile process;

[0129] S82. Collect and analyze the application data of recycled nylon 6 fiber in different textile products;

[0130] S83. Evaluate the cost-effectiveness of the treatment process, including material cost, energy consumption and production efficiency;

[0131] S84. Based on the test data, make improvement suggestions and provide data support and process optimization solutions for large-scale production.

[0132] The treated nylon 6 fiber is used in textile production to verify its industrial feasibility, evaluate the performance of recycled nylon 6 fiber in different application fields, record and analyze the cost-effectiveness of the treatment process, and provide data support for large-scale production. The advantage of this process is that the treated nylon 6 fiber is sent to the textile mill for actual production trials, so that the performance of the fiber in the textile process can be observed and its industrial feasibility can be verified. Collecting and analyzing the application data of recycled nylon 6 fiber in different textile products can evaluate the performance of the fiber in various application fields and ensure its applicability and quality. Evaluating the cost-effectiveness of the treatment process, including material cost, energy consumption and production efficiency, helps to understand the economy and sustainability of the treatment process. Based on the test data, improvement suggestions are put forward to provide data support and process optimization solutions for large-scale production, which can continuously optimize the process flow and improve production efficiency and product quality.

[0133] The fibers are sent to textile mills for actual production tests, and the textile properties of the fibers are verified through actual operations; application data are collected and analyzed, and the application effects of the fibers are evaluated through data analysis; the cost-effectiveness of the treatment process is evaluated, and the economic feasibility of the process is understood through calculation and comparison; improvement suggestions are made based on the test data, and the process flow is optimized through data-driven optimization to improve overall production efficiency.

[0134] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. The replacement may be a replacement of a part of the structure, device, method step, or a complete technical solution. Any equivalent replacement or change according to the technical solution and the inventive concept of the present invention shall be covered within the protection scope of the present invention.

Claims

1. A method for increasing the molecular weight of nylon 6 carpet fiber, characterized in that: The following steps are involved: S1, cleaning the waste nylon 6 carpet fibers, removing surface impurities, and then drying the cleaned fibers. Finally, crushing the dried fibers into fiber fragments of appropriate sizes; S2. Prepare an organic acid or inorganic acid solution with a concentration of 0.1%-1%, soak the waste nylon 6 carpet fiber in the acid solution, control the treatment temperature at 70-100°C, and soak for 30-60 minutes to ensure that the fiber is fully cationic; S3, preparing a benzyl alcohol and formic acid system solution, wherein the ratio of benzyl alcohol to formic acid is 1:10-20, and immersing the cationized fiber in the swelling solution, wherein the swelling treatment temperature is 50-100° C., and the treatment time is 1-1.5 hours; S4, preparing a reaction medium solution, mainly benzyl alcohol, adding an appropriate amount of formic acid as a reducing agent to the reaction medium, and preparing a glutaraldehyde solution as a cross-linking chain extender; S5, placing the swollen nylon 6 fiber in a reaction medium, and mixing it with the glutaraldehyde solution at a molar ratio of 1:1-1:8, controlling the reaction temperature at 100-120° C., and the reaction time at 1-3 hours; S6. After the reaction is completed, the fiber is taken out from the reaction solution, and the fiber is washed with pure water to remove the residual reactants and by-products, and then the washed fiber is dried; S7. Test the molecular weight change of nylon 6 fiber before and after treatment, detect the mechanical properties of the fiber, including tensile strength and elongation at break, and check the abrasion resistance and dyeing uniformity of the fiber; S8. Use the treated nylon 6 fiber in textile production to verify its industrial feasibility, evaluate the performance of recycled nylon 6 fiber in different application fields, record and analyze the cost-effectiveness of the treatment process, and provide data support for large-scale production.

2. The method for increasing the molecular weight of nylon 6 carpet fiber according to claim 1, characterized in that: The step S1 can be refined as follows: S11. Prepare an appropriate amount of clean water and detergent, soak the waste nylon 6 carpet fibers in the detergent solution, and stir evenly; S12. Clean the fibers with a brush or mechanical equipment to ensure that all dirt and impurities are removed; S13, placing the cleaned fibers in a dry area and drying them naturally or using a drying device; S14. Use a pulverizer to pulverize the dried fibers to ensure that the fiber fragments are of moderate size for subsequent processing.

3. The method for increasing the molecular weight of nylon 6 carpet fiber according to claim 1, characterized in that: The step S2 can be refined as follows: S21. In the laboratory, accurately weigh organic or inorganic acids and prepare 0.1%-1% acid solutions; S22, evenly distribute the waste nylon 6 carpet fibers in the acid solution to ensure that all fibers are in contact with the acid solution; S23, heating the acid solution to 70-100° C. and maintaining the temperature for 30-60 minutes; S24. Stir the solution regularly to ensure that the fibers are evenly cationized.

4. The method for increasing the molecular weight of nylon 6 carpet fiber according to claim 1, characterized in that: The step S3 can be refined as follows: S31. Accurately weigh benzyl alcohol and formic acid to prepare a solution in a ratio of 1:10-20; S32, taking out the cationized fiber from the acid solution, and gently rinsing it with water to remove excess acid; S33, placing the rinsed fiber into the prepared benzyl alcohol and formic acid solution, ensuring that the fiber is completely immersed; S34, heating the swelling solution to 50-100°C and maintaining it at this temperature for 1-1.5 hours, stirring the solution regularly during this period.

5. The method for increasing the molecular weight of nylon 6 carpet fiber according to claim 1, characterized in that: The step S4 can be refined as follows: S41, prepare benzyl alcohol and formic acid solution in proportion, and ensure that the solution is evenly mixed; S42, accurately weighing glutaraldehyde and preparing a glutaraldehyde solution of a certain concentration; S43, gradually adding the glutaraldehyde solution to the benzyl alcohol and formic acid solution, stirring evenly to ensure sufficient mixing; S44. Ensure that the reaction medium solution remains uniform and stable before use.

6. The method for increasing the molecular weight of nylon 6 carpet fiber according to claim 1, characterized in that: The step S5 can be refined as follows: S51, taking out the nylon 6 fiber after swelling treatment from the swelling solution, and gently removing excess solution; S52, placing the fibers into the prepared reaction medium, ensuring that the fibers are evenly distributed; S53, adding glutaraldehyde solution to the reaction medium in a molar ratio of 1:1-1:8, and stirring evenly; S54, heating the reaction medium to 100-120°C, maintaining the reaction time for 1-3 hours, and periodically stirring the solution during the reaction to ensure that the reaction proceeds fully.

7. The method for increasing the molecular weight of nylon 6 carpet fiber according to claim 1, characterized in that: The step S6 can be refined as follows: S61, taking out the fiber after the reaction is completed from the reaction medium, and gently removing the excess solution; S62, washing the fiber multiple times with a large amount of pure water to remove residual reactants and by-products; S63, placing the washed fibers in a drying area to dry them naturally or using a drying device for drying; S64. Check the dried fibers to ensure that there is no residual moisture and impurities.

8. The method for increasing the molecular weight of nylon 6 carpet fiber according to claim 1, characterized in that: The step S7 can be refined as follows: S71. Using gel permeation chromatography (GPC) or other appropriate methods to test the molecular weight change of the fiber before and after treatment; S72, using a tensile testing machine to detect the tensile strength and elongation at break of the fiber; S73, perform abrasion resistance test to evaluate the performance of the fiber under abrasion conditions; S74. Carry out dyeing tests to check the dyeing uniformity and color fastness of the fibers.

9. The method for increasing the molecular weight of nylon 6 carpet fiber according to claim 1, characterized in that: The step S8 can be refined as follows: S81, sending the treated nylon 6 fiber to a textile factory for actual production test to observe the performance of the fiber in the textile process; S82. Collect and analyze the application data of recycled nylon 6 fiber in different textile products; S83. Evaluate the cost-effectiveness of the treatment process, including material cost, energy consumption and production efficiency; S84. Based on the test data, make improvement suggestions and provide data support and process optimization solutions for large-scale production.

Citation Information

Patent Citations

  • Process of regenerating nylon 6 and nylon 66 from waste carpet by selective dissolving-precipitating method

    CN103642065A

  • Surface processing method of for nylon 66 fiber

    CN109183405A

  • Method for preparing cationic dye dyeable polyamide fibers

    CN113005795A

  • New process for synthesizing vonoprazan and application thereof

    CN117466867A

  • Individualized, crosslinked fibers and process for making said fibers

    EP0251676A2