Method for desorbing and recycling collecting agent in flotation concentrate
By performing stirring desorption treatment and hydrochloric acid solution pretreatment in acid solution, the problem of difficulty in desorbing fatty acid collectors in flotation concentrates is solved, efficient collector desorption and reuse is achieved, and the cost of smelting wastewater treatment is reduced. and the amount of smelting tailings, improving the quality of the concentrate.
Patent Information
- Application Number
- CN202410054963.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-01-15
AI Technical Summary
Existing technology is difficult to efficiently desorb fatty acid collectors in flotation concentrates, resulting in loss of chemicals and increased smelting wastewater treatment costs, and traditional methods cannot realize the reuse of collectors.
Stirring and desorption treatment are carried out in the acid solution, controlling the pH value to be less than or equal to 4.0 and the temperature between 0 and 10°C. Combined with the pretreatment of hydrochloric acid solution in the pretreatment stage, the selective desorption and recycling of the organic acid collector can be achieved.
It achieves efficient desorption and reuse of fatty acid collectors in flotation concentrates, reduces the COD content of smelting wastewater and the cost of chemicals during the smelting process, and improves the management of concentrate quality and smelting tailings volume.
Smart Images

Figure BDA0004664424950000041 
Figure BDA0004664424950000051 
Figure BDA0004664424950000052
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mineral flotation, in particular to a method for desorbing a collector in a flotation concentrate. Background Art
[0002] The concentrate obtained after flotation usually has a large amount of flotation reagents, generally collectors, on its surface. When these concentrates with a large amount of flotation reagents remain in the smelter, they will not only cause difficulties in the smelting process, but also lose a large amount of flotation reagents, causing waste, and also increase the cost of smelting wastewater treatment.
[0003] There are two main methods for desorbing reagents from the surface of flotation concentrates: physical desorption and chemical desorption. Physical desorption mainly includes heating, exposure, stirring, filtering and washing. Chemical desorption is to use various acids, alkalis, hydrogen peroxide, potassium permanganate and other desorbents to replace, electrochemically or redox react with reagents adsorbed on the surface of minerals, change the surface potential of minerals, and destroy the molecular structure of reagents, so as to achieve the purpose of desorption. The existing methods have low desorption efficiency, and when chemical desorption is used, adding desorbents will destroy the activity of the reagents, making them impossible to reuse.
[0004] In addition, compared with chelating collectors, fatty acid collectors have stronger interactions with active sites on the mineral surface, which results in the inability of traditional physical or chemical desorption methods to efficiently desorb fatty acids from the surface of flotation concentrates. Therefore, it is urgent to develop methods for desorption and recycling of fatty acid collectors. Summary of the invention
[0005] The object of the present invention is to provide a method for desorbing a collector in a flotation concentrate, aiming to effectively desorb the collector in the concentrate to obtain a high-quality concentrate, and not only that, but also to selectively reuse the desorbed collector or reduce the treated COD.
[0006] The present invention also includes a method for recycling the desorbed reagent.
[0007] A method for desorbing a collector in a flotation concentrate, wherein the flotation concentrate is subjected to stirring desorption treatment in an acid solution, followed by solid-liquid separation to obtain a desorbed concentrate;
[0008] The flotation concentrate comprises a mineral and a collector bonded to the surface thereof, wherein the collector comprises an organic acid collector;
[0009] In the desorption stage, the pH of the system is less than or equal to 4.0, the temperature is 0-10°C, and the stirring speed is above 1000r / min.
[0010] In view of the problems of lack of desorption means for organic acid collectors, great difficulty in desorption, and easy failure of desorption agents, the present invention desorbs the concentrate of organic acid flotation in acid solution, and cooperates with the joint control of pH, stirring and temperature in the treatment stage to achieve synergy, which can improve the desorption effect of organic acid collectors and minerals in the concentrate. Not only that, it is also beneficial to avoid failure and degradation of the collector caused by desorption, and can also reduce the COD content of the treated solution.
[0011] In the present invention, the flotation concentrate is the flotation concentrate obtained by flotating a mineral in a flotation reagent containing a collector.
[0012] The minerals may be oxidized ores and / or non-metallic ores;
[0013] In the present invention, the oxide ore includes at least one of scheelite, cassiterite, bauxite, apatite and fluorite, for example.
[0014] In the present invention, when the mineral is a mineral containing calcium gangue, it is pretreated with a hydrochloric acid solution before the desorption treatment. In the present invention, the flotation concentrate is pretreated in a hydrochloric acid solution, and then the solid-liquid separation is performed to obtain the pretreated concentrate, which is then subjected to subsequent desorption treatment. The preferred scheme of the present invention, based on the combination of the pretreatment and desorption processes, can synergistically further improve the desorption effect of the collector and the mineral, improve the quality of the flotation concentrate, and not only that, but also facilitate the recycling of the desorbed collector.
[0015] In the present invention, the pH of the system in the pretreatment stage is 4.5 to 6.5.
[0016] In the present invention, the collector comprises at least one of fatty acid collectors, sulfonic acid collectors, sulfuric acid collectors, and phosphonic acid collectors; more preferably, it is one or more anionic collectors selected from oleic acid and its salts, cyclohexane acid and its salts, sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, oxidized paraffin soap, tall oil and its salts, and dodecylaminobis(methylenephosphonic acid).
[0017] In the present invention, the acidic solute dissolved in the acid solution is at least one of HCl, H2SO4, and HNO3.
[0018] In the present invention, the combined control of pH, strong stirring and temperature in the desorption stage is the key to synergistically improving the desorption of the collector.
[0019] Preferably, the pH of the desorption stage system is 0 to 4, preferably 1 to 3. In the present invention, under the process described above, further with the preferred pH, a better organic acid desorption effect can be unexpectedly obtained, and in addition, the deactivation and degradation of the organic acid in the desorption stage can be avoided.
[0020] Preferably, the temperature of the desorption stage system is 0-5° C., more preferably 1-3° C. In the present invention, under the process, further with the preferred temperature, a better organic acid desorption effect can be unexpectedly obtained, and in addition, the deactivation and degradation of the organic acid in the desorption stage can be avoided.
[0021] In the present invention, the concentration of the ore pulp during the desorption process is 5 to 40%, and more preferably 5 to 20%.
[0022] Preferably, the stirring speed is 1000-3000 r / min, preferably 1500-3000 r / min.
[0023] Preferably, the desorption treatment time is more than 5 minutes, preferably 5 to 60 minutes.
[0024] An illustrative scheme of the present invention (also referred to as scheme A) is as follows: tungsten concentrate is desorbed in a hydrochloric acid solution, wherein the pH of the desorption stage is controlled between 1.0 and 3.5, and the temperature is controlled between 0 and 5°C, followed by solid-liquid separation to obtain desorbed tungsten concentrate, and the liquid portion is low-COD treated wastewater. The scheme described in the present invention can achieve efficient separation of the collector and the mineral in the concentrate, which is helpful for obtaining high-quality tungsten concentrate. Not only that, it can also reduce the impact of the desorbed collector on the treated water, and can simultaneously obtain low-COD treated water.
[0025] A further scheme of the present invention (also referred to as scheme B) is as follows: the tungsten concentrate is placed in a hydrochloric acid solution for pretreatment, solid-liquid separation is performed to obtain a pretreated concentrate, and then the pretreated concentrate is desorbed in an acid solution, and solid-liquid separation is performed to obtain the desorbed tungsten concentrate and the desorption liquid, and the desorption liquid is saponified and recycled as a collector. The pH of the pretreatment stage is 4.5 to 6.5. The pH of the desorption stage is controlled between 1.0 and 3.5, and the temperature is controlled between 0 and 5°C. The preferred embodiment of the present invention can achieve the recycling of the collector.
[0026] The present invention also provides a method for recycling mineral surface flotation reagents, wherein the reagents after desorption treatment are obtained by the method described in the present invention, and the reagents are recycled for flotation of the next batch of minerals.
[0027] Preferably, the solution containing the reagent after the desorption treatment is subjected to saponification treatment, and the saponified solution is used for mineral flotation.
[0028] Beneficial effects:
[0029] (1) Realize the selective desorption and recycling of fatty acid collectors on the surface of flotation concentrate
[0030] In the present invention, the flotation concentrate is treated with an acid solution under a low temperature environment, and the fatty acid collector on the mineral surface is efficiently desorbed based on a physical and chemical combination method, and the loss of the reagent is reduced. Furthermore, if the desorption collector containing highly active molecules or ions after solid-liquid separation is recycled, the cost of flotation reagents can be reduced and the flotation index of the target mineral can be improved.
[0031] (2) Improve the quality of flotation concentrate and reduce the amount of smelting tailings
[0032] The method for desorption of collectors from the surface of flotation concentrate of the present invention, whether it is the preferred scheme A or scheme B, after the flotation concentrate is treated with hydrochloric acid, calcium-containing gangue minerals and the like are eliminated, which helps to improve the quality of the flotation concentrate and reduce the amount of tailings after smelting the flotation concentrate.
[0033] (3) Recycling of desorption reagents helps reduce the cost of flotation reagents and smelting water treatment costs, while improving the smelting process
[0034] The present invention provides a simple and efficient selective desorption technology for reagents on the surface of minerals, and recycles the desorbed reagents back to the flotation process, thereby realizing the sustainable use technology of reagent adsorption-desorption-reuse-adsorption. This technology not only realizes the sustainable recycling of fatty acid collectors and reduces the cost of flotation reagents, but also reduces the wastewater treatment cost and the smelting process (the less the residual reagents on the surface of the concentrate, the less impact on the smelting process), protects the ecological environment, achieves a win-win situation for mineral processing enterprises and smelting enterprises, and ensures their economic benefits and sustainable development. DETAILED DESCRIPTION
[0035] Embodiment 1:
[0036] Typical case of plan A;
[0037] Step (1): Ore concentrate source
[0038] The raw ore was selected from a certain scheelite in Chenzhou, Hunan, where the raw ore grade WO3 was 0.40%, and the main gangue minerals were garnet, quartz and calcite. After one roughing, five fines and three sweeps at room temperature, a tungsten concentrate with a WO3 grade of 51.10% and a recovery rate of 80.05% was obtained. Among them, the amount of oxidized paraffin soap used as the roughing collector was 320g / t, the amount of depressant water glass was 3000g / t, the amount of oxidized paraffin soap used in sweep 1 was 80g / t, the amount of oxidized paraffin soap used in sweep 2 and sweep 3 was 40g / t, the amount of water glass used in select 1 was 2000g / t, the amount of acidified water glass used in select 2 and select 3 was 500g / t and 300g / t respectively, and select 4 and select 5 were blank selects.
[0039] Step (2): Desorption
[0040] The tungsten concentrate slurry is placed in a stirrer, the slurry concentration is adjusted to 5%, the stirring speed of the stirrer is 2500r / min, the temperature is controlled at 0-8°C, and then concentrated hydrochloric acid is added to adjust the pH value of the slurry. The stirring time is 30min. After the stirring is completed, the slurry is allowed to stand for 10min, and then solid-liquid separation is performed, and the COD value of the flotation concentrate concentrated filtration wastewater before and after the collector desorption treatment is measured. The desorption rate under different conditions is shown in Table 1.
[0041] Table 1
[0042]
[0043]
[0044] It can be seen from Table 1 that at 2°C and pH 2.0, the fatty acid desorption rate is as high as 87.94%; the COD value of the concentrated filtered wastewater before desorption treatment of the flotation concentrate is 320.14 mg / L, and the COD value of the wastewater is reduced to 38.99 mg / L after desorption treatment, and the COD is reduced by 87.82%; the grade of tungsten concentrate WO3 is increased to 65.35%.
[0045] Embodiment 2:
[0046] Typical case of pH and temperature in Scheme A;
[0047] Different from Example 1, the raw ore is selected from a certain place in Hengyang, Hunan Province, wherein the raw ore grade WO3 is 0.34%, and the main gangue minerals are calcite, feldspar, and quartz. After one roughing, three fines, and two sweeping, a tungsten concentrate with a grade of WO3 of 6.52% and a recovery rate of 80.86% is obtained at room temperature. Then, the tungsten rough concentrate is further subjected to heating and fine selection to obtain a tungsten concentrate with a grade of WO3 of 57.72% and a recovery rate of 75.98%. Among them, the amount of sodium oleate used as a roughing collector is 300g / t, the amount of water glass used as an inhibitor is 500g / t, the amount of sodium oleate used in scavenging 1 is 70g / t, the amount of sodium oleate used in scavenging 2 is 35g / t, the amount of water glass used in fine selection 1 is 2500g / t, the amount of water glass used in fine selection 2 is 120g / t, and fine selection 3 is blank fine selection.
[0048] The tungsten concentrate slurry was placed in a stirrer, the slurry concentration was adjusted to 10%, the stirring speed of the stirrer was 2000r / min, the temperature was controlled at 0-6°C, and then concentrated hydrochloric acid was added to adjust the pH value of the slurry. The stirring time was 6 minutes. After the stirring was completed, the slurry was allowed to stand for 20 minutes, and then solid-liquid separation was performed, and the COD value of the flotation concentrate concentrated filtration wastewater before and after the collector desorption treatment was measured. The desorption rate under different conditions is shown in Table 2.
[0049] Table 2
[0050]
[0051] It can be seen from Table 2 that at 1°C and pH 1.0, the fatty acid desorption rate is as high as 88.72%; the COD value of the concentrated filtered wastewater before desorption treatment of the flotation concentrate is 271.68 mg / L, and the COD value of the wastewater is reduced to 30.45 mg / L after desorption treatment, and the COD is reduced by 88.79%; the grade of tungsten concentrate WO3 is increased to 72.60%.
[0052] Embodiment 3:
[0053] Examples in Scheme B, and examples of typical values of pH and temperature;
[0054] Step (1): The raw ore is selected from a certain place in Jiujiang, Jiangxi Province, wherein the raw ore grade WO3 is 0.40%, and the gangue is mainly garnet, calcite, fluorite, etc. After one roughing, four fines and two sweeps, a tungsten concentrate with a WO3 grade of 45.12% and a recovery rate of 82.30% is obtained. The amount of sodium oleate used as the roughing collector is 300g / t, the amount of water glass used as the inhibitor is 4000g / t, the amount of sodium oleate used in sweeping 1 is 100g / t, the amount of water glass used is 500g / t, the amount of sodium oleate used in sweeping 2 is 50g / t, the amount of water glass used in concentrating 1 is 2000g / t, the amount of water glass used in concentrating 2 is 1000g / t, and concentrating 3 and concentrating 4 are blank concentrating. The flotation results (without desorption liquid) are shown in Table 3.
[0055] Step (2): adding concentrated hydrochloric acid, pre-adjusting the pH of the obtained tungsten concentrate slurry to 6.0, and treating for 5 minutes. At this time, a large amount of gangue minerals in the slurry are dissolved (calcite, etc.), followed by solid-liquid separation, placing the pre-treated slurry in a stirrer, controlling the temperature at 0-5°C, adjusting the slurry concentration to 10%, adjusting the pH to 2.5, stirring at a speed of 2500r / min, stirring for 25 minutes, and allowing the slurry to stand for 10 minutes, followed by solid-liquid separation, the desorption rate of the collector on the surface of the tungsten concentrate is 89.70%. At the same time, after being treated by the above desorption method, the grade WO3 of the tungsten concentrate can be increased to 64.27%, and the recovery rate remains basically unchanged.
[0056] Step (3): Then, the desorption liquid containing a large amount of collector after solid-liquid separation is returned to the tungsten roughing. Except for the change in the amount of collector, other flotation conditions remain unchanged. The flotation results with or without the addition of desorption liquid are shown in Table 3.
[0057] It can be seen from Table 3 that by desorbing and reusing the collector on the surface of tungsten concentrate, the amount of collector can be reduced to 180g / t of sodium oleate, a reduction of up to 40%, and the flotation index of scheelite is improved.
[0058] Table 3
[0059]
[0060] Embodiment 4:
[0061] The raw ore was selected from a fluorite mine in Henan Province, with a CaF2 grade of 49.71% and main gangue minerals of calcite, quartz and a small amount of mica, feldspar, etc. After pre-desulfurization, one roughing and seven fines, the selected middlings were concentrated and re-selected and then returned to the roughing, a fluorite concentrate with a CaF2 grade of 90.43% and a recovery rate of 81.38% was obtained. Among them, the dosage of oleic acid as roughing collector is 1000g / t, the dosage of water glass as inhibitor is 2500g / t, the dosage of oleic acid in selection 1 is 50g / t, the dosage of water glass is 400g / t, the dosage of acidified water glass in selection 2 is 400g / t, the dosage of acidified water glass in selection 3 is 300g / t, the dosage of acidified water glass in selection 4 is 240g / t, the dosage of acidified water glass in selection 5 is 180g / t, the dosage of acidified water glass in selection 6 is 180g / t, the dosage of acidified water glass in selection 7 is 180g / t, the dosage of oleic acid in concentrated re-selection of middlings is 200g / t, and the dosage of water glass is 800g / t.
[0062] The above fluorite concentrate slurry was placed in a stirrer, the slurry concentration was adjusted to 15%, the stirring speed of the stirrer was 1800r / min, the temperature was controlled at 0-5°C, and then concentrated hydrochloric acid was added to adjust the pH value of the slurry. The stirring time was 20min. After the stirring was completed, the slurry was allowed to stand for 10min, and then solid-liquid separation was performed, and the COD value of the flotation concentrate concentrated filtration wastewater before and after the collector desorption treatment was measured. The desorption rate under different conditions is shown in Table 4. It can be seen from Table 4 that at 2°C and pH 2.0, the fatty acid desorption rate was as high as 81.56%; the COD value of the concentrated filtration wastewater before the flotation concentrate desorption treatment was 143.37mg / L, and the COD value of the wastewater after desorption treatment was reduced to 55.04mg / L, and the COD was reduced by 61.61%; the CaF2 grade of the fluorite concentrate was increased to 97.02%.
[0063] Table 4
[0064]
[0065] Comparative Example 1
[0066] Compared with Example 1, the only difference is that in the desorption stage of step (2), the pH is 9.0 (temperature is 2°C), and the rest is the same as Example 1. The desorption rate of the collector on the surface of the tungsten concentrate is 29.35%. After the desorption treatment, the COD value of the concentrated filtered wastewater of the tungsten concentrate is increased to 395.20 mg / L, the COD is increased by 23.35%, and the grade of tungsten concentrate WO3 is still maintained at about 51%.
[0067] Comparative Example 2
[0068] Compared with Example 1, the only difference is that in the desorption stage of step (2), the temperature is 35°C (pH is 2), and the rest is the same as Example 1. The desorption rate of the collector on the surface of the tungsten concentrate is 21.06%, and the COD value of the concentrated filtered wastewater of the tungsten concentrate after desorption treatment is reduced to 50.02 mg / L, COD is reduced by 84.38%, and the grade of tungsten concentrate WO3 is 65.28%.
[0069] Comparative Example 3
[0070] Compared with Example 3, the only difference is that the stirring speed during desorption is 800r / min, and the others are the same as Example 3. The desorption rate of the collector on the surface of the tungsten concentrate is 23.72%, and the grade of WO3 of the tungsten concentrate after desorption treatment is 56.10%. The collector is reused after desorption, and the amount of the collector is reduced to 270g / t of sodium oleate, which is reduced by 10%.
[0071] Through Examples 1 to 3 and Comparative Examples 1 to 3, it can be seen that in the desorption process, the desorption effect under low temperature and strong acid conditions is excellent, and the desorption rate can reach about 90%. In addition, in the desorption process, too low stirring speed and too short stirring time will also affect the desorption, and then affect the flotation process after the desorption liquid is reused.
Claims
1. A method for desorbing a collector in a flotation concentrate, It is characterized in that The flotation concentrate is subjected to stirring and desorption treatment in an acid solution, followed by solid-liquid separation to obtain a desorbed concentrate; The flotation concentrate comprises a mineral and a collector bonded to the surface thereof, wherein the collector comprises an organic acid collector; In the desorption stage, the pH of the system is less than or equal to 4.0, the temperature is 0-10°C, and the stirring speed is above 1000r / min.
2. The method for desorbing a collector in a flotation concentrate according to claim 1, It is characterized in that The minerals include oxide minerals and / or non-metallic minerals; Preferably, the oxide ore includes at least one of scheelite, cassiterite, bauxite, apatite and fluorite.
3. The method for desorbing a collector in a flotation concentrate according to claim 2, It is characterized in that When the mineral is a mineral containing calcium gangue, it is pretreated with a hydrochloric acid solution before the desorption treatment.
4. The method for desorbing a collector in a flotation concentrate according to claim 3, It is characterized in that The pH of the system in the pretreatment stage is 4.5-6.
5.
5. The method for desorbing a collector in a flotation concentrate according to claim 1, It is characterized in that The collector comprises at least one of fatty acid collectors, sulfonic acid collectors, sulfuric acid collectors, and phosphonic acid collectors; more preferably, it is one or more anionic collectors selected from oleic acid and its salts, cyclopentaneic acid and its salts, sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, oxidized paraffin soap, tall oil and its salts, and dodecylaminobis(methylenephosphonic acid).
6. The method for desorbing a collector in a flotation concentrate according to any one of claims 1 to 5, It is characterized in that The acidic solutes dissolved in the acid solution are HCl, H 2 SO 4 , HNO 3 At least one of .
7. The method for desorbing a collector in a flotation concentrate according to any one of claims 1 to 5, It is characterized in that The pH of the system in the desorption stage is 0-4, preferably 1-3.
8. The method for desorbing a collector in a flotation concentrate according to any one of claims 1 to 5, It is characterized in that The concentration of the slurry during the desorption process is 5-40%.
9. The method for desorbing a collector in a flotation concentrate according to any one of claims 1 to 5, It is characterized in that The stirring speed is 1000-3000 r / min, preferably 1500-3000 r / min; Preferably, the desorption treatment time is more than 5 minutes, preferably 5 to 60 minutes.
10. A method for recycling mineral surface flotation reagents, It is characterized in that The recovered reagent is obtained by the method described in any one of claims 1 to 9; and the recovered reagent is reused in the flotation of the next batch of minerals; Preferably, the solution containing the reagent after the desorption treatment is subjected to saponification treatment, and the saponified solution is used for mineral flotation.
Citation Information
Patent Citations
Scheelite flotation
CA1140276A
Method for recycling collecting agent from flotation concentrate
CN102489413A
Fluorite fine separating method
CN110292991A
Method for selectively desorbing and recycling mineral surface medicament
CN111992336A
Desorption method and recycling method of concentrate surface flotation reagent
CN115041304A