Hard surface surfacing method suitable for SM570 surface
By using a combination of carbon dioxide gas shielded welding and specific welding wire on the surface of SM570, the problem that existing welding methods are difficult to meet high hardness requirements is solved, the reliability of welding performance and hardness are significantly improved, and the safety and economy of the equipment are ensured. benefit.
Patent Information
- Application Number
- CN202411060784.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-15
AI Technical Summary
Existing welding methods are difficult to meet the high hardness requirements after surface surfacing of SM570, especially in the surface surfacing operations of the contact surface between the thruster body and the track of metallurgical equipment, electrical furnaces, etc., resulting in unreliable welding performance and insufficient surface hardness of the base metal, which affects The equipment operates safely.
A hard-surfacing method suitable for SM570 surfaces is adopted, including cleaning the surface of the base metal, using carbon dioxide gas shielded welding, first using THY-A309LQ stainless steel flux-cored gas shielded welding wire for bottom welding, and then using MT-FZ9 0 Hard-facing welding wire is used for middle and upper layer welding. The welding voltage and current are set to 25V and 210A or 220A. The welding speed is 8.8mm/s or 11.4mm/s. Two hardness measurements are performed and the weld bead is not polished. deal with.
Significantly improves the welding performance, enhances the hardness of the base metal surface, and ensures the safety, reliability and economic benefits of the equipment.
Smart Images

Figure CN118768694A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of welding technology, and in particular relates to a hard surface surfacing method suitable for SM570 surface. Background Art
[0002] SM570 is a low-carbon, low-alloy steel with excellent mechanical properties and corrosion resistance. It is mainly used in construction, bridges, vehicles, ships and other fields. The composition of SM570 mainly includes iron, carbon, manganese, phosphorus, sulfur and other elements. Among them, the carbon content is low, only about 0.1%, which is conducive to improving the toughness and ductility of the steel plate. The manganese content is high, in the range of 1.6%-1.8%, which can increase the strength and hardness of the steel plate. The phosphorus and sulfur content are also low, which is conducive to improving the corrosion resistance of the steel plate. In addition, appropriate amounts of alloying elements such as chromium, molybdenum, and copper are added to SM570 to further improve the corrosion resistance and mechanical properties of the steel plate. The tensile strength of SM570 is between 1100-1300MPa, the yield strength is between 800-900MPa, and the elongation is between 18%-25%. In addition, SM570 also has good bending and welding properties, which can meet various processing and manufacturing requirements. In some special working conditions, in addition to ensuring the good performance of SM570 itself, it is also necessary to further enhance the hardness of the material surface. For example, in the surface surfacing operation of the thruster body and the track contact surface of the electric furnace of metallurgical equipment, the welding method in the existing technology is difficult to ensure the reliability of welding performance, and the surface hardness of the parent material is low. Therefore, how to make it meet the high hardness requirements of the use conditions after surface surfacing is the key to ensure the safe operation of the equipment, and it is necessary to improve the welding method. Summary of the invention
[0003] In view of this, the present invention aims to overcome the defects in the prior art and proposes a hard surface surfacing method suitable for SM570 surface.
[0004] To achieve the above object, the technical solution created by the present invention is implemented as follows:
[0005] A hardfacing welding method suitable for SM570 surface comprises the following steps:
[0006] S1. Clean the surface of the base material and keep the surface temperature of the workpiece at room temperature before welding;
[0007] S2, the bottom layer is welded by carbon dioxide gas shielded welding, the welding wire is THY-A309LQ stainless steel flux-cored gas shielded welding wire, the welding voltage is set to 25V, the welding current is 210A, and the welding speed is 8.8mm / s;
[0008] S3, use carbon dioxide gas shielded welding for middle layer welding, use MT-FZ90 hard facing welding wire, set welding voltage to 25V, welding current to 220A, welding speed to 11.4mm / s;
[0009] S4, perform the first hardness measurement;
[0010] S5. Use carbon dioxide gas shielded welding to weld the upper layer. The welding wire is MT-FZ90 hardfacing welding wire. The welding voltage is set to 25V, the welding current is 220A, and the welding speed is 11.4mm / s.
[0011] S6. After welding is completed, the second hardness measurement is carried out after the specimen has cooled down.
[0012] Furthermore, in step S1, a sandblasting process is used to clean the surface of the base material.
[0013] Furthermore, the welding wire used for the bottom layer welding is φ1.2mm, and the welding wire used for the middle and upper layers is φ1.6mm.
[0014] Further, in step S4, during the first hardness measurement, there are no less than 15 test points, and the test hardness is ≥ HV500.
[0015] Furthermore, after welding, the upper cladding surface is not subjected to grinding treatment.
[0016] Furthermore, in step S6, the second hardness measurement is performed in accordance with standard ISO 6507-1:2008.
[0017] Furthermore, the heights of the welding layers of the bottom layer, the middle layer and the upper layer are all greater than or equal to 3 mm.
[0018] Furthermore, when welding the bottom layer, the middle layer and the upper layer, the shielding gas uses CO2 with a concentration greater than 99.99%.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] The welding method provided by the invention can be used for surface surfacing operation of the contact surface between the main body of the propeller of an electric furnace and the track, has reliable welding performance, greatly enhances the surface hardness of the parent material, is safe to use, and has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments and descriptions of the present invention are used to explain the present invention and do not constitute an improper limitation on the present invention. In the drawings:
[0022] Figure 1 It is a schematic diagram of the solder layer structure in the present invention. DETAILED DESCRIPTION
[0023] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0024] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0025] In the description of the invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installation", "connection" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the invention can be understood according to specific circumstances.
[0026] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments.
[0027] A hardfacing welding method suitable for SM570 surface comprises the following steps:
[0028] S1. Clean the surface of the base material and keep the surface temperature of the workpiece at room temperature (maintain 20℃~30℃) before welding;
[0029] S2, the bottom layer 3 is welded by carbon dioxide gas shielded welding, the welding wire is THY-A309LQ stainless steel flux-cored gas shielded welding wire, the welding voltage is set to 25V, the welding current is 210A, and the welding speed is 8.8mm / s;
[0030] S3, use carbon dioxide gas shielded welding to weld the middle layer 2, the welding layer structure is as follows Figure 1As shown, the welding wire is MT-FZ90 hard facing welding wire, the welding voltage is set to 25V, the welding current is 220A, and the welding speed is 11.4mm / s;
[0031] S4. Carry out the first hardness measurement to estimate whether the hardness can reach the final required hardness value;
[0032] S5. The upper layer 1 is welded by carbon dioxide gas shielded welding. The welding wire is MT-FZ90 hard facing welding wire. The welding voltage is set to 25V, the welding current is 220A, and the welding speed is 11.4mm / s. After the upper layer welding surface is welded, the weld is not ground because grinding will cause heat effects and micro cracks to the weld, thereby affecting the surface hardness value.
[0033] S6. After welding is completed, the second hardness measurement is carried out after the specimen has cooled down.
[0034] In the scheme of the present invention, the bottom layer is clad with stainless steel welding wire for base laying, because the cladding welding wire cannot be directly clad on the surface of the material, and the welding layer of the middle layer is a transition layer. Although hard welding wire is clad, the cladding layer formed by the stainless steel welding wire cannot reach the required hardness. Therefore, the upper layer is continued to be clad on the middle layer to meet the hardness requirements.
[0035] In step S1, a sandblasting process is used to clean the surface of the base material from oil, rust and other debris or moisture. In step S4, during the first hardness measurement, the test points are not less than 15, and the test hardness is ≥ HV500. In step S6, during the second hardness measurement, it is performed in accordance with standard ISO 6507-1:2008.
[0036] The height of the welding layer of the bottom layer, middle layer and upper layer is greater than or equal to 3mm. The welding wire used for the bottom layer is φ1.2mm, and the welding wire used for the middle layer and upper layer is φ1.6mm. When welding the bottom layer, middle layer and upper layer, the shielding gas is CO2 with a concentration greater than 99.99%.
[0037] The welding method provided by the invention can be used for surface surfacing operation of the contact surface between the main body of the propeller of an electric furnace and the track, has reliable welding performance, greatly enhances the surface hardness of the parent material, is safe to use, and has good economic benefits.
[0038] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A hardfacing method suitable for SM570 surface, It is characterized in that The steps include: S1. Clean the surface of the base material and keep the surface temperature of the workpiece at room temperature before welding; S2, the bottom layer is welded by carbon dioxide gas shielded welding, the welding wire is THY-A309LQ stainless steel flux-cored gas shielded welding wire, the welding voltage is set to 25V, the welding current is 210A, and the welding speed is 8.8mm / s; S3, use carbon dioxide gas shielded welding for middle layer welding, use MT-FZ90 hard facing welding wire, set welding voltage to 25V, welding current to 220A, welding speed to 11.4mm / s; S4, perform the first hardness measurement; S5. Use carbon dioxide gas shielded welding to weld the upper layer. The welding wire is MT-FZ90 hardfacing welding wire. The welding voltage is set to 25V, the welding current is 220A, and the welding speed is 11.4mm / s. S6. After welding is completed, the second hardness measurement is carried out after the specimen has cooled down.
2. A hard facing welding method for SM570 surface according to claim 1, Features: In step S1, the surface of the base material is cleaned by sandblasting.
3. A hard facing welding method for SM570 surface according to claim 1, Features: The welding wire used for the bottom layer is φ1.2mm, and the welding wire used for the middle and upper layers is φ1.6mm.
4. A hard facing welding method for SM570 surface according to claim 1, Features: In step S4, during the first hardness measurement, the number of test points is no less than 15, and the test hardness is ≥ HV500.
5. A hard facing welding method for SM570 surface according to claim 1, Features: After welding, the upper cladding surface is not ground.
6. A hard facing welding method for SM570 surface according to claim 1, Features: In step S6, the second hardness measurement is performed in accordance with standard ISO 6507-1:2008.
7. A hard facing welding method for SM570 surface according to claim 1, Features: The height of the welding layers of the bottom layer, the middle layer and the upper layer are all greater than or equal to 3mm.
8. A hard facing welding method for SM570 surface according to claim 1, Features: When welding the bottom, middle and upper layers, the shielding gas used is CO2 with a concentration greater than 99.99%.