Interface layer, composite flame-retardant diaphragm and battery

By using a composite flame-retardant separator structure containing fluorine organic matter, toughening agent, aramid and solid electrolyte in the lithium battery separator, the problems of poor flame retardant effect and low conductivity in the existing technology are solved, and a higher Flame retardant performance and conductive efficiency extend the cycle life of the battery.

CN118763359APending Publication Date: 2024-10-11SHENZHEN INX ENERGY TECHNOLOGY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410994792.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing lithium battery separator has poor flame retardant effect and low conductivity, which affects the overall performance of the battery.

Method used

It adopts a composite flame-retardant separator structure, including a base film, an interface layer and a flame-retardant layer. The base film is composed of fluorine-containing organic matter and toughening agent. Aramid and solid electrolyte are added to the interface layer and flame-retardant layer to form a network structure to improve Mechanical properties and conductive efficiency.

Benefits of technology

It significantly improves the flame retardant performance and conductivity, enhances the mechanical strength and cycle life of the battery, and reduces the internal resistance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763359A_ABST
    Figure CN118763359A_ABST
Patent Text Reader

Abstract

The invention discloses a composite flame-retardant diaphragm and a preparation method and application thereof.The composite flame-retardant diaphragm comprises a base film, an interface layer and a flame-retardant layer, the interface layer is located between the base film and the flame-retardant layer, the base film is made of fluorine-containing organic matter and a flexibilizer, the flame-retardant layer is made of aramid fiber, the interface layer is made of fluorine-containing organic matter, a flexibilizer and aramid fiber, and the flame-retardant layer is made of aramid fiber. The interface layer has a network structure. The fluorine-containing organic matter is used as a film-forming main body material, the flame-retardant effect is good, the flexibilizer is added into the fluorine-containing organic matter, namely, a framework is formed in a base film, the strength is improved, the mechanical performance of the diaphragm is further improved by adding the aramid fiber, the aramid fiber can be rapidly carbonized and thickened when encountering high temperature, a heat insulation barrier is formed, and the high temperature is isolated; the flame retardance is further improved; the fluorine-containing organic matter has higher polarity and higher dielectric constant, the lyophilic property of the composite flame-retardant diaphragm is improved, ionization of lithium salt is facilitated, the conductive efficiency is improved, and the base film and the flame-retardant layer are firmly connected through the net structure.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The application number of the original application is: 202410448925.6, the application date is April 15, 2024, and the name of the invention is: A composite flame-retardant diaphragm and its preparation method and application. Technical Field

[0002] The present application relates to the field of battery technology, and in particular to a composite flame-retardant diaphragm, a method for preparing the composite flame-retardant diaphragm, and a lithium-ion battery. Background Art

[0003] Lithium batteries include four major materials: positive electrode, negative electrode, diaphragm and electrolyte. In the structure of lithium batteries, the diaphragm is one of the key inner components. The diaphragm is mainly a polyolefin diaphragm made of polyethylene and polypropylene. The performance of the diaphragm determines the interface structure and internal resistance of the battery, and directly affects the battery's capacity, cycle and safety performance. A diaphragm with excellent performance plays an important role in improving the overall performance of the battery.

[0004] The current flame retardant technology mainly relies on flame retardants. A flame retardant layer is coated on the surface of the base film. The flame retardant layer is mainly composed of flame retardants and binders, but its flame retardant effect is not good. The addition of a large amount of flame retardants will reduce the conductivity of the diaphragm, hinder the transmission of lithium ions, and affect the overall performance of the battery. Summary of the invention

[0005] In view of this, the present application provides a composite flame-retardant diaphragm, aiming to improve the problems of poor flame-retardant effect and poor conductivity of the existing flame-retardant diaphragm.

[0006] The embodiment of the present application is implemented as follows: a composite flame retardant diaphragm, comprising:

[0007] A base film, an interface layer and a flame retardant layer, wherein the interface layer is located between the base film and the flame retardant layer, the material of the base film includes a fluorine-containing organic substance and a toughening agent, the material of the flame retardant layer includes aramid, the material of the interface layer includes the fluorine-containing organic substance, the toughening agent and the aramid, and the interface layer has a mesh structure.

[0008] Optionally, the fluorine-containing organic compound includes one or more of polyvinylidene fluoride, polyvinylidene fluoride-hydrofluoric acid copolymer, polyvinylidene fluoride-trifluoroethylene copolymer; and / or

[0009] The toughening agent includes one or more of silicon carbide whiskers, silicon nitride whiskers, glass fibers, and polymethyl methacrylate; and / or

[0010] The aramid fiber includes at least one of meta-aramid fiber and para-aramid fiber.

[0011] Optionally, in some embodiments of the present application, the flame retardant layer further includes a solid electrolyte, and the solid electrolyte includes one or more of LATP, doped or undoped LLZO.

[0012] Optionally, in some embodiments of the present application, in the base film, the mass ratio of the fluorine-containing organic compound to the toughening agent is (0.6-0.9):(0.01-0.5); and / or

[0013] In the flame retardant layer, the mass ratio of the solid electrolyte to the aramid fiber is (1-10):1; and / or

[0014] The general formula of the doped LLZO is Li 7-x La 3 Zr 2-x M x O 12 , wherein 0.25≤x<2, the doping element M includes one or more of Ta, Ga, Al, and Nb; the doped LLZO includes Li 6.7 La 3 Zr 1.7 Ta 0.3 O 12 , Li 6.5 La 3 Zr 1.5 Ga 0.5 O 12 , Li 6.2 La 3 Zr 1.2 Al 0.8 O 12 , Li 6 La 3 ZrNbO 12 , Li 5.8 La 3 Zr 0.8 Ta 1.2 O 12 , Li 5.5 La 3 Zr 0.5 Nb 1.5 O 12 , Li 5.4 La 3 Zr 0.4 Ga 1.6 O 12 , Li 5.2 La 3 Zr 0.2 Ta 1.8 O 12 , Li 5.1 La 3 Zr 0.1 Nb1.9 O 12 , Li 6.75 La 3 Zr 1.75 Nb 0.25 O 12、 Li 5.8 La 3 Zr 1.4 Ta 0.6 Al 0.2 O 12 One or more of .

[0015] Optionally, in some embodiments of the present application, the thickness of the composite flame retardant membrane is 8 to 24 μm; and / or

[0016] The thickness of the base film is 7 to 19 μm; and / or

[0017] The thickness of the interface layer is 100-200 nm; and / or

[0018] The thickness of the flame retardant layer is 1-4 μm.

[0019] Accordingly, the present application also provides a method for preparing a composite flame-retardant diaphragm, comprising:

[0020] Providing a prefabricated base film, wherein the material of the prefabricated base film includes a fluorine-containing organic compound and a toughening agent;

[0021] Providing a second mixed liquid, wherein the second mixed liquid includes aramid fiber;

[0022] The second mixed liquid is set on the prefabricated base film, wherein part of the second mixed liquid penetrates into the upper surface of the prefabricated base film to form a base film and an interface layer combined with the base film; the second mixed liquid that has not penetrated into the prefabricated base film forms a flame retardant layer on the interface layer to obtain a composite flame retardant diaphragm.

[0023] Optionally, in some embodiments of the present application, the method for preparing the prefabricated base film includes:

[0024] Providing a first mixed liquid, wherein the first mixed liquid includes a fluorine-containing organic compound, a toughening agent and a first solvent;

[0025] A substrate is provided, and the first mixed liquid is disposed on the substrate to obtain a prefabricated base film.

[0026] Optionally, in some embodiments of the present application, the second mixed liquid further includes a solid electrolyte, a dispersant and a second solvent.

[0027] Optionally, in some embodiments of the present application, the first solvent and the second solvent independently include one or more of N-methylpyrrolidone, dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, acetone, dichloroethane, chloroform, ethanol, isopropanol, and toluene; and / or

[0028] The dispersant comprises one or more of polyacrylamide, polyvinyl pyrrolidone, carboxymethyl cellulose and acrylic resin; and / or

[0029] The fluorine-containing organic compound includes one or more of polyvinylidene fluoride, polyvinylidene fluoride-hydrofluoric acid copolymer, polyvinylidene fluoride-trifluoroethylene copolymer; and / or

[0030] The toughening agent includes one or more of silicon carbide whiskers, silicon nitride whiskers, glass fibers, and polymethyl methacrylate; and / or

[0031] The solid electrolyte comprises one or more of LATP, doped or undoped LLZO, wherein the doping element in the doped LLZO comprises one or more of tantalum, gallium, aluminum, and niobium; and / or

[0032] The aramid fiber includes at least one of meta-aramid fiber and para-aramid fiber.

[0033] Optionally, in some embodiments of the present application, the mass ratio of the fluorine-containing organic compound to the toughening agent is (0.6-0.9):(0.01-0.5); and / or

[0034] In the first mixed solution, the mass concentration of the fluorine-containing organic matter is 89.9-134.8 mg / mL; and / or

[0035] The mass ratio of the solid electrolyte to the aramid fiber is (1-10):1; and / or

[0036] The mass ratio of the dispersant to the second solvent is 1:(200-1000); and / or

[0037] In the second mixed solution, the mass concentration of the solid electrolyte is 17.236-237 mg / mL.

[0038] Optionally, in some embodiments of the present application, the method of disposing the first mixed liquid on the substrate includes a first coating; and / or

[0039] After the first mixed solution is disposed on the substrate, the method further comprises first phase conversion and drying to obtain a prefabricated base film; and / or

[0040] The method for providing the second mixed solution comprises adding the solid electrolyte and the dispersant into the second solvent for dispersion, and then adding the aramid fiber and continuing to stir; and / or

[0041] The method of disposing the second mixed liquid on the prefabricated base film comprises a second coating; and / or

[0042] After the second mixed liquid is disposed on the prefabricated base film, the method further includes a second phase conversion and drying.

[0043] Optionally, in some embodiments of the present application, the temperatures of the drying and the baking are independently 40 to 80° C.; and / or

[0044] The drying time and the drying time are each independently 1 to 300 minutes; and / or

[0045] The dispersion includes dispersion at a speed of n1 for a time of t1; and / or

[0046] The stirring comprises stirring at a speed of n2 for a time of t2; and / or

[0047] The first coating and the second coating independently include one or more of spin coating, spray coating, wire rod coating, and dip coating.

[0048] Optionally, in some embodiments of the present application, the n1 and the n2 are each independently 500-3000 r / min; and / or

[0049] The t1 and the t2 are each independently 1 to 6 hours.

[0050] Correspondingly, an embodiment of the present application further provides a battery, which includes the above-mentioned composite flame-retardant diaphragm or the composite flame-retardant diaphragm prepared by the preparation method of the above-mentioned composite flame-retardant diaphragm.

[0051] In the technical solution of this application:

[0052] The Chinese name of PVDF is polyvinylidene fluoride; the Chinese name of PVDF-HFP is polyvinylidene fluoride-hydrofluoric acid copolymer; the Chinese name of PVDF-TrFE is polyvinylidene fluoride-trifluoroethylene copolymer; the Chinese name of PMMA is polymethyl methacrylate; the Chinese name of NMP is N-methylpyrrolidone; the Chinese name of DMAc is dimethylacetamide; the Chinese name of DMF is N,N-dimethylformamide; the Chinese name of DMSO is dimethyl sulfoxide; LATP stands for lithium aluminum titanium phosphate; LLZO stands for lithium lanthanum zirconium oxide.

[0053] In the composite flame-retardant diaphragm provided by the present application, the base film uses fluorine-containing organic matter as the main film-forming material, which has good flame-retardant effect itself. Adding toughening agent to the fluorine-containing organic matter is equivalent to forming a skeleton in the base film, which improves the strength of the base film and the tape running rate, thereby further improving the production efficiency. Adding aramid further improves the mechanical properties of the composite flame-retardant diaphragm. Aramid will quickly carbonize and thicken when encountering high temperature to form an insulating barrier to isolate high temperature and further improve the flame retardant performance. Fluorine-containing organic matter has stronger polarity and higher dielectric constant, which improves the lyophilicity of the composite flame-retardant diaphragm and helps the ionization of lithium salts, thereby improving the conductivity. A mesh structure is formed between the base film and the flame-retardant layer to firmly connect the base film and the flame-retardant layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0055] Figure 1 is a SEM image of the composite flame retardant diaphragm prepared in Example 1 of the present application;

[0056] Figure 2 This is a flow chart of a method for preparing a composite flame-retardant diaphragm provided in an embodiment of the present application;

[0057] Figure 3 is another SEM image of the composite flame-retardant diaphragm prepared in Example 1 of the present application;

[0058] Description of reference numerals:

[0059] Base film 10 ; flame retardant layer 20 ; interface layer 30 . DETAILED DESCRIPTION

[0060] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0061] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0062] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0063] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or several", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0064] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0065] The technical solution of this application is as follows:

[0066] In a first aspect, an embodiment of the present application provides a composite flame-retardant diaphragm, comprising:

[0067] A base film 10, an interface layer 30 and a flame retardant layer 20, wherein the interface layer 30 is located between the base film 10 and the flame retardant layer 20, the material of the base film 10 includes fluorine-containing organic matter and a toughening agent, the material of the flame retardant layer 20 includes aramid, the material of the interface layer 30 includes the fluorine-containing organic matter, the toughening agent and the aramid, and the interface layer 30 is a mesh structure.

[0068] In the embodiment of the present application, the base film 10 uses fluorine-containing organic matter as the main film-forming material, which has good flame retardant effect. Adding a toughening agent to the fluorine-containing organic matter is equivalent to forming a skeleton in the base film 10, thereby improving the strength of the base film 10 and increasing the tape running rate, thereby further improving the production efficiency. The addition of aramid further improves the mechanical properties of the composite flame retardant diaphragm. When aramid encounters high temperature, it will quickly carbonize and thicken to form an insulating barrier, isolate high temperature, and further improve the flame retardant performance; fluorine-containing organic matter has a stronger polarity and a higher dielectric constant, which improves the lyophilicity of the composite flame retardant diaphragm and helps the ionization of lithium salts, thereby improving the conductivity efficiency. The network structure formed by the fluorine organic matter, toughening agent and aramid makes the base film 10 firmly connected to the flame retardant layer 20.

[0069] In some embodiments, in the base film 10, the mass ratio of the fluorine-containing organic compound to the toughening agent is (0.6-0.9):(0.01-0.5), for example, it can be 0.6:0.01, 0.6:0.02, 0.6:0.05, 0.6:0.08, 0.6:0.1, 0.6:0.12, 0.6:0.14, 0.6:0.16, 0.6:0.18, 0.6 :0.2, 0.6:0.22, 0.6:0.24, 0.6:0.26, 0.6:0.28, 0.6:0.3, 0.6:0.32, 0.6:0.35, 0.6:0.38, 0.6:0.4, 0.6:0.42, 0.6:0.46, 0.6:0.48, 0.6:0.5, 0.7:0.01, 0.7:0.05, 0.7:0.1 , 0.7:0.15, 0.7:0.2, 0.7:0.25, 0.7:0.3, 0.7:0.35, 0.7:0.4, 0.7:0.45, 0.7:0.5, 0.8:0.01, 0.8:0.05, 0.8:0.1, 0.8:0.15, 0.8:0.2, 0.8:0.25, 0.8:0.3, 0.8:0.35, 0.8:0. 4. 0.8:0.45, 0.8:0.5, 0.9:0.01, 0.9:0.05, 0.9:0.1, 0.9:0.15, 0.9:0.2, 0.9:0.25, 0.9:0.3, 0.9:0.35, 0.9:0.4, 0.9:0.45, 0.9:0.5, etc., within the mass ratio range, it is beneficial to form a base film 10 with excellent flame retardant properties and strength.

[0070] In some embodiments, the fluorine-containing organic compound includes one or more of polyvinylidene fluoride, polyvinylidene fluoride-hydrofluoric acid copolymer, and polyvinylidene fluoride-trifluoroethylene copolymer.

[0071] In some embodiments, the toughening agent includes one or more of silicon carbide whiskers, silicon nitride whiskers, glass fibers, and PMMA.

[0072] In some embodiments, the aramid includes at least one of meta-aramid and para-aramid.

[0073] In some embodiments, the flame retardant layer 20 further includes a solid electrolyte.

[0074] Furthermore, the solid electrolyte includes one or more of LATP, doped or undoped LLZO.

[0075] Furthermore, the general formula of the doped LLZO is Li 7-x La 3 Zr 2-x M x O 12 , wherein 0.25≤x<2, and the doping element M includes one or more of tantalum (Ta), gallium (Ga), aluminum (Al), and niobium (Nb).

[0076] For example, the doped LLZO includes Li 6.7 La 3 Zr 1.7 Ta 0.3 O 12 , Li 6.5 La 3 Zr 1.5 Ga 0.5 O 12 , Li 6.2 La 3 Zr 1.2 Al 0.8 O 12 , Li 6 La 3 ZrNbO 12 , Li 5.8 La 3 Zr 0.8 Ta 1.2 O 12 , Li 5.5 La 3 Zr 0.5 Nb 1.5 O 12 , Li 5.4 La 3 Zr 0.4 Ga 1.6 O 12 , Li 5.2 La 3 Zr 0.2 Ta 1.8 O 12 , Li5.1 La 3 Zr 0.1 Nb 1.9 O 12 , Li 6.75 La 3 Zr 1.75 Nb 0.25 O 12、 Li 5.8 La 3 Zr 1.4 Ta 0.6 Al 0.2 O 12 One or more of .

[0077] In some embodiments, in the flame retardant layer 20, the mass ratio of the solid electrolyte to the aramid is (1-10):1, for example, it can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc. Within the mass ratio range, it is beneficial to improve the high temperature resistance, mechanical strength and conductivity of the composite flame retardant diaphragm.

[0078] In some embodiments, the thickness of the composite flame retardant membrane is 8 to 24 μm, for example, it can be 8 μm, 8.1 μm, 8.5 μm, 9 μm, 10 μm, 11 μm, 12 μm, 14 μm, 15 μm, 16 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 23.2 μm, 23.5 μm, 24 μm, etc. Within the thickness range, it is beneficial to improve the mechanical strength of the composite flame retardant membrane and has excellent conductive properties.

[0079] In some embodiments, the base film 10 has a thickness of 7 to 19 μm, for example, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, etc.

[0080] In some embodiments, the thickness of the interface layer 30 is 100-200 nm, for example, it can be 100 nm, 105 nm, 110 nm, 115 nm, 120 nm, 125 nm, 130 nm, 135 nm, 140 nm, 145 nm, 150 nm, 155 nm, 160 nm, 165 nm, 170 nm, 175 nm, 180 nm, 185 nm, 190 nm, 195 nm, 200 nm, etc.

[0081] In some embodiments, the thickness of the flame retardant layer 20 is 1 to 4 μm, for example, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm, 2.2 μm, 2.5 μm, 2.8 μm, 3 μm, 3.2 μm, 3.4 μm, 3.5 μm, 3.6 μm, 3.8 μm, 4 μm, etc.

[0082] Second, see Figure 2 The present application also provides a method for preparing a composite flame-retardant diaphragm, comprising:

[0083] S01, providing a prefabricated base film 10, wherein the material of the prefabricated base film 10 includes a fluorine-containing organic compound and a toughening agent;

[0084] S02, providing a second mixed liquid, wherein the second mixed liquid includes aramid fiber;

[0085] S03. The second mixed liquid is set on the prefabricated base film 10, wherein a part of the second mixed liquid penetrates into the upper surface of the prefabricated base film 10 to form the base film 10 and an interface layer 30 combined with the base film 10; the second mixed liquid that has not penetrated into the prefabricated base film 10 forms a flame retardant layer 20 on the interface layer 30 to obtain a composite flame retardant diaphragm.

[0086] In the S01:

[0087] The preparation method of the prefabricated base film 10 includes:

[0088] S011, providing a first mixed liquid, wherein the first mixed liquid includes a fluorine-containing organic compound, a toughening agent and a first solvent;

[0089] S012, providing a substrate, and placing the first mixed liquid on the substrate to obtain a prefabricated base film 10.

[0090] In some embodiments, the first solvent includes one or more of N-methylpyrrolidone, dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, acetone, ethylene dichloride, chloroform, ethanol, isopropanol, and toluene.

[0091] In some embodiments, the fluorine-containing organic compound includes one or more of polyvinylidene fluoride, polyvinylidene fluoride-hydrofluoric acid copolymer, and polyvinylidene fluoride-trifluoroethylene copolymer.

[0092] In some embodiments, the toughening agent includes one or more of silicon carbide whiskers, silicon nitride whiskers, glass fibers, and PMMA.

[0093] In some embodiments, the mass ratio of the fluorinated organic compound to the toughening agent is (0.6-0.9):(0.01-0.5), for example, 0.6:0.01, 0.6:0.02, 0.6:0.05, 0.6:0.08, 0.6:0.1, 0.6:0.12, 0.6:0.14, 0.6:0.16, 0.6:0.18, 0.6:0.2, 0.6:0. 0.22, 0.6:0.24, 0.6:0.26, 0.6:0.28, 0.6:0.3, 0.6:0.32, 0.6:0.35, 0.6:0.38, 0.6:0.4, 0.6:0.42, 0.6:0.46, 0.6:0.48, 0.6:0.5, 0.7:0.01, 0.7:0.05, 0.7:0.1, 0.7:0 .15, 0.7:0.2, 0.7:0.25, 0.7:0.3, 0.7:0.35, 0.7:0.4, 0.7:0.45, 0.7:0.5, 0.8:0.01, 0.8:0.05, 0.8:0.1, 0.8:0.15, 0.8:0.2, 0.8:0.25, 0.8:0.3, 0.8:0.35, 0.8:0.4, 0 .8:0.45, 0.8:0.5, 0.9:0.01, 0.9:0.05, 0.9:0.1, 0.9:0.15, 0.9:0.2, 0.9:0.25, 0.9:0.3, 0.9:0.35, 0.9:0.4, 0.9:0.45, 0.9:0.5, etc., within the mass ratio range, it is conducive to forming a base film 10 with excellent flame retardant properties and strength.

[0094] Further, in the first mixed solution, the mass concentration of the fluorine-containing organic matter is 89.9-134.8 mg / mL, for example, it can be 89.8 mg / mL, 90 mg / mL, 92 mg / mL, 95 mg / mL, 98 mg / mL, 100 mg / mL, 102 mg / mL, 105 mg / mL, 108 mg / mL, 110 mg / mL, 112 mg / mL, 115 mg / mL, 118 mg / mL, 120 mg / mL, 122 mg / mL, 124 mg / mL, 126 mg / mL, 128 mg / mL, 130 mg / mL, 132 mg / mL, 134 mg / mL, 134.8 mg / mL, etc. Within the mass concentration range, it is beneficial to fully dissolve the fluorine-containing organic matter.

[0095] In said S012:

[0096] In some embodiments, the method of disposing the first mixed solution on a substrate includes a first coating.

[0097] Furthermore, the first coating method includes one or more of spin coating, spray coating, wire rod coating, and dip coating.

[0098] In some embodiments, after the first mixed solution is disposed on the substrate, a first phase conversion and drying are further performed to obtain the base film 10 .

[0099] In some embodiments, the substrate includes a release film or a glass substrate.

[0100] In some embodiments, after the first mixed liquid is disposed on the substrate, a first phase conversion is further performed, and drying is performed to obtain the prefabricated base film 10 .

[0101] Furthermore, the drying temperature is 40-80°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C, etc., and the drying time is 1-300min, for example, 1min, 10min, 50min, 60min, 80min, 100min, 120min, 150min, 180min, 200min, 220min, 250min, 280min, 300min, etc. Within the temperature and time range, it is beneficial to dry the first mixed liquid after the first phase conversion and obtain the prefabricated base film 10.

[0102] It can be understood that the first phase inversion is a conventional technique in the art, and its purpose is to remove the solvent to quickly form a film and create pores.

[0103] It can be understood that after the first phase transition, the film falls off from the substrate and is then dried to obtain the prefabricated base film 10 .

[0104] In the S02:

[0105] In some embodiments, the second mixed liquid further includes a solid electrolyte, a dispersant, and a second solvent.

[0106] In some embodiments, the solid electrolyte includes one or more of LATP, doped or undoped LLZO.

[0107] Furthermore, the general formula of the doped LLZO is Li 7-x La 3 Zr 2-x M x O 12 , wherein 0.25≤x<2, and the doping element M includes one or more of tantalum (Ta), gallium (Ga), aluminum (Al), and niobium (Nb).

[0108] Furthermore, the doped LLZO includes Li 6.7 La 3 Zr 1.7 Ta 0.3 O12 , Li 6.5 La 3 Zr 1.5 Ga 0.5 O 12 , Li 6.2 La 3 Zr 1.2 Al 0.8 O 12 , Li 6 La 3 ZrNbO 12 , Li 5.8 La 3 Zr 0.8 Ta 1.2 O 12 , Li 5.5 La 3 Zr 0.5 Nb 1.5 O 12 , Li 5.4 La 3 Zr 0.4 Ga 1.6 O 12 , Li 5.2 La 3 Zr 0.2 Ta 1.8 O 12 , Li 5.1 La 3 Zr 0.1 Nb 1.9 O 12 , Li 6.75 La 3 Zr 1.75 Nb 0.25 O 12、 Li 5.8 La 3 Zr 1.4 Ta 0.6 Al 0.2 O 12 wait.

[0109] The dispersant includes one or more of polyacrylamide, polyvinyl pyrrolidone, carboxymethyl cellulose and acrylic resin.

[0110] In some embodiments, the second solvent includes one or more of N-methylpyrrolidone, dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, acetone, ethylene dichloride, chloroform, ethanol, isopropanol, and toluene.

[0111] In some embodiments, the aramid includes at least one of meta-aramid and para-aramid.

[0112] In some embodiments, the mass ratio of the solid electrolyte to the aramid is (1-10):1, for example, it can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc. Within the mass ratio range, it is beneficial to improve the high temperature resistance, mechanical strength and conductivity of the composite flame retardant diaphragm.

[0113] In some embodiments, the mass ratio of the dispersant to the second solvent is 1:(200-1000), for example, it can be 1:200, 1:250, 1:300, 1:350, 1:400, 1:450, 1:500, 1:550, 1:600, 1:650, 1:700, 1:750, 1:800, 1:850, 1:900, 1:950, 1:1000, etc.

[0114] Further, in the second mixed solution, the mass concentration of the solid electrolyte is 17.236-237 mg / mL, for example, 17.236 mg / mL, 18 mg / mL, 20 mg / mL, 50 mg / mL, 80 mg / mL, 100 mg / mL, 110 mg / mL, 130 mg / mL, 150 mg / mL, 180 mg / mL, 200 mg / mL, 210 mg / mL, 220 mg / mL, 230 mg / mL, 235 mg / mL, 237 mg / mL, etc. Within the mass concentration range, it is beneficial to fully dissolve the solid electrolyte.

[0115] Furthermore, the method for providing the second mixed solution includes adding the solid electrolyte and the dispersant into the second solvent for dispersion, and then adding the aramid and continuing to stir.

[0116] In some embodiments, the dispersing includes dispersing for a time t1 at a rotation speed n1.

[0117] In some embodiments, the stirring includes stirring at a speed of n2 for a time of t2.

[0118] Furthermore, n1 is 500-3000 r / min, for example, it can be 500 r / min, 550 r / min, 580 r / min, 1000 r / min, 1100 r / min, 1200 r / min, 1500 r / min, 1800 r / min, 2000 r / min, 2200 r / min, 2500 r / min, 2600 r / min, 2800 r / min, 3000 r / min, etc.

[0119] Furthermore, t1 is 1 to 6 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, etc., within the dispersion rotation speed and time range, which is conducive to dissolving and fully dispersing the solid electrolyte.

[0120] Furthermore, n2 is 500~3000r / min, for example, it can be 500r / min, 550r / min, 580r / min, 1000r / min, 1100r / min, 1200r / min, 1500r / min, 1800r / min, 2000r / min, 2200r / min, 2500r / min, 2600r / min, 2800r / min, 3000r / min, etc.

[0121] Furthermore, t2 is 1 to 6 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, etc., within the stirring speed and time range, it is beneficial to stir and mix the aramid fiber evenly.

[0122] In said S03:

[0123] In some embodiments, the method of disposing the second mixed liquid on the base film 10 includes a second coating.

[0124] Furthermore, the second coating method includes one or more of spin coating, spray coating, wire rod coating, and dip coating.

[0125] In some embodiments, after the second mixed liquid is disposed on the base film 10 , a second phase conversion and drying are further included.

[0126] It is understood that the second phase inversion is a conventional technology in the art, and its purpose is to remove the dispersant and the solvent and to quickly form a film and pores.

[0127] Furthermore, the drying temperature is 40-80°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C, etc., and the drying time is 1-300min, for example, 1min, 10min, 50min, 60min, 80min, 100min, 120min, 150min, 180min, 200min, 220min, 250min, 280min, 300min, etc. Within the temperature and time range, it is beneficial to dry the second mixed liquid after the second phase conversion and obtain a composite flame retardant diaphragm.

[0128] In the embodiment of the present application, part of the second solvent in the second mixed liquid will dissolve the fluorinated organic matter in the prefabricated base film 10. After coating, this part of the solvent will dissolve a small amount of fluorinated organic matter. The dissolved fluorinated organic matter is a flexible polymer. Aramid is a macromolecule arranged in a zigzag shape. The flexibility of the fluorinated organic matter and aramid is utilized, and the two are mixed and staggered. At the same time, the toughening agent is a rod-like structure, which is interspersed in the fluorinated organic matter and aramid, and is arranged randomly and flexibly. After drying, the solvent evaporates to form a network structure, so that an interface layer 30 is formed between the base film 10 and the flame retardant layer 20, and the interface layer 30 is tightly bonded.

[0129] In a third aspect, an embodiment of the present application further provides a battery, wherein the battery comprises the composite flame retardant diaphragm described in the first aspect or the composite flame retardant diaphragm prepared by the preparation method described in the second aspect.

[0130] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0131] Example 1

[0132] This embodiment provides a method for preparing a composite flame-retardant diaphragm as follows:

[0133] 800g of PVDF and 250g of silicon carbide whiskers were added to 4500g of DMF solvent and mixed at 1500r / min for 3h to obtain a first mixed liquid; then the first mixed liquid was coated on the release film using a coater, and a base film with a thickness of 12μm was obtained through phase conversion, drying, demolding and winding.

[0134] 250g solid electrolyte LLZO and 12.5g dispersant polyacrylamide were added to a mixed solvent of 2250g DMF and 250g ethanol and dispersed at 1500r / min for 3h. Subsequently, 25g meta-aramid was added and stirred at 1500r / min for 3h to obtain a second mixed liquid. The second mixed liquid was coated on the base film using a coating machine, and then dried and rolled to obtain a composite flame retardant diaphragm with a thickness of 14.15μm.

[0135] Example 2

[0136] This embodiment provides a method for preparing a composite flame-retardant diaphragm as follows:

[0137] 600 g of PVDF and 10 g of silicon carbide whiskers were added to 2700 g of DMF solvent and mixed at 500 r / min for 6 hours to obtain a first mixed solution; then the first mixed solution was coated on a release film using a coating machine, and then phase inversion method, drying, demolding, and winding were performed.

[0138] 500g of solid electrolyte LLZO and 25g of dispersant polyacrylamide were added to a mixed solvent of 4500g DMF and 500g ethanol and dispersed at 500r / min for 6h. Subsequently, 500g of meta-aramid was added and stirred at 500r / min for 6h to obtain a second mixed liquid. The second mixed liquid was coated on the base film using a coating machine, and the composite flame-retardant diaphragm was obtained after drying and winding.

[0139] Example 3

[0140] This embodiment provides a method for preparing a composite flame-retardant diaphragm as follows:

[0141] 900 g of PVDF and 500 g of silicon carbide whiskers were added to 6000 g of DMF solvent and mixed at 3000 r / min for 3 hours to obtain a first mixed solution; then the first mixed solution was coated on a release film using a coating machine, and then phase inversion method, drying, demolding, and winding were performed.

[0142] 500g of solid electrolyte LLZO and 25g of dispersant polyacrylamide were added to a mixed solvent of 4500g DMF and 500g ethanol and dispersed at 3000r / min for 1h, then 50g of meta-aramid was added and stirred at 3000r / min for 1h to obtain a second mixed liquid, and the second mixed liquid was coated on the base film using a coating machine, and the composite flame retardant diaphragm was obtained after drying and winding.

[0143] Example 4

[0144] This embodiment is basically the same as Embodiment 1, except that PVDF is replaced by PVDF-HFP.

[0145] Example 5

[0146] This embodiment is basically the same as embodiment 1, except that PVDF is replaced by PVDF-TrFE.

[0147] Example 6

[0148] This embodiment is basically the same as Embodiment 1, except that the meta-aramid is replaced by para-aramid.

[0149] Example 7

[0150] This embodiment is basically the same as Embodiment 1, except that LLZO is replaced by LATP.

[0151] Example 8

[0152] This embodiment is basically the same as embodiment 1, except that LLZO is replaced by LLZO doped with niobium, and the molecular formula is Li 6.75 La 3 Zr 1.75 Nb 0.25 O12 .

[0153] Example 9

[0154] This embodiment is basically the same as the embodiment 1, except that LLZO is replaced by LLZO of aluminum and tantalum elements, and the molecular formula is Li 5.8 La 3 Zr 1.4 Ta 0.6 Al 0.2 O 12 .

[0155] Example 10

[0156] This embodiment is substantially the same as Embodiment 1, except that the silicon carbide whiskers are replaced with silicon nitride whiskers.

[0157] Embodiment 11

[0158] This embodiment is basically the same as Embodiment 1, except that the silicon carbide whiskers are replaced with glass fibers.

[0159] Comparative Example 1

[0160] The difference between this comparative example and Example 1 is that the amount of PVDF in Example 1 is replaced with 10 g, and a film cannot be formed.

[0161] Comparative Example 2

[0162] The difference between this comparative example and Example 1 is that the meta-aramid in Example 1 is removed.

[0163] Comparative Example 3

[0164] This comparative example is a conventional lithium battery separator available on the market.

[0165] Figure 1 and Figure 3 This is the SEM image of the composite flame retardant membrane prepared in Example 1. Figure 1 and Figure 3 It can be seen that an interface layer is formed between the base membrane and the flame retardant layer, and particles are interspersed in the flame retardant layer, which improves the strength of the composite flame retardant membrane. At the same time, the existence of the interface layer makes the base membrane and the flame retardant layer quite tightly combined. In addition, the flame retardant layer formed by aramid and solid electrolyte has a rich pore structure, which enhances the affinity between the composite flame retardant membrane and the electrolyte, increases the liquid absorption, and effectively reduces the internal resistance of the battery.

[0166] The flame retardant properties, ionic conductivity and tensile strength of the composite flame retardant membranes of Examples 1 to 11 and the battery membranes of Comparative Examples 2-3 were tested respectively. The test results are shown in Table 1, wherein the flame retardant properties were measured by a vertical combustion method; the ionic conductivity was measured by an AC impedance method; and the tensile strength was tested according to GB / T10403-2006 "Test of Tensile Properties of Plastics" and ASTMD882-10 "Standard Test Method for Tensile Properties of Thin Plastic Sheeting".

[0167] Table 1

[0168]

[0169]

[0170] From Table 1, we can see that:

[0171] Compared with Comparative Example 3, Examples 1-11 of the present invention have very good combustion performance of the composite flame-retardant membranes of the embodiments of the present application. In addition, the ionic conductivity of the composite flame-retardant membranes of the embodiments of the present application is higher than that of Comparative Example 3. This is because the base membrane uses fluorine-containing organic matter as the main film-forming material, which has good flame retardant effect itself. When aramid encounters high temperature, it will quickly carbonize and thicken to form an insulating barrier, isolate high temperature, and further improve the flame retardant performance. The commercially available conventional lithium battery membrane of Comparative Example 3 is a non-polar polymer with poor electrolyte wettability, resulting in a large internal resistance of the battery and low ionic conductivity. The fluorine-containing organic matter of the present application has a stronger polarity and a higher dielectric constant, which improves the lyophilicity of the composite flame-retardant membrane and helps the ionization of lithium salts, thereby improving the conductivity efficiency.

[0172] Compared with Comparative Example 2, Examples 1-11 of the present invention have higher tensile strengths than Comparative Example 2, indicating that the addition of aramid is beneficial to improving the mechanical properties of the composite flame-retardant diaphragm.

[0173] In Comparative Example 1, since the amount of PVDF was too small, a film could not be formed.

[0174] Battery Example 1

[0175] This embodiment provides a battery, and the preparation method is as follows:

[0176] Lithium nickel cobalt manganese oxide, conductive agent Super P, and binder PVDF are mixed in a mass ratio of 8:1:1, dispersed in an organic solvent NMP (N-methylpyrrolidone), and stirred until stable and uniform to form a positive electrode slurry. The positive electrode slurry is scraped onto an aluminum foil with a thickness of 10 μm, dried at 80°C, and then heated to 120°C for further vacuum drying, and then rolled and sliced ​​to form a positive electrode sheet;

[0177] In an inert atmosphere in a glove box, the negative electrode shell | spring sheet | gasket | lithium sheet | electrolyte | composite flame-retardant separator of Example 1 | positive electrode sheet | positive electrode shell were assembled in sequence, and the assembly was completed by pressing at 800 kPa for 5 s to obtain a fully electric button cell.

[0178] Battery Examples 2 to 11

[0179] Battery Examples 2 to 11 are substantially the same as Battery Example 1, with the only difference being that the composite flame-retardant diaphragm of Example 1 is replaced by the composite flame-retardant diaphragms of Examples 2 to 11 in Battery Examples 2 to 11, respectively.

[0180] Based on the test results of the composite flame-retardant membrane comparison example, battery comparison example 2 and battery comparison example 3 were set up.

[0181] Battery Comparison Example 2 and Battery Comparison Example 3

[0182] Battery Comparison Example 2 and Battery Comparison Example 3 are basically the same as Battery Example 1, with the only difference being that the composite flame retardant diaphragm of Example 1 is replaced by the composite flame retardant diaphragm of Battery Comparison Example 2 and the lithium battery diaphragm of Battery Comparison Example 3, respectively.

[0183] The capacity retention rates of battery examples 1 to 11, battery comparative example 2 and battery comparative example 3 were tested respectively, and the data results are shown in Table 2.

[0184] Among them, the test method of capacity retention rate (cycle curve) is: charge the battery to 4.2V at 0.33C constant current and constant voltage at 25°C, and then discharge it to 3.0V at 0.5C constant current. This is one cycle. The remaining capacity is the capacity retention rate. Compare the number of cycles and capacity retention rates of each battery.

[0185] Table 2

[0186]

[0187]

[0188] From Table 2, we can see that:

[0189] Compared with battery comparison example 2, the composite flame retardant diaphragm prepared in battery examples 1-11 of the present invention is applied to the battery, and the number of cycles of battery examples 1-11 is much higher than that of battery comparison example 2, indicating that the battery of the present invention has a longer life; the capacity retention rate of battery examples 1-11 after 100 cycles is higher than that of battery comparison example 2, indicating that the battery of the present invention has a better capacity retention rate after 100 cycles and a longer cycle life.

[0190] Compared with battery comparison example 3, i.e., commercial diaphragm, battery examples 1-11 of the present invention can still maintain a relatively high capacity retention rate after a relatively long cycle time; at the same time, it can be clearly seen from Table 2 that the battery of the present invention has a better capacity retention rate within 100 cycles and a longer cycle life.

[0191] The composite flame-retardant diaphragm provided in the embodiments of the present application, its preparation method and application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. An interface layer, characterized in that: The material of the interface layer includes fluorine-containing organic matter, toughening agent and aramid, and the interface layer is a mesh structure.

2. The interface layer according to claim 1, characterized in that The interface layer also includes a solid electrolyte.

3. The interface layer according to claim 2, characterized in that The solid electrolyte in the interface layer includes one or more of LATP, doped or undoped LLZO; and / or The thickness of the interface layer is 100-200 nm.

4. The interface layer according to any one of claims 1 to 3, characterized in that: The fluorine-containing organic compound in the interface layer includes one or more of polyvinylidene fluoride, polyvinylidene fluoride-hydrofluoric acid copolymer, polyvinylidene fluoride-trifluoroethylene copolymer; and / or The toughening agent in the interface layer includes one or more of silicon carbide whiskers, silicon nitride whiskers, glass fibers, and polymethyl methacrylate; and / or The aramid fiber includes at least one of meta-aramid fiber and para-aramid fiber.

5. A composite flame retardant diaphragm, characterized in that: The composite flame-retardant membrane comprises the interface layer as claimed in any one of claims 1 to 4.

6. The composite flame-retardant diaphragm according to claim 5, characterized in that: The composite flame-retardant diaphragm further comprises a base film, and the interface layer is integrally formed on the surface of the base film; and / or The composite flame-retardant membrane further comprises a base film and a flame-retardant layer. The flame-retardant layer and the interface layer are integrally formed on the surface of the base film, and the interface layer is located between the flame-retardant layer and the base film.

7. A composite flame retardant diaphragm according to claim 6, characterized in that: The flame retardant layer comprises aramid; and / or The material of the base film includes fluorine-containing organic matter and a toughening agent; and / or The base film has a thickness of 7 to 19 μm.

8. The composite flame-retardant diaphragm according to claim 6, characterized in that: The flame retardant layer further comprises a solid electrolyte, and in the flame retardant layer, the mass ratio of the solid electrolyte to the aramid fiber is (1-10):1; And / or, the thickness of the flame retardant layer is 1 to 4 μm; And / or, the toughening agent in the base film includes one or more of silicon carbide whiskers, silicon nitride whiskers, glass fibers, and polymethyl methacrylate; And / or, the fluorine-containing organic compound in the base film includes one or more of polyvinylidene fluoride, polyvinylidene fluoride-hydrofluoric acid copolymer, and polyvinylidene fluoride-trifluoroethylene copolymer; And / or, in the base film, the mass ratio of the fluorine-containing organic compound to the toughening agent is (0.6-0.9):(0.01-0.5).

9. A composite flame retardant diaphragm according to claim 6, characterized in that: The material of the base film includes a fluorine-containing organic substance and a toughening agent; the toughening agent includes one or more of silicon carbide whiskers, silicon nitride whiskers, glass fibers, and polymethyl methacrylate; in the base film, the mass ratio of the fluorine-containing organic substance to the toughening agent is (0.6-0.9):(0.01-0.5); The flame retardant layer includes aramid and a solid electrolyte. In the flame retardant layer, the mass ratio of the solid electrolyte to the aramid is (1-10):

1.

10. A battery, characterized in that: The battery comprises the composite flame-retardant separator according to any one of claims 5 to 9.

Citation Information

Patent Citations

  • Coating for power lithium battery diaphragm, power lithium battery diaphragm and preparation thereof

    CN102433745A

  • Aramid coated lithium ion battery diaphragm and preparation method thereof

    CN104993089A

  • Fluorine-containing resin based membrane reinforced by homogenous fibers modified by oriented fibers

    CN105261722A

  • Toughening-modified polyvinylidene fluoride composite material used for injection extrusion molding, and preparation method thereof

    CN106854328A

  • Preparation method of para-aramid nanometer fiber composite lithium ion battery separator

    CN107452921A