Method for protecting rework of crystal bump of integrated circuit

By coating positive photoresist on the surface of the integrated circuit during the BumpRework process and using plasma bombardment and acetone to remove it, the problem of failing to effectively protect the IC circuit in the existing technology is solved, and the corrosion of the chemical solution is completely prevented and the efficiency is improved. Safety and reliability of heavy engineering processes.

CN118762992APending Publication Date: 2024-10-11ASE (KUNSHAN) INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410904970.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing BumpRework method fails to effectively protect the circuits and pads of the IC when removing integrated circuit bumps or pillars. As a result, if the operation time is too short or too long, it may cause corrosion of the circuit, resulting in the risk of IC failure or the entire wafer being scrapped. .

Method used

The IC circuit is protected by coating a positive photoresist on the wafer surface, removing the photoresist through plasma bombardment, using an etching solution to remove the bumps or pillars, and completely removing the photoresist with acetone to ensure the safety of the IC circuit. .

Benefits of technology

It completely prevents the corrosion of IC circuits and Pads by the chemical liquid during the rework process, improves the safety and reliability of the BumpRework process, and is suitable for all back-end bump packaging fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118762992A_ABST
    Figure CN118762992A_ABST
Patent Text Reader

Abstract

The invention discloses a method for protecting the rework of a crystal bump of an integrated circuit in the technical field of the rework of the crystal bump of the integrated circuit, and the method comprises the following specific steps: S1, coating a layer of positive photoresist on the surface of a wafer for protecting an IC line; s2, removing the photoresist on the surface of the bump or the cylinder through plasma bombardment; s3, the bumps or the cylinders are removed through the etching liquid, and the IC circuit is protected by the photoresist, so that damage of the etching liquid to the circuit can be completely avoided; s4, removing the metal barrier layer; and S5, removing the photoresist through acetone, wherein the acetone does not cause damage to the IC circuit. According to the reworking mode provided by the invention, the IC circuit and the Pad can be completely prevented from being corroded by the liquid medicine in the reworking process, the safety of reworking is ensured, and the method can be applied to all the subsequent bump packaging fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of integrated circuit crystal bump rework, and in particular relates to a method for protecting integrated circuit crystal bump rework. Background Art

[0002] In the semiconductor packaging process, after the bumping process is completed, the wafer may fail to function or fail to meet the yield standard of the integrated circuit (IC) due to improper process parameter settings, equipment failure or material problems. In this case, the bumps or pillars on the wafer need to be removed, and this process is called bump rework.

[0003] At present, the BumpRework method commonly used in the industry includes four steps:

[0004] First, the first layer of bumps or pillars are removed;

[0005] Secondly, confirm whether the first layer of bumps or pillars have been completely removed;

[0006] Then removing the second metal barrier layer;

[0007] Finally, confirm whether the second metal barrier layer is also completely removed.

[0008] Although this method is simple to operate, it does not protect the circuits and pads of the IC when removing the first layer of bumps or pillars. It is completely dependent on the protection ability of the liquid and the operator's skills and operation time. If the operation time is too short, the bumps or pillars may not be completely removed; if the time is too long, the risk of circuit corrosion may increase. Once the liquid corrodes the circuits and pads, it will cause the IC to fail, resulting in irreversible damage. Minor cases may cause partial IC failure, and serious cases may cause the entire wafer to be scrapped. Summary of the invention

[0009] In view of the shortcomings of the prior art, the present invention proposes a new method for protecting the bump rework of integrated circuit wafers to improve the safety and reliability of the bump rework process.

[0010] In order to achieve the above-mentioned purpose, the following technical solution is adopted: The present invention provides a method for protecting the rework of integrated circuit bumps, comprising the following specific steps:

[0011] S1: Coat a layer of positive photoresist on the surface of the wafer to protect the IC circuit;

[0012] S2: removing the photoresist on the surface of the bump or pillar by plasma bombardment;

[0013] S3: Etching solution is used to remove bumps or pillars. Because the IC circuit is protected by photoresist, it can completely avoid damage to the circuit by etching solution.

[0014] S4: removing the metal barrier layer;

[0015] S5: Photoresist is removed by acetone, which will not damage the IC circuit.

[0016] Furthermore, the thickness of the positive photoresist is 3-10 μm.

[0017] Furthermore, the etching amount in step S2 is controlled at 0.3 μm.

[0018] The beneficial effect of the present invention is that the rework method proposed by the present invention can completely prevent the chemical solution from corroding the IC circuit and the Pad during the rework process, ensure the safety of the rework, and can be applied to all back-end bump packaging fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram of a process of a bump on a metal barrier layer in a method for protecting an integrated circuit wafer bump rework of the present invention;

[0020] Figure 2 The present invention is a schematic flow chart of a method for protecting integrated circuit wafer bump rework with a column on a metal barrier layer.

[0021] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.

[0022] Legend: 1. IC; 2. IC circuit layer; 3. Pad; 4. Metal barrier layer; 5. Bump; 6. Photoresist; 7. Plasma bombardment; 8. Pillar. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0025] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0026] Example

[0027] According to the attached Figure 1-2 An embodiment of the present invention provides a method for protecting integrated circuit bump rework, comprising the following specific steps:

[0028] S1: coating positive photoresist:

[0029] Before applying photoresist, the wafer is first ultrasonically cleaned to remove surface particles and organic contaminants, and then chemically cleaned using oxidants and solvents to remove metal impurities and residues;

[0030] Select a positive photoresist that is suitable for the wafer material and subsequent process requirements. The photoresist must have good thermal stability and chemical resistance.

[0031] Use an automatic coating machine to evenly coat the photoresist, and control the thickness of the photoresist by adjusting the coating speed and pressure to ensure that the thickness consistency of the photoresist on the entire wafer surface is within the range of 3-10μm;

[0032] After coating, the wafer is placed in a heat treatment furnace for soft baking, controlling the appropriate temperature and time to remove the solvent and enhance the adhesion of the photoresist;

[0033] S2: Plasma bombardment to remove photoresist:

[0034] Select appropriate plasma gas (such as oxygen, argon, etc.) according to the characteristics of the photoresist, and set the plasma power, pressure and bombardment time;

[0035] Place the wafer into the plasma processing chamber, start the plasma equipment, and gradually remove the photoresist on the surface of the bump or column through plasma bombardment. At the same time, monitor the etching depth in real time to ensure that it does not exceed 0.3μm;

[0036] S3: Etching solution to remove bumps or pillars:

[0037] Select a solution that has a high etching rate for bump or pillar materials and a low etching rate for IC circuits and pad materials;

[0038] The wafer is immersed in an etching solution, and the etching temperature and etching time are determined according to the thickness of the bump or column and the etching rate of the solution;

[0039] After etching is completed, use a neutralizing solution to neutralize the remaining etching solution, and then rinse with deionized water several times to ensure that the residue is completely removed;

[0040] S4: Removal of metal barrier layer:

[0041] Removal of the metal barrier layer by physical or chemical methods;

[0042] If chemical methods are used, select chemical reagents that have a high dissolution rate for the metal barrier layer while ensuring safety for IC circuits and pad materials;

[0043] If mechanical methods are used, use precision grinding or polishing equipment, control the grinding force and speed to ensure that the metal barrier layer is removed evenly;

[0044] After removing the metal barrier layer, perform a thorough cleaning to remove all chemical reagents or abrasive particles, and inspect the surface using an optical microscope or scanning electron microscope to ensure there is no damage or residue;

[0045] S5: Removal of photoresist:

[0046] Immerse the wafer in acetone or clean it with acetone vapor to ensure that the photoresist is completely dissolved;

[0047] After cleaning, use nitrogen purge or dry in a vacuum drying oven to ensure that there is no acetone residue on the wafer surface;

[0048] After drying, the wafer undergoes a final inspection to ensure that the photoresist is completely removed and the surface is clean and free of damage.

[0049] Results Analysis

[0050] At present, the commonly used rework method includes four steps:

[0051] First, the first layer of bumps or pillars are removed;

[0052] Secondly, confirm whether the first layer of bumps or pillars have been completely removed;

[0053] Then removing the second metal barrier layer;

[0054] Finally, confirm whether the second metal barrier layer is also completely removed.

[0055] The above method is relatively simple and easy to operate, but the IC circuit and pad are not protected when removing the first layer of bumps or pillars. It depends entirely on the protection ability of the liquid itself to the circuit and the operator's operation method and time. A short time will cause the bumps or pillars to not be completely removed, and a long time will increase the risk of circuit corrosion. Therefore, this method has a certain probability of circuit corrosion risk.

[0056] The rework method proposed in the present invention can completely prevent the chemical solution from corroding the IC circuit and the Pad during the rework process, ensure the safety of the rework, and can be applied to all back-end bump packaging fields.

[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0058] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for protecting integrated circuit wafer bump rework, characterized in that: The specific steps include: S1: Coat a layer of positive photoresist on the surface of the wafer to protect the IC circuit; S2: removing the photoresist on the surface of the bump or pillar by plasma bombardment; S3: Etching solution is used to remove bumps or pillars. Because the IC circuit is protected by photoresist, it can completely avoid damage to the circuit by etching solution. S4: removing the metal barrier layer; S5: Photoresist is removed by acetone, which will not damage the IC circuit.

2. A method for protecting integrated circuit wafer bump rework according to claim 1, characterized in that: The thickness of the positive photoresist is 3-10 μm.

3. A method for protecting IC wafer bump rework according to claim 2, characterized in that: The etching amount in step S2 is controlled at 0.3 μm.

Citation Information

Patent Citations

  • Method for processing offset gold bump in driving display chip

    CN112309834A

  • Process for reworking gold bump wafer

    CN116072559A

  • High-reliability reworking process for gold bump wafer

    CN116153794A

  • High yield and ultra-fine pitch large package for large integrated circuits or large advanced integrated circuits