Preparation method of high-strength ultrathin porous titanium plate

By grading titanium powder and rolling-forming spare titanium powder of suitable particle size, combined with constrained sintering technology, a high-strength ultra-thin porous titanium plate is prepared, which solves the problems of complex process and low strength in the existing technology and achieves porosity and strength uniformity and efficient production.

CN118768570APending Publication Date: 2024-10-15NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410809164.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When preparing high-strength ultra-thin porous titanium plates, the existing technology has complex processes and low strength, making it difficult to ensure the uniformity of porosity and strength, especially when there are uncertainties in large-scale commercial production.

Method used

By grading the titanium powder raw material powder, selecting spare titanium powder with appropriate particle size, and controlling the parameters in the rolling and sintering process through one-time rolling forming and constrained sintering, a product with a porosity of 20% to 60%, Porous titanium plates with a thickness less than 0.4mm and a width of 400mm to 550mm have a tensile strength greater than 100MPa.

Benefits of technology

The process is simplified, the production cost is reduced, the size, thickness and tensile strength of the porous titanium plate are significantly increased. The process is highly operable, suitable for large-scale production, and is expected to improve the performance and efficiency of electrolytic hydrogen production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-strength ultrathin porous titanium plate, which comprises the following steps: 1, grading titanium powder raw material powder to obtain standby titanium powder; secondly, the standby titanium powder is continuously fed into a gap between two working rollers through a feeding device, the two working rollers are located on the same horizontal plane and rotate in the opposite directions, rolling is conducted, and a green plate is obtained; and 3, carrying out constraint sintering on the green body plate, and carrying out furnace cooling to obtain the porous titanium plate. According to the method, the titanium powder raw material powder is graded, the standby titanium powder with the proper granularity is selected, it is guaranteed that the standby titanium powder has the proper fluidity and apparent density in the subsequent rolling process, the standby titanium powder is rolled into the green body plate through one-time rolling forming, and finally the porous titanium plate is obtained through constraint sintering. The prepared porous titanium plate is large in size, small in thickness, high in tensile strength, simple in technological process and high in operability, and the effects of further improving the performance and efficiency of hydrogen production through water electrolysis, reducing the cost and the like are expected to be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous metal materials, and in particular relates to a method for preparing a high-strength ultra-thin porous titanium plate. Background Art

[0002] With the proposal of the "dual carbon" strategic goal, the development and utilization of hydrogen energy will enter a substantial development stage, and the application of hydrogen energy will be diversified in the fields of energy storage, fuel, chemical industry, steel metallurgy, etc. In terms of hydrogen production, the proton exchange membrane (PEM) water electrolysis hydrogen production technology has many advantages such as high hydrogen purity, fast dynamic response speed, wide load range, high operating current density, high output hydrogen pressure, and compact structure. It is the most promising water electrolysis hydrogen production technology.

[0003] The porous diffusion layer is a key core component of the PEM water electrolysis hydrogen production device. The PEM electrolyzer usually needs to operate under high pressure or differential pressure conditions, which places high requirements on the mechanical strength of the diffusion layer. The porous titanium material has a wide range of application prospects in the gas diffusion layer material of the PEM water electrolyzer due to its good mechanical strength, ductility, electrical conductivity and corrosion resistance. Its design and preparation play a key role in further improving the performance and efficiency of hydrogen production by electrolysis and reducing costs.

[0004] The patent with application number CN202311126354.6 discloses a method for preparing an ultra-thin metal titanium plate with high porosity. The invention obtains raw materials by mixing titanium powder with a pore-forming agent, sintering the obtained green billet after the first rolling of the raw materials, and then rolling the sintered billet for the second time to obtain a metal porous titanium plate with a final thickness of less than 0.29mm, a porosity of ≥65%, and a width of 300-500mm. This patent increases the porosity of the titanium plate by adding a pore-forming agent and reduces the thickness of the titanium plate by increasing the number of rolling times. Although a porous titanium plate with a thin thickness and high porosity is obtained, the preparation process is relatively complicated and the strength of the obtained titanium plate is relatively low.

[0005] The patent with application number CN201911203716.0 discloses a preparation method for improving the uniformity of large-size powder-rolled metal porous plates. The invention adds a forming agent to the metal raw material powder to obtain a bonding powder and then saturates the bonding powder on the surface of the roller to improve the roller's bite ability on the fed raw material powder, improve the uniformity of the thickness and porosity of the rolled metal porous plate, and prepare a metal porous plate with a width of 450mm and a thickness deviation of ±5%. However, only the feeding speed is controlled during rolling feeding, and there is a certain difficulty in controlling the thickness and porosity.

[0006] Patent application number CN200710097748.8 discloses a method for preparing a metal porous thin titanium plate. The invention first pre-sinters the metal titanium powder through a mold to obtain a porous titanium plate body, and then controls the thickness through rolling on a rolling mill to obtain a porous thin titanium plate with a porosity of more than 45% and a thickness of 0.2-0.8 mm. However, for the preparation of porous materials, especially large-scale commercial preparation, the process preparation is relatively complicated, and it is difficult to ensure the uniformity of porosity and strength at various positions on a wide horizontal width, and there are many uncertain factors.

[0007] In view of the above-mentioned shortcomings of the prior art, a method for preparing a high-strength ultra-thin porous titanium plate is needed. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a method for preparing a high-strength ultra-thin porous titanium plate in view of the deficiencies of the above-mentioned prior art. The method classifies the titanium powder raw material powder, selects the spare titanium powder of suitable particle size, ensures that the spare titanium powder has suitable fluidity and bulk density in the subsequent rolling process, rolls the spare titanium powder into a green sheet through one-time rolling molding, and finally obtains a porous titanium plate through constrained sintering. The prepared porous titanium plate has large size, small thickness, high tensile strength, simple process flow and strong operability.

[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a high-strength ultra-thin porous titanium plate, characterized in that the method comprises the following steps:

[0010] Step 1: Raw material preparation: Classify the titanium powder raw material powder, select the titanium powder with the required particle size, and obtain the spare titanium powder;

[0011] Step 2: rolling green sheet: the spare titanium powder obtained in step 1 is continuously fed into the gap between two working rolls located on the same horizontal plane but rotating in opposite directions through a feeding device, and rolled by the pressure of the two working rolls to obtain a green sheet;

[0012] Step 3, sintering: the green sheet obtained in step 2 is cut and cleaned of floating powder, and then constrained sintering is performed, and a porous titanium plate is obtained after cooling in the furnace. The porous titanium plate has a porosity of 20% to 60%, a thickness of no more than 0.4 mm, a width of 400 mm to 550 mm, and a tensile strength of more than 100 MPa.

[0013] The present invention classifies titanium powder raw material powder and selects spare titanium powder of suitable particle size, thereby ensuring that the spare titanium powder has suitable fluidity and loose density in the subsequent rolling process, rolling the spare titanium powder into a green sheet, and finally obtaining a porous titanium plate by constrained sintering. The porous structure in the porous titanium plate is because a certain spatial structure is formed between titanium powder particles during the rolling and sintering processes, and these spatial structures are retained after cooling and solidification. The prepared porous titanium plate has a large size, a small thickness and a high tensile strength.

[0014] The above-mentioned method for preparing a high-strength ultra-thin porous titanium plate is characterized in that the particle size of the spare titanium powder in step 1 is -70 to +180 mesh, wherein -100 to +150 mesh accounts for 50% to 90%. The present invention controls the particle size of the spare titanium powder to ensure that its fluidity and loose density are within a suitable range, thereby controlling the amount of powder bite between the two working rollers during the rolling process, and finally obtaining a porous titanium plate with a porosity of 20% to 60% and a thickness of less than 0.4 mm, wherein -70 to +180 mesh means that the powder can leak through the 70 mesh but not the 180 mesh, and -100 to +150 mesh means that the powder can leak through the 100 mesh but not the 150 mesh.

[0015] The above-mentioned method for preparing a high-strength ultra-thin porous titanium plate is characterized in that support rollers are provided on both sides of the two working rollers in step 2 to support the working rollers. The main function of the support rollers in the present invention is to provide support and stability for the working rollers. They are located on both sides of the working rollers and help the working rollers maintain a stable rolling posture by bearing part of the rolling force, preventing them from bending or deflecting due to uneven force, which helps to ensure the continuity and stability of the rolling process and improve the quality and output of the plate or strip.

[0016] The above-mentioned method for preparing a high-strength ultra-thin porous titanium plate is characterized in that the diameter of the working roll in step 2 is 20 mm to 70 mm, and the diameter of the support roll is 300 mm to 600 mm. The present invention controls the bite angle during rolling by controlling the diameter of the working roll and the diameter of the support roll, thereby controlling the amount of bite powder, and finally obtaining a porous titanium plate with a thickness of less than 0.4 mm in combination with the particle size of the working roll.

[0017] The above-mentioned method for preparing a high-strength ultra-thin porous titanium plate is characterized in that the gap width between the two working rollers in step 2 is 0.01 mm to 0.4 mm. The present invention controls the thickness of the porous titanium plate by controlling the gap width between the two working rollers, thereby realizing the preparation of a porous titanium plate with a thickness of less than 0.4 mm.

[0018] The above-mentioned method for preparing a high-strength ultra-thin porous titanium plate is characterized in that the rolling speed in step 2 is 2m / min to 20m / min, and the rolling force is 8T to 20T. The present invention reduces the amount of bite of the spare titanium powder by the rolling speed, thereby achieving a porosity of 20% to 60% for the porous titanium plate, significantly improving production efficiency while controlling the porosity, and controlling the rolling force also plays a role in controlling the porosity, and at the same time, it also improves the structural strength of the porous titanium plate.

[0019] The above-mentioned method for preparing a high-strength ultra-thin porous titanium plate is characterized in that the constrained sintering in step 3 is to place the green sheet after cutting and cleaning the floating powder on the support plate, and then place the cover plate for constrained sintering. The present invention prevents the porous titanium plate from deforming during the sintering process through constrained sintering, thereby ensuring the performance of the porous titanium plate.

[0020] The above-mentioned method for preparing a high-strength ultra-thin porous titanium plate is characterized in that the constrained sintering in step 3 is performed at a vacuum degree of no more than 1×10 -3 Pa, the temperature is 900°C to 1200°C, and the time is 30min to 180min. The present invention controls the sintering parameters to fully sinter the spare titanium powder into a porous titanium plate, while ensuring the porosity and structural strength of the porous titanium plate.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] 1. The present invention classifies titanium powder raw material powder and selects spare titanium powder of suitable particle size, thereby ensuring that the spare titanium powder has suitable fluidity and loose density in the subsequent rolling process, and rolling the spare titanium powder into a green sheet through one-time rolling molding, and finally obtaining a porous titanium plate through constrained sintering. The prepared porous titanium plate has large size, small thickness, high tensile strength, simple process flow and strong operability.

[0023] 2. In the present invention, there is no need to add a pore-forming agent, so no degreasing treatment is required, which significantly simplifies the process flow and reduces production costs.

[0024] 3. The present invention controls the particle size of the spare titanium powder to ensure its fluidity and loose density within an appropriate range, thereby controlling the amount of powder bitten between the two rollers during the rolling process. The present invention controls the diameters of the two working rollers to control the biting angle during rolling, thereby controlling the amount of powder bitten, and finally obtaining a porous titanium plate with a porosity of 20% to 60% and a thickness of less than 0.4 mm, in combination with the powder particle size.

[0025] 4. The present invention can not only reduce the amount of powder bite and achieve a porosity of 20% to 60% by controlling the rolling speed, but also significantly improve production efficiency. By controlling the rolling force and coordinating the subsequent constrained sintering parameters, the porosity can be controlled to be 20% to 60% and the tensile strength to be greater than 100 MPa.

[0026] 5. The porous titanium plate prepared by the present invention, which has the characteristics of thin thickness and high strength, is expected to further play a key role in improving the performance and efficiency of electrolytic hydrogen production and reducing costs.

[0027] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION

[0028] Example 1

[0029] This embodiment includes the following steps:

[0030] Step 1, raw material preparation: the titanium powder raw material powder is classified, and the titanium powder of the required particle size is selected to obtain the spare titanium powder with a particle size of -90 to +140 mesh, and the powder of -100 to +140 mesh accounts for 82% of the spare titanium powder;

[0031] Step 2, rolling green billet: the spare titanium powder obtained in step 1 is continuously fed into the gap between two working rolls located in the same horizontal plane but rotating in opposite directions through a feeding device, and rolling is performed by the pressure of the two working rolls to obtain a green sheet; support rolls are provided on both sides of the two working rolls to support the working rolls; the diameters of the working rolls are 45 mm, the diameters of the support rolls are 400 mm, the gap width of the two working rolls is 0.1 mm, the rolling speed is 5 m / min, and the rolling force is 10 T;

[0032] Step 3: Sintering: Cut the green sheet obtained in step 2 and clean the floating powder, then place it on the firing plate and cover it. -3 Pa, the temperature is 1000 ° C, and the temperature is kept for 60 min for constrained sintering, and the porous titanium plate is obtained after cooling with the furnace.

[0033] After testing, the porous titanium plate prepared in this embodiment has a porosity of 31.5%, a thickness of 0.27 mm, a width of 410 mm, and a tensile strength of 128 MPa.

[0034] Example 2

[0035] The difference between this embodiment and embodiment 1 is that: in step 1, a spare titanium powder with a particle size of -100 to +160 mesh is obtained, and the powder with a particle size of -100 to +150 mesh accounts for 76% of the spare titanium powder; the rolling speed in step 2 is 18m / min; and the temperature in step 3 is 1100°C.

[0036] After testing, the porous titanium plate prepared in this embodiment has a porosity of 32.3%, a thickness of 0.25 mm, a width of 400 mm, and a tensile strength of 122 MPa.

[0037] Example 3

[0038] The difference between this embodiment and embodiment 1 is that: in step 1, a spare titanium powder with a particle size of -80 to +180 mesh is obtained, and the powder of -100 to +150 mesh accounts for 65% of the spare titanium powder; the rolling speed in step 2 is 12m / min; and the temperature in step 3 is 1050°C.

[0039] After testing, the porous titanium plate prepared in this embodiment has a porosity of 29.7%, a thickness of 0.26 mm, a width of 530 mm, and a tensile strength of 147 MPa.

[0040] Example 4

[0041] The difference between this embodiment and embodiment 1 is that: in step one, spare titanium powder with a particle size of -70 to +180 mesh is obtained, and the powder with a particle size of -100 to +150 mesh accounts for 90% of the spare titanium powder; in step two, the diameter of the support rollers is 600 mm, the gap width between the two working rollers is 0.01 mm, and the rolling force is 20 T; in step three, the temperature is 900°C.

[0042] After testing, the porous titanium plate prepared in this embodiment has a porosity of 20.3%, a thickness of 0.10 mm, a width of 450 mm, and a tensile strength of 173 MPa.

[0043] Example 5

[0044] The difference between this embodiment and embodiment 1 is that: in step one, spare titanium powder with a particle size of -80 to +180 mesh is obtained, and the powder with a particle size of -100 to +150 mesh accounts for 50% of the spare titanium powder; in step two, the diameter of the support rollers is 300 mm, the gap width between the two working rollers is 0.4 mm, the rolling speed is 20 m / min, and the rolling force is 8 T; in step three, the temperature is 1200°C.

[0045] After testing, the porous titanium plate prepared in this embodiment has a porosity of 59.5%, a thickness of 0.39 mm, a width of 510 mm, and a tensile strength of 104 MPa.

[0046] Example 6

[0047] The difference between this embodiment and embodiment 1 is that: in step 1, spare titanium powder with a particle size of -100 to +180 mesh is obtained, and the powder of -100 to +150 mesh accounts for 70% of the spare titanium powder; in step 2, the gap width between the two working rollers is 0.2 mm, the rolling speed is 18 m / min, and the rolling force is 17 T; in step 3, the temperature is 1050°C and the time is 100 min.

[0048] After testing, the porous titanium plate prepared in this embodiment has a porosity of 41.7%, a thickness of 0.26 mm, a width of 550 mm, and a tensile strength of 124 MPa.

[0049] Example 7

[0050] The difference between this embodiment and embodiment 1 is that: in step 2, the diameter of the working rolls is 20 mm, the rolling speed is 2 m / min, and the rolling force is 9 T; in step 3, the temperature is 1050° C. and the time is 180 min.

[0051] After testing, the porous titanium plate prepared in this embodiment has a porosity of 33.4%, a thickness of 0.19 mm, a width of 520 mm, and a tensile strength of 150 MPa.

[0052] Example 8

[0053] The difference between this embodiment and embodiment 1 is that: in step 2, the diameter of the working rolls is 70 mm, the roll gap width is 0.3 mm, the rolling speed is 12 m / min, and the rolling force is 9 T; in step 3, the sintering temperature is 1050° C., and the holding time is 30 min.

[0054] After testing, the porous titanium plate prepared in this embodiment has a porosity of 39.5%, a thickness of 0.31 mm, a width of 480 mm, and a tensile strength of 120 MPa.

[0055] Example 9

[0056] The difference between this embodiment and embodiment 1 is that: in step 2, the diameter of the working rolls is 20 mm, the gap width between the two working rolls is 0.2 mm, the rolling speed is 12 m / min, and the rolling force is 16 T; in step 3, the sintering temperature is 1050° C., and the holding time is 30 min.

[0057] After testing, the porous titanium plate prepared in this embodiment has a porosity of 40.6%, a thickness of 0.25 mm, a width of 490 mm, and a tensile strength of 113 MPa.

[0058] Example 10

[0059] The difference between this embodiment and embodiment 1 is that: in step 2, the diameter of the working rolls is 20 mm, the rolling speed is 12 m / min, and the rolling force is 8 T; in step 3, the temperature is 1100° C. and the time is 60 min.

[0060] After testing, the porous titanium plate prepared in this embodiment has a porosity of 24.3%, a thickness of 0.17 mm, a width of 420 mm, and a tensile strength of 118 MPa.

[0061] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a high-strength ultra-thin porous titanium plate, characterized in that: The method comprises the following steps: Step 1: Raw material preparation: Classify the titanium powder raw material powder, select the titanium powder with the required particle size, and obtain the spare titanium powder; Step 2: rolling green sheet: the spare titanium powder obtained in step 1 is continuously fed into the gap between two working rolls located on the same horizontal plane but rotating in opposite directions through a feeding device, and rolled by the pressure of the two working rolls to obtain a green sheet; Step 3, sintering: the green sheet obtained in step 2 is cut and cleaned of floating powder, and then constrained sintering is performed, and a porous titanium plate is obtained after cooling in the furnace. The porous titanium plate has a porosity of 20% to 60%, a thickness of no more than 0.4 mm, a width of 400 mm to 550 mm, and a tensile strength of more than 100 MPa.

2. The method for preparing a high-strength ultra-thin porous titanium plate according to claim 1, characterized in that: The particle size of the spare titanium powder in step 1 is -70 to +180 mesh, of which -100 to +150 mesh accounts for 50% to 90%.

3. The method for preparing a high-strength ultra-thin porous titanium plate according to claim 1, characterized in that: Support rollers for supporting the working rollers are arranged on both sides of the two working rollers in step 2.

4. The method for preparing a high-strength ultra-thin porous titanium plate according to claim 3, characterized in that: The diameters of the working rolls in step 2 are all 20 mm to 70 mm, and the diameters of the support rolls are all 300 mm to 600 mm.

5. The method for preparing a high-strength ultra-thin porous titanium plate according to claim 1, characterized in that: The width of the gap between the two working rolls in step 2 is 0.01 mm to 0.4 mm.

6. The method for preparing a high-strength ultra-thin porous titanium plate according to claim 1, characterized in that: The rolling speed in step 2 is 2m / min to 20m / min, and the rolling force is 8T to 20T.

7. The method for preparing a high-strength ultra-thin porous titanium plate according to claim 1, characterized in that: The constrained sintering in step three is to place the green sheet material after cutting and cleaning the floating powder on the support plate, and then put the cover plate on it for constrained sintering.

8. The method for preparing a high-strength ultra-thin porous titanium plate according to claim 1, characterized in that: The constrained sintering in step 3 is performed at a vacuum degree not greater than 1×10 -3 Pa, the temperature is 900℃~1200℃, and the time is 30min~180min.

Citation Information

Cited By

  • PEM water electrolysis hydrogen production gas diffusion layer and preparation method thereof

    CN119372676A